PEEK fine-denier monofilament spinning process for PEM electrolytic cell proton exchange membrane and PEEK fine-denier monofilament prepared by spinning process
By adopting the PEEK fine denier monofilament spinning process with a fiber diameter less than 25 μm in the PEM electrolytic cell, the problem of reducing proton conductivity caused by the thickness of the proton exchange film of the PEM electrolytic cell is solved, and the electrolytic efficiency of hydrogen production by PEM water electrolytic is improved.
Patent Information
- Application Number
- CN202411148084.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing PEM electrolytic cell proton exchange membrane has a large diameter of PEEK monofilament, which increases the thickness of the proton exchange membrane, which reduces the proton conductivity, improves the internal resistance of the electrolytic cell, and affects the electrolysis of hydrogen production by PEM water electrolysis. efficiency.
Using PEEK fine denier monofilament spinning process with fiber diameter less than 25μm, the aspect ratio of spinneret holes is designed and multi-channel stretching is performed by adjusting the temperature in the screw extruder, using a multi-layer filter mesh and metal sand layer. and the styling treatment, a high-performance PEEK fine denier monofilament proton exchange membrane was prepared.
The fluidity and stability of PEEK monofilament is improved, the thickness of the proton exchange membrane is reduced, the proton conductivity is enhanced, the internal resistance of the electrolytic cell is reduced, and the electrolytic efficiency of hydrogen production by PEM water electrolysis is improved.
Smart Images

Figure CN118957773A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PEM electrolyzers, and in particular to a PEEK fine-denier monofilament spinning process for a proton exchange membrane of a PEM electrolyzer and the PEEK fine-denier monofilaments prepared by the spinning process. Background Art
[0002] As an efficient, clean and ideal secondary energy source, hydrogen energy has received widespread attention around the world. Large-scale and cheap production of hydrogen is one of the important links in the development and utilization of hydrogen energy. Using green electricity to produce H2 using water electrolysis technology can achieve zero carbon in the entire process, which is in line with the country's development strategy, and the operation is relatively simple and the technology is relatively mature.
[0003] Depending on the different materials of the electrolyzer diaphragm, the industry usually divides water electrolysis to produce hydrogen into alkaline water electrolysis (ALK), proton exchange membrane water electrolysis (PEM), and high-temperature solid oxide water electrolysis (SOEC).
[0004] Compared with alkaline water electrolysis hydrogen production technology, PEM water electrolysis hydrogen production technology has the advantages of high current density, high hydrogen purity, fast response speed and high working efficiency. PEM water electrolysis hydrogen production uses proton exchange membrane as solid electrolyte and pure water as raw material. Under the action of direct current, an oxidation reaction occurs at the anode to precipitate oxygen, and a reduction reaction occurs at the cathode to precipitate hydrogen.
[0005] Proton exchange membrane is the core component of PEM water electrolysis hydrogen production. Proton exchange membrane is generally composed of a substrate and a perfluorosulfonic acid resin coated on the surface of the substrate. Currently, expanded polytetrafluoroethylene (ePTFE) is commonly used as the substrate. However, due to the poor rigidity and softness of ePTFE, the proton exchange membrane made of it has too much ductility, unstable dimensions, and is prone to rupture and failure.
[0006] In order to obtain a proton exchange membrane with high mechanical strength and high dimensional stability, people use polyetheretherketone (PEEK) monofilaments to make the substrate of the proton exchange membrane. However, the diameter of the PEEK monofilaments currently used is relatively large, generally above 40μm, which makes the substrate made of PEEK monofilaments thicker, resulting in a thicker proton exchange membrane. The increase in the thickness of the proton exchange membrane will reduce proton conductivity, increase the internal resistance of the electrolytic cell, reduce current density, and increase the decomposition voltage, thereby affecting the electrolysis efficiency of PEM water electrolysis to produce hydrogen. Summary of the invention
[0007] The purpose of the present invention is to provide a spinning process for PEEK fine-denier monofilaments with a fiber diameter of less than 25 μm for use in PEM electrolyzer proton exchange membranes.
[0008] To achieve the above object, the present invention adopts the following technical scheme: a PEEK fine-denier monofilament spinning process for a PEM electrolyzer proton exchange membrane comprises the following steps: S1: slice and dry the PEEK resin; S2: adding the sliced and dried PEEK resin into a screw extruder for melt extrusion, wherein the temperature range of the feed section of the screw extruder is 330-380°C, the temperature range of the compression section is 390-450°C, and the temperature range of the metering section is 390-440°C; S3: The PEEK melt extruded by the screw extruder is first filtered through a filter group, and the filtered PEEK melt passes through a layer of metal sand and then enters the spinneret, and then is ejected from the spinneret holes of the spinneret to form a number of primary monofilaments. During the entire step of S3, the PEEK melt temperature is maintained at 390-440° C.; The filter mesh group is composed of a filter mesh with a mesh number of 1600 to 2000, and the metal sand layer is composed of metal sand with a mesh number of 16 to 40. The spinneret of the spinneret plate is composed of an upper spinneret guide hole and a lower spinneret micropore, and the aspect ratio of the spinneret micropore of the spinneret hole is 8 to 10. S4: Cooling the primary monofilaments and applying oil to bundle them into primary multifilaments; S5: The spun multifilament is stretched, shaped, wound and then divided into PEEK fine denier monofilaments with a fiber diameter of less than 25 μm; wherein the stretching of the spun multifilament is a two-pass stretching, the first pass of stretching is completed by a primary stretching hot roller, the roller temperature of the primary stretching hot roller is 160-210° C., and the roller speed is 300-400 m / min; the second pass of stretching is completed by a secondary stretching hot roller, the roller temperature of the secondary stretching hot roller is 180-240° C., and the roller speed is 800-1200 m / min; and the stretching ratio of the secondary stretching hot roller to the primary stretching hot roller is 2-4; the shaping of the spun multifilament is completed by a shaping hot roller, the roller temperature of the shaping hot roller is 180-240° C., and the roller speed is 700-1100 m / min.
[0009] Furthermore, the aforementioned PEEK fine-denier monofilament spinning process for the proton exchange membrane of the PEM electrolyzer, wherein: in S3, the filter mesh group includes three layers of filtration, each layer of filtration is stacked by filter mesh sheets with a mesh size of 1600 to 2000, and the three layers of filtration are gradually encrypted along the flow direction of the PEEK melt.
[0010] Furthermore, the aforementioned PEM electrolyzer proton exchange membrane uses a PEEK fine denier single filament spinning process, wherein: in the three-layer filtration of the filter mesh group along the flow direction of the PEEK melt, the first layer is formed by stacking filter mesh sheets with a mesh number of 1600, the second layer is formed by stacking filter mesh sheets with a mesh number of 1800, and the third layer is formed by stacking filter mesh sheets with a mesh number of 2000.
[0011] Furthermore, the aforementioned PEM electrolyzer proton exchange membrane uses a PEEK fine-denier monofilament spinning process, wherein: the thickness of the metal sand layer is 1 cm.
[0012] Furthermore, the aforementioned PEEK fine-denier single-filament spinning process for the proton exchange membrane of the PEM electrolyzer, wherein: in S3, the aspect ratio of the spinning micropores of the spinneret is 9.
[0013] Further, the aforementioned PEEK fine denier single-filament spinning process for proton exchange membrane of PEM electrolyzer, wherein: in S5, the stretching of the nascent multifilament is a two-pass stretching, the first pass stretching is completed by a primary stretching hot roller, the roller temperature of the primary stretching hot roller is 210°C, the roller speed is 400m / min, and the residence time of the nascent multifilament on the primary stretching hot roller is 0.4 seconds; the second pass stretching is completed by a secondary stretching hot roller, the roller temperature of the secondary stretching hot roller is 240°C, the roller speed is 1100m / min, and the residence time of the nascent multifilament on the secondary stretching hot roller is 0.2 seconds; and the stretching ratio of the secondary stretching hot roller to the primary stretching hot roller is 4; the shaping of the nascent multifilament is completed by a shaping hot roller, the roller temperature of the shaping hot roller is 240°C, the roller speed is 1100m / min, and the residence time of the nascent multifilament on the tertiary shaping hot roller is 0.2 seconds.
[0014] The second object of the present invention is to provide a PEEK fine-denier monofilament for a PEM electrolyzer proton exchange membrane having a fiber diameter of less than 25 μm.
[0015] Through the implementation of the above technical scheme, the beneficial effects of the present invention are as follows: the entire spinning process is designed, (1) in the PEEK melt extrusion process, the temperature of the feed end, compression section and metering section of the screw extruder is designed, and the temperature of the compression section and the metering section is increased to further improve the fluidity of the PEEK melt, making the viscosity of the PEEK melt smaller, making the monofilament spun from the PEEK melt easier to be stretched and refined in the subsequent process, and providing further guarantee for the production of PEEK fine denier monofilaments with a fiber diameter of less than 25 μm; (2) in the spinneret spinning process, firstly, a 1600-2000 mesh filter group is used to filter the PEEK melt, effectively filtering out impurities in the PEEK melt, which can not only increase the PEEK melt spinning through the spinneret (3) In the spinning process of the spinneret, the filtered PEEK melt needs to pass through a layer of metal sand before entering the spinneret. The metal sand layer can keep the melt pressure and flow rate of the PEEK melt uniform, further increasing the stability of the PEEK melt when it is spun through the spinneret, further improving the performance of the PEEK monofilament after spinning, making the PEEK monofilament less likely to break during the subsequent stretching, making the PEEK monofilament easier to stretch and refine, and providing a guarantee for the production of PEEK fine-denier monofilaments with a fiber diameter of less than 25 μm. One-step guarantee; (4) In the spinning process of the spinneret, the aspect ratio of the spinneret micropores of the spinneret hole is designed to be 8-10. This spinneret micropore aspect ratio design, on the one hand, can effectively reduce the extrusion expansion effect, effectively eliminate the unstable flow of the melt, increase the stability of the PEEK melt when it is spun through the spinneret, make the PEEK monofilament less likely to break during the subsequent stretching, and make the PEEK monofilament easier to be stretched and refined in the subsequent stretching, which provides further guarantee for the production of PEEK fine denier monofilaments with a fiber diameter of less than 25μm. On the other hand, the spun PEEK monofilaments are relatively thin, and the PEEK monofilaments are preliminarily refined first, so that the PEEK monofilaments can be further refined by the subsequent stretching, which provides a guarantee for the production of PEEK fine denier monofilaments with a fiber diameter of less than 25μm. Further guarantee; (5) in the stretching and shaping process, the roller temperature, roller speed, residence time and stretching ratio of each level of stretching hot rollers and shaping rollers are designed to ensure that the PEEK fine denier monofilament is stretched to a fiber diameter of less than 25μm, and to ensure that the performance of the stretched PEEK fine denier monofilament can meet the preparation requirements of water electrolysis hydrogen production diaphragm; (6) PEEK fine denier monofilaments with a fiber diameter of less than 25μm can be obtained. The substrate made of the PEEK fine denier monofilament of the present invention is thinner than the traditional substrate, so that the produced proton exchange membrane is also thinner. The reduction in the thickness of the proton exchange membrane will improve the proton conductivity, reduce the internal resistance of the electrolytic cell, increase the current density, and reduce the decomposition voltage, thereby improving the electrolysis efficiency of PEM water electrolysis hydrogen production. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the structure of the spinneret holes in the spinning process of PEEK fine-denier single filaments for PEM electrolyzer proton exchange membrane according to the present invention.
[0017] Figure 2 Schematic diagram of the fiber diameter of the PEEK fine denier monofilament obtained in Example 1 of the present invention under an electron microscope.
[0018] Figure 3 Schematic diagram of the fiber diameter of the PEEK fine denier monofilament obtained in Example 2 of the present invention under an electron microscope.
[0019] Figure 4 Schematic diagram of the fiber diameter of the PEEK fine denier monofilament obtained in Example 3 of the present invention under an electron microscope. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Example 1
[0021] The PEEK fine-denier monofilament for water electrolysis hydrogen production diaphragm is prepared by a spinning process of PEEK fine-denier monofilament for PEM electrolyzer proton exchange membrane. The spinning process of PEEK fine-denier monofilament for PEM electrolyzer proton exchange membrane comprises the following steps: S1: slice and dry the PEEK resin; S2: adding the sliced and dried PEEK resin into a screw extruder for melt extrusion, wherein the temperature range of the feed section of the screw extruder is 380°C, the temperature range of the compression section is 450°C, and the temperature range of the metering section is 440°C; increasing the temperature of the compression section and the metering section to further improve the fluidity of the PEEK melt, making the viscosity of the PEEK melt smaller, and making the monofilament spun from the PEEK melt easier to be stretched and refined in the subsequent process; S3: The PEEK melt extruded by the screw extruder is first filtered through a filter group, and the filtered PEEK melt passes through a layer of metal sand and then enters the spinneret, and then is ejected from the spinneret holes of the spinneret to form a number of primary monofilaments. During the entire step of S3, the PEEK melt temperature is maintained at 440° C., so that the temperature of the spinneret can be kept uniform, ensuring the stability of the melt when it is ejected from the spinneret holes of the spinneret; Among them, the filter mesh group includes three layers of filtration. In this embodiment, in the three-layer filtration of the filter mesh group along the flow direction of the PEEK melt, the first layer is formed by stacking filter mesh sheets with a mesh number of 1600, the second layer is formed by stacking filter mesh sheets with a mesh number of 1800, and the third layer is formed by stacking filter mesh sheets with a mesh number of 2000; the 1600-2000 mesh filter mesh group is used to filter the PEEK melt, which effectively filters out impurities in the PEEK melt, not only increasing the stability of the PEEK melt when it is spun through the spinneret, but also making the PEEK monofilaments after spinning less likely to break during the subsequent stretching, making the PEEK monofilaments easier to be stretched and refined in the subsequent process; The metal sand layer is composed of metal sand with a mesh number of 40; the thickness of the metal sand layer is 1 cm; the metal sand is made of stainless steel material, and the metal sand layer can keep the melt pressure and flow rate of the PEEK melt uniform, further increase the stability of the PEEK melt when spinning through the spinneret, further improve the performance of the PEEK monofilament after spinning, make the PEEK monofilament not easy to break during the subsequent stretching, and make the PEEK monofilament easier to be stretched and refined in the subsequent process; Among them, Figure 1 As shown, the spinneret of the spinneret plate is composed of an upper spinneret guide hole 1 and a lower spinneret microhole 2, and the aspect ratio of the spinneret microhole of the spinneret hole is 9, that is: Figure 1 As shown in the figure, X / Y=9, X is the length of the spinneret microhole, and Y is the diameter of the spinneret microhole; this spinneret microhole aspect ratio design, on the one hand, can effectively reduce the extrusion expansion effect, effectively eliminate the unstable flow of the melt, increase the stability of the PEEK melt when spinning through the spinneret, make the PEEK monofilament less likely to break during the subsequent stretching, make the PEEK monofilament easier to be stretched and refined in the subsequent stretching, and provide further guarantee for producing PEEK fine denier monofilaments with a fiber diameter of less than 25μm. On the other hand, the spun PEEK monofilaments are relatively thin, and the PEEK monofilaments are preliminarily refined first, so that the PEEK monofilaments can be further refined by the subsequent stretching; S4: Cooling the primary monofilaments and applying oil to bundle them into primary multifilaments; S5: The spun multifilament is stretched, shaped, and wound to form a PEEK fine-denier monofilament with a fiber diameter of 22.826 μm; the fiber diameter of the PEEK fine-denier monofilament is as follows: Figure 2As shown; wherein, the stretching of the primary multifilament is two-pass stretching, the first stretching is completed by the primary stretching hot roller, the roller temperature of the primary stretching hot roller is 210°C, the roller speed is 300m / min, and the residence time of the primary multifilament on the primary stretching hot roller is 0.4 seconds; the second stretching is completed by the secondary stretching hot roller, the roller temperature of the secondary stretching hot roller is 240°C, the roller speed is 1200m / min, and the residence time of the primary multifilament on the secondary stretching hot roller is 0.2 seconds; the stretching ratio of the secondary stretching hot roller to the primary stretching hot roller is 4; the shaping of the primary multifilament is completed by the shaping hot roller, the roller temperature of the shaping hot roller is 240°C, the roller speed is 1100m / min, and the residence time of the nascent multifilament on the three-stage shaping hot roller is 0.2 seconds; in this stretching and shaping process, the parameter designs of the primary stretching hot roller, the secondary stretching hot roller and the shaping hot roller are specially designed for the performance of the PEEK monofilament obtained after the previous processes. Through the parameter design of the primary stretching hot roller, the secondary stretching hot roller and the shaping hot roller of the present invention, the PEEK fine denier monofilament can be stretched to 22.826μm, and at the same time, it can be ensured that the performance of the stretched PEEK fine denier monofilament can meet the preparation requirements of the water electrolysis hydrogen production diaphragm. Example 2
[0022] The PEEK fine-denier monofilament for water electrolysis hydrogen production diaphragm is prepared by a spinning process of PEEK fine-denier monofilament for PEM electrolyzer proton exchange membrane. The spinning process of PEEK fine-denier monofilament for PEM electrolyzer proton exchange membrane comprises the following steps: S1: slice and dry the PEEK resin; S2: adding the sliced and dried PEEK resin into a screw extruder for melt extrusion, wherein the temperature range of the feed section of the screw extruder is 330°C, the temperature range of the compression section is 390°C, and the temperature range of the metering section is 390°C; the temperature design of the compression section and the metering section can further improve the fluidity of the PEEK melt, make the viscosity of the PEEK melt smaller, and make the monofilament spun from the PEEK melt easier to be stretched and refined in the subsequent process; S3: The PEEK melt extruded by the screw extruder is first filtered through a filter group, and the filtered PEEK melt passes through a layer of metal sand and then enters the spinneret, and then is ejected from the spinneret holes of the spinneret to form a number of primary monofilaments. During the entire step of S3, the PEEK melt temperature is maintained at 390° C.; Among them, the filter mesh group is composed of filter meshes with a mesh number of 1600 to 2000, and the filter mesh group includes three layers of filtration. In this embodiment, in the three-layer filtration of the filter mesh group along the flow direction of the PEEK melt, the first layer is formed by stacking filter meshes with a mesh number of 1600, the second layer is formed by stacking filter meshes with a mesh number of 1800, and the third layer is formed by stacking filter meshes with a mesh number of 2000; the 1600-2000 mesh filter mesh group is used to filter the PEEK melt, which effectively filters out impurities in the PEEK melt, and can not only increase the PEEK melt through the spinneret The metal sand layer is composed of metal sand with a mesh number of 16; the thickness of the metal sand layer is 1 cm; the metal sand is made of stainless steel material, and the metal sand layer can keep the melt pressure and flow rate of the PEEK melt uniform, further increasing the stability of the PEEK melt when it is spun through the spinneret, further improving the performance of the PEEK monofilament after spinning, making the PEEK monofilament not easy to break during the subsequent stretching, and making the PEEK monofilament easier to be stretched and refined in the subsequent process; Among them, Figure 1 As shown, the spinneret of the spinneret plate is composed of an upper spinneret guide hole 1 and a lower spinneret microhole 2, and the aspect ratio of the spinneret microhole of the spinneret hole is 8, that is: Figure 1 As shown in the figure, X / Y=8, X is the length of the spinneret microhole, and Y is the diameter of the spinneret microhole; this spinneret microhole aspect ratio design, on the one hand, can effectively reduce the extrusion expansion effect, effectively eliminate the unstable flow of the melt, increase the stability of the PEEK melt when spinning through the spinneret, make the PEEK monofilament less likely to break during the subsequent stretching, make the PEEK monofilament easier to be stretched and refined in the subsequent stretching, and provide further guarantee for producing PEEK fine denier monofilaments with a fiber diameter of less than 25μm. On the other hand, the spun PEEK monofilaments are relatively thin, and the PEEK monofilaments are preliminarily refined first, so that the PEEK monofilaments can be further refined by the subsequent stretching; S4: Cooling the primary monofilaments and applying oil to bundle them into primary multifilaments; S5: The spun multifilament is stretched, shaped, and wound to form a PEEK fine-denier monofilament with a fiber diameter of 24.499 μm; the fiber diameter of the PEEK fine-denier monofilament is as follows: Figure 3As shown; wherein, the stretching of the primary multifilament is a two-pass stretching, the first pass stretching is completed by a primary stretching hot roller, the roller temperature of the primary stretching hot roller is 160°C, the roller speed is 400m / min, and the residence time of the primary multifilament on the primary stretching hot roller is 0.3 seconds; the second pass stretching is completed by a secondary stretching hot roller, the roller temperature of the secondary stretching hot roller is 180°C, the roller speed is 800m / min, and the residence time of the primary multifilament on the secondary stretching hot roller is 0.3 seconds; and the stretching ratio of the secondary stretching hot roller to the primary stretching hot roller is 2; the shaping of the primary multifilament is completed by a shaping hot roller, the roller temperature of the shaping hot roller is 1 80℃, roller speed is 700m / min, and the residence time of the nascent multifilament on the three-stage shaping hot roller is 0.3 seconds; in this stretching and shaping process, the parameter designs of the primary stretching hot roller, the secondary stretching hot roller and the shaping hot roller are specially designed for the performance of the PEEK monofilament obtained after the previous processes. Through the parameter design of the primary stretching hot roller, the secondary stretching hot roller and the shaping hot roller of the present invention, the PEEK fine denier monofilament can be stretched to a fiber diameter of 24.499μm, and the performance of the stretched PEEK fine denier monofilament can meet the preparation requirements of the water electrolysis hydrogen production diaphragm. Example 3
[0023] The PEEK fine-denier monofilament for water electrolysis hydrogen production diaphragm is prepared by a spinning process of PEEK fine-denier monofilament for PEM electrolyzer proton exchange membrane. The spinning process of PEEK fine-denier monofilament for PEM electrolyzer proton exchange membrane comprises the following steps: S1: slice and dry the PEEK resin; S2: adding the sliced and dried PEEK resin into a screw extruder for melt extrusion, wherein the temperature range of the feed section of the screw extruder is 350°C, the temperature range of the compression section is 420°C, and the temperature range of the metering section is 410°C; the temperature design of the compression section and the metering section can further improve the fluidity of the PEEK melt, make the viscosity of the PEEK melt smaller, and make the monofilament spun from the PEEK melt easier to be stretched and refined in the subsequent process; S3: The PEEK melt extruded by the screw extruder is first filtered through a filter group, and the filtered PEEK melt passes through a layer of metal sand and then enters the spinneret, and then is ejected from the spinneret holes of the spinneret to form a number of primary monofilaments. During the entire step of S3, the PEEK melt temperature is maintained at 410° C.; Among them, the filter group includes three layers of filtration. In the three layers of filtration of the filter group along the flow direction of the PEEK melt, the first layer is formed by stacking filter mesh sheets with a mesh number of 1600, the second layer is formed by stacking filter mesh sheets with a mesh number of 1800, and the third layer is formed by stacking filter mesh sheets with a mesh number of 2000; the metal sand layer is composed of metal sand with a mesh number of 30; the thickness of the metal sand layer is 1 cm; the metal sand is made of stainless steel material, and the metal sand layer can keep the melt pressure and flow rate of the PEEK melt uniform, further increase the stability of the PEEK melt when spinning through the spinneret, further improve the performance of the PEEK monofilament after spinning, make the PEEK monofilament not easy to break during the subsequent stretching, and make the PEEK monofilament easier to stretch and refine in the subsequent process; Among them, Figure 1 As shown, the spinneret of the spinneret plate is composed of an upper spinneret guide hole 1 and a lower spinneret microhole 2, and the aspect ratio of the spinneret microhole of the spinneret hole is 10, that is: Figure 1 As shown in the figure, X / Y=10, X is the length of the spinneret micropore, and Y is the diameter of the spinneret micropore; this spinneret micropore aspect ratio design, on the one hand, can effectively reduce the extrusion expansion effect, effectively eliminate the unstable flow of the melt, increase the stability of the PEEK melt when spinning through the spinneret, make the PEEK monofilament less likely to break during the subsequent stretching, make the PEEK monofilament easier to be stretched and refined in the subsequent stretching, and provide further guarantee for producing PEEK fine denier monofilaments with a fiber diameter of less than 25μm. On the other hand, the spun PEEK monofilaments are relatively thin, and the PEEK monofilaments are preliminarily refined first, so that the PEEK monofilaments can be further refined by the subsequent stretching; S4: Cooling the primary monofilaments and applying oil to bundle them into primary multifilaments; S5: The spun multifilament is stretched, shaped, and wound to form a PEEK fine-denier monofilament with a fiber diameter of 23.764 μm; the fiber diameter of the PEEK fine-denier monofilament is as follows: Figure 4As shown; wherein, the stretching of the primary multifilament is a two-pass stretching, the first pass stretching is completed by a primary stretching hot roller, the roller temperature of the primary stretching hot roller is 190°C, the roller speed is 350m / min, and the residence time of the primary multifilament on the primary stretching hot roller is 0.5 seconds; the second pass stretching is completed by a secondary stretching hot roller, the roller temperature of the secondary stretching hot roller is 230°C, the roller speed is 1100m / min, and the residence time of the primary multifilament on the secondary stretching hot roller is 0.4 seconds; and the stretching ratio of the secondary stretching hot roller to the primary stretching hot roller is 3.14; the shaping of the primary multifilament is completed by a shaping hot roller, the roller temperature of the shaping hot roller is 230℃, roller speed is 1000m / min; and the residence time of the nascent multifilament on the three-stage shaping hot roller is 0.4 seconds; in this stretching and shaping process, the parameter designs of the primary stretching hot roller, the secondary stretching hot roller and the shaping hot roller are specially designed for the performance of the PEEK monofilament obtained after the previous processes. Through the parameter design of the primary stretching hot roller, the secondary stretching hot roller and the shaping hot roller of the present invention, the PEEK fine denier monofilament can be stretched to a fiber diameter of 23.764μm, and the performance of the stretched PEEK fine denier monofilament can meet the preparation requirements of the water electrolysis hydrogen production diaphragm.
[0024] In order to more intuitively understand the data changes of each embodiment of the present invention, the data of each embodiment is explained below by forming a table, wherein the feeding section temperature, compression section temperature, metering section temperature, mesh number of each layer of the filter screen group, thickness and mesh number of the metal sand, and spinneret micropore long hole ratio of the spinneret of each embodiment are listed in Table 1: Table 1:
[0025] The roller temperature, roller speed, and residence time of the primary stretching hot roller, the roller temperature, roller speed, and residence time of the secondary stretching hot roller, the stretching ratio, the roller temperature, roller speed, and residence time of the shaping hot roller, and the PEEK fiber diameter in each embodiment are listed in Table 2: Table 2:
[0026] The advantages of the present invention are as follows: the entire spinning process is designed, (1) in the PEEK melt extrusion process, the temperature of the feed end, compression section and metering section of the screw extruder is designed, and the temperature of the compression section and the metering section is increased, so as to further improve the fluidity of the PEEK melt, make the viscosity of the PEEK melt smaller, and make the monofilament spun from the PEEK melt easier to be stretched and refined in the subsequent process, thereby providing further guarantee for producing PEEK fine denier monofilaments with a fiber diameter of less than 25 μm; (2) in the spinneret spinning process, firstly, a 1600-2000 mesh filter group is used to filter the PEEK melt, so as to effectively filter out impurities in the PEEK melt, which can not only increase the stability of the PEEK melt when it is spun through the spinneret, but also make The PEEK monofilament after spinning is not easy to break during the subsequent stretching, making the PEEK monofilament easier to stretch and refine in the subsequent stretching, providing further guarantee for producing PEEK fine-denier monofilaments with a fiber diameter of less than 25 μm; (3) In the spinneret spinning process, the filtered PEEK melt needs to pass through a layer of metal sand before entering the spinneret. The metal sand layer can keep the melt pressure and flow rate of the PEEK melt uniform, further increasing the stability of the PEEK melt when spinning through the spinneret, further improving the performance of the PEEK monofilament after spinning, making the PEEK monofilament less likely to break during the subsequent stretching, making the PEEK monofilament easier to stretch and refine in the subsequent stretching, providing further guarantee for producing PEEK fine-denier monofilaments with a fiber diameter of less than 25 μm; (4 ) In the spinning process of the spinneret, the aspect ratio of the spinneret micropores of the spinneret hole is designed to be 8 to 10. This spinneret micropore aspect ratio design, on the one hand, can effectively reduce the extrusion expansion effect, effectively eliminate the unstable flow of the melt, and increase the stability of the PEEK melt when it is spun through the spinneret, making the PEEK monofilament less likely to break during the subsequent stretching, making the PEEK monofilament easier to stretch and refine in the subsequent stretching, providing further guarantee for the production of PEEK fine denier monofilaments with a fiber diameter of less than 25μm. On the other hand, the spun PEEK monofilaments are relatively thin, and the PEEK monofilaments are preliminarily refined first, so that the PEEK monofilaments can be further refined in the subsequent stretching, providing further guarantee for the production of PEEK fine denier monofilaments with a fiber diameter of less than 25μm. (5) In the stretching and shaping process, the roller temperature, roller speed, residence time and stretching ratio of each level of stretching hot rollers and shaping rollers are designed to ensure that the PEEK fine denier monofilaments are stretched to a fiber diameter of less than 25 μm, and the performance of the stretched PEEK fine denier monofilaments can meet the preparation requirements of water electrolysis hydrogen production diaphragm; (6) PEEK fine denier monofilaments with a fiber diameter of less than 25 μm can be obtained. The substrate made of the PEEK fine denier monofilaments of the present invention is thinner than the traditional substrate, so that the prepared proton exchange membrane is also thinner. The reduction in the thickness of the proton exchange membrane will improve the proton conductivity, reduce the internal resistance of the electrolytic cell, increase the current density, and reduce the decomposition voltage, thereby improving the electrolysis efficiency of PEM water electrolysis hydrogen production.
[0027] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any other form. Any modification or equivalent change made according to the technical essence of the present invention still falls within the scope of protection required by the present invention.
Claims
1. The PEEK fine-denier monofilament spinning process for PEM electrolyzer proton exchange membrane is characterized by: The following steps are involved: S1: slice and dry the PEEK resin; S2: adding the sliced and dried PEEK resin into a screw extruder for melt extrusion, wherein the temperature range of the feed section of the screw extruder is 330-380°C, the temperature range of the compression section is 390-450°C, and the temperature range of the metering section is 390-440°C; S3: The PEEK melt extruded by the screw extruder is first filtered through a filter group, and the filtered PEEK melt passes through a layer of metal sand and then enters the spinneret, and then is ejected from the spinneret holes of the spinneret to form a number of primary monofilaments. During the entire step of S3, the PEEK melt temperature is maintained at 390-440° C.; The filter mesh group is composed of a filter mesh with a mesh number of 1600 to 2000, and the metal sand layer is composed of metal sand with a mesh number of 16 to 40. The spinneret of the spinneret plate is composed of an upper spinneret guide hole and a lower spinneret micropore, and the aspect ratio of the spinneret micropore of the spinneret hole is 8 to 10. S4: Cooling the primary monofilaments and applying oil to bundle them into primary multifilaments; S5: The spun multifilament is stretched, shaped, and wound to form PEEK fine denier monofilaments with a fiber diameter of less than 25 μm; wherein the stretching of the spun multifilament is a two-pass stretching, the first pass stretching is completed by a primary stretching hot roller, the roller temperature of the primary stretching hot roller is 160-210° C., and the roller speed is 300-400 m / min, and the second pass stretching is completed by a secondary stretching hot roller, the roller temperature of the secondary stretching hot roller is 180-240° C., and the roller speed is 800-1200 m / min, and the stretching ratio of the secondary stretching hot roller to the primary stretching hot roller is 2-4; the shaping of the spun multifilament is completed by a shaping hot roller, the roller temperature of the shaping hot roller is 180-240° C., and the roller speed is 700-1100 m / min.
2. The PEEK fine-denier monofilament spinning process for PEM electrolyzer proton exchange membrane according to claim 1, characterized in that: In S3, the filter group includes three layers of filtration, each layer of filtration is formed by stacking filter mesh sheets with a mesh number of 1600 to 2000, and the three layers of filtration are gradually encrypted along the flow direction of the PEEK melt.
3. The PEEK fine-denier monofilament spinning process for PEM electrolyzer proton exchange membrane according to claim 2, characterized in that: In the three-layer filtration of the filter mesh group along the flow direction of the PEEK melt, the first layer is composed of filter mesh sheets with a mesh number of 1600, the second layer is composed of filter mesh sheets with a mesh number of 1800, and the third layer is composed of filter mesh sheets with a mesh number of 2000.
4. The PEEK fine-denier monofilament spinning process for PEM electrolyzer proton exchange membrane according to claim 1, characterized in that: The thickness of the metal sand layer is 1 cm.
5. The PEEK fine-denier monofilament spinning process for PEM electrolyzer proton exchange membrane according to claim 1, characterized in that: In S3, the aspect ratio of the spinning micropores of the spinneret is 9.
6. The PEEK fine-denier monofilament spinning process for PEM electrolyzer proton exchange membrane according to claim 1, characterized in that: In S5, the stretching of the spun multifilament is a two-pass stretching, the first pass of stretching is completed by a primary stretching hot roller, the roller temperature of the primary stretching hot roller is 210°C, and the roller speed is 300m / min; the second pass of stretching is completed by a secondary stretching hot roller, the roller temperature of the secondary stretching hot roller is 240°C, and the roller speed is 1200m / min; the stretching ratio of the secondary stretching hot roller to the primary stretching hot roller is 4; the shaping of the spun multifilament is completed by a shaping hot roller, and the roller temperature of the shaping hot roller is 240°C, and the roller speed is 1100m / min. 7.PEEK fine denier monofilament for PEM electrolyzer proton exchange membrane, characterized by: The PEEK fine-denier monofilament is prepared by the PEEK fine-denier monofilament spinning process for the PEM electrolyzer proton exchange membrane as claimed in any one of claims 1 to 6.
Citation Information
Patent Citations
Melt-spinning hot-stretch forming preparation method of polyetheretherketone fibre
CN101225555A
Method for cleaning chemical fiber melt melting conveying system
CN102061528A
Production technology of superfine flat fiber
CN108103599A
PEEK FDY (Polyether Ether Ketone Fully Drawn Yarn) preparation process and PEEK FDY
CN115418732A
PEEK monofilament preparation system and preparation method thereof
CN116623304A
Cited By
Preparation method of polyether ketone amide / polyether ether ketone superfine denier monofilament
CN120082982A