Anti-static wool felt material and application thereof
By treating the wool plush fibers in metal ions and vulcanization reduction solutions, a high-conductivity sulfide is formed, which solves the electrostatic problem of high-end wool plush fabrics, achieving long-lasting anti-static effect and good washing resistance.
Patent Information
- Application Number
- CN202411111828.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-15
AI Technical Summary
High-end pure wool plush fabrics are prone to static electricity in dry environments, resulting in static accumulation and discharge of thugs, affecting the comfort and safety of wearing. The existing anti-static treatment methods are not lasting and fail after washing.
The pretreated pure wool fiber is immersed in a metal ion solution and a sulfurization reduction solution to react to form sulfides with silver, copper and nickel, which improves the conductivity of the fibers, thereby preparing anti-static wool fibers and fabrics. .
It significantly improves the anti-static performance and washing resistance. Compared with fabrics with anti-static agents, the prepared anti-static wool plush fabric still maintains a good anti-static effect after friction and washing.
Smart Images

Figure BDA0004992456270000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textile fibers, and in particular to an antistatic wool velvet material and application thereof. Background Art
[0002] Wool fleece fabric refers to fabric made of wool or cashmere through spinning, weaving and finishing. It is divided into knitted and woven fabrics according to the weaving form. Clothing made of it has the characteristics of warmth and comfort, moisture absorption and breathability, drape and crispness, visual dignity, and soft touch. However, since wool fleece is an insulating material, it is easy to be charged and generate static electricity when rubbed, especially in a dry environment. The greater the friction intensity and the higher the dryness, the easier it is to generate static electricity. Static electricity accumulation will produce a discharge phenomenon, which not only brings discomfort to people, but also the static electricity on clothes can easily absorb dust and bacteria, seriously affecting people's comfort and safety in wearing.
[0003] In order to solve the problem of static electricity, a certain proportion of organic conductive fibers are generally added to wool fabrics to disperse the charge and reduce discharge, but this method is only applicable to low-end wool and chemical fiber blended fabrics. For high-end pure wool fabrics, most of them currently use antistatic spray or spray or immerse antistatic agents on the surface of wool fibers, which can form a layer of antistatic agents on the surface of wool or cashmere fibers, but the effect of this treatment method is not long-lasting, and most of them lose their effect after one washing. Summary of the invention
[0004] In view of the above-mentioned prior art, the object of the present invention is to provide an antistatic wool plush material and application thereof.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] In a first aspect of the present invention, an antistatic wool fiber is provided, which is prepared by the following method:
[0007] (1) immersing the pretreated pure wool fiber in a metal ion solution, reacting at 20-60° C. for 3-5 hours, and drying after the reaction to obtain wool fiber with metal ions;
[0008] (2) immersing the wool plush fiber with metal ions obtained in step (1) into a sulfide reduction solution, reacting at 60-100° C. for 3-5 hours, cooling down, taking out, rinsing and drying, to obtain an antistatic wool plush fiber;
[0009] In step (1), the mass concentration of the metal ion solution is 1-10%, the solute is a mixture of silver nitrate, copper sulfate and nickel sulfate in a mass ratio of (0.5-1.5): (1-2): (0.4-0.6), and the solvent is water.
[0010] Preferably, in step (1), the pretreatment method is: placing the pure wool velvet fiber in a penetrant, washing it at 50-60° C. for 20 minutes, dehydrating and drying it to obtain the pretreated pure wool velvet fiber.
[0011] Preferably, the pure wool fibers are one or more of cashmere fibers and wool fibers.
[0012] Preferably, in step (1), the bath ratio of the pretreated wool fibers to the metal ion solution is 1:(10-50).
[0013] Preferably, in step (2), the mass concentration of the sulfide-reducing solution is 2-20%, the solute is one or more of sodium sulfide, sodium thiosulfate, and sodium sulfate, and the solvent is water.
[0014] Preferably, in step (2), the bath ratio of the wool fibers carrying metal ions to the sulfide-reducing solution is 1:(10-50).
[0015] The second aspect of the present invention discloses the use of the antistatic wool plush fiber in the preparation of antistatic wool plush products.
[0016] Preferably, the antistatic wool plush product is an antistatic wool plush fabric.
[0017] The third aspect of the present invention provides an antistatic wool plush product, characterized in that it is prepared by the following method:
[0018] The antistatic wool velvet fiber is uniformly mixed with wool velvet fiber that has not been treated with antistatic treatment at a mass ratio of 1%-10%, and antistatic functional wool velvet fabric is obtained through blending, weaving, dyeing and finishing;
[0019] Or the pretreated semi-finished pure wool plush fabric is immersed in a metal ion solution for reaction to obtain a wool plush fabric with metal ions; the wool plush fabric with metal ions is immersed in a sulfide reduction solution for reaction to obtain an antistatic wool plush fabric; the mass concentration of the metal ion solution is 1-10%, the solute is a mixture of silver nitrate, copper sulfate, and nickel sulfate in a mass ratio of (0.5-1.5): (1-2): (0.4-0.6), and the solvent is water.
[0020] Preferably, the pretreatment method is: putting the semi-finished pure wool velvet fabric into a penetrant, washing it at 50-60° C. for 20 minutes, dehydrating and drying it to obtain the pretreated semi-finished pure wool velvet fabric.
[0021] Preferably, the semi-finished pure wool plush fabric is made of pure wool plush fiber through wool blending, combing, drawing, roving, spun yarn, winding, warping, reeding and weaving to make pure wool plush grey cloth, and the pure wool plush grey cloth is washed, shrunk, washed and dried to make the semi-finished pure wool plush fabric to be dyed and finished.
[0022] Beneficial effects of the present invention:
[0023] The present invention utilizes a mixed metal ion solution containing silver ions, copper ions, and nickel ions to modify woolen cashmere fibers or semi-finished pure woolen cashmere fabrics, so that the woolen cashmere fibers adsorb metal ions, and utilize a sulfide reducing agent to reduce the metal ions and react with sulfur to generate sulfides of silver, copper, and nickel, and a certain silver and nickel mixture may also exist, thereby improving the conductivity of the cashmere fabric. Compared with the woolen cashmere fabric added with an antistatic agent, the antistatic woolen cashmere fabric prepared by the present invention has significantly improved antistatic performance and washing resistance. DETAILED DESCRIPTION
[0024] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0025] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the technical solution of the present application will be described in detail below in conjunction with specific embodiments.
[0026] The test materials used in the examples of the present invention are all conventional test materials in the art and can be purchased through commercial channels.
[0027] The penetrant used in the present invention was purchased from Weifang Jintai Material Factory, and the model is penetrant JFC.
[0028] The antistatic agent used in the present invention is purchased from Guangdong Tiansheng Environmental Protection New Material Technology Co., Ltd., and the model is HIT-STATSNO9 antistatic agent.
[0029] The cashmere fabric specifications of the present application examples and comparative examples are: 12 metric yarns, weight: 500 g / m 2 , width 1.8 meters.
[0030] Example 1: Preparation of antistatic cashmere fabric:
[0031] (1) placing pure cashmere fiber in a penetrant JFC solution (1% mass concentration), washing at 55° C. for 20 min, dehydrating and drying to obtain pretreated cashmere fiber;
[0032] (2) immersing the pretreated pure cashmere fiber into a metal ion solution with a mass concentration of 5%, and the bath ratio of the pretreated pure cashmere fiber to the metal ion solution is 1:50;
[0033] The reaction was carried out at 40°C for 4 hours, and then dried to obtain cashmere fibers with metal ions; the solute of the metal ion solution was a mixture of silver nitrate, copper sulfate and nickel sulfate in a mass ratio of 1:1.5:0.5, and the solvent was water;
[0034] (3) immersing the cashmere fiber with metal ions obtained in step (2) into a sulfide-reducing solution with a mass concentration of 10%, wherein the bath ratio of the cashmere fiber with metal ions to the sulfide-reducing solution is 1:50;
[0035] The solute of the sulfide reduction solution is composed of sodium sulfide and sodium sulfate in a mass ratio of 1:1, and the solvent is water; the solution is reacted at 80°C for 4 hours, and after cooling, the solution is taken out, rinsed and dried to obtain antistatic cashmere fiber;
[0036] (4) adding antistatic cashmere fiber at a weight ratio of 10% and uniformly mixing with dyed cashmere fiber, and subjecting the mixture to a strip making machine, a drawing machine, a roving machine, a spinning machine, and a bobbin winder to produce cashmere yarn with antistatic function; subjecting the cashmere yarn with antistatic function to warping, reeding, and weaving to produce cashmere grey cloth with antistatic function; subjecting the cashmere grey cloth with antistatic function to washing, shrinking, washing, drying, raising, smoothing, ironing, shearing, and steaming to produce cashmere fabric with antistatic function.
[0037] Example 2: Preparation of antistatic cashmere fabric:
[0038] (1) pure cashmere fiber is processed through wool blending, combing, slivering, roving, spun yarn, winding, warping, reeding and weaving to prepare pure cashmere grey cloth; the pure cashmere grey cloth is processed through washing, shrinking, washing and drying to prepare semi-finished pure cashmere fabric to be dyed and finished; the semi-finished pure cashmere fabric is placed in a penetrant JFC solution (1% mass concentration), washed at 55° C. for 20 minutes, dehydrated and dried to obtain a pre-treated semi-finished pure cashmere fabric;
[0039] (2) immersing the pretreated semi-finished pure wool velvet fabric into a metal ion solution with a mass concentration of 2%, and the bath ratio of the pretreated semi-finished pure wool velvet fabric and the metal ion solution is 1:50;
[0040] The reaction was carried out at 40°C for 4 hours, and then dried to obtain cashmere fabric with metal ions; the solute of the metal ion solution was a mixture of silver nitrate, copper sulfate and nickel sulfate in a mass ratio of 1:1.5:0.5, and the solvent was water;
[0041] (3) immersing the cashmere fabric with metal ions obtained in step (2) into a sulfide-reducing solution with a mass concentration of 4%, wherein the bath ratio of the cashmere fabric with metal ions to the sulfide-reducing solution is 1:50;
[0042] The solute of the sulfide reduction solution is composed of sodium sulfide and sodium sulfate in a mass ratio of 1:1, and the solvent is water; the solution is reacted at 80°C for 4 hours, and after cooling, the solution is taken out, rinsed and dried to obtain an antistatic cashmere fabric;
[0043] (4) The anti-static cashmere fabric is made into a finished anti-static functional cashmere fabric through dyeing, raising, smoothing, ironing, shearing and steaming processes.
[0044] Comparative Example 1:
[0045] (1) placing pure cashmere fiber in a penetrant JFC solution (1% mass concentration), washing at 55° C. for 20 min, dehydrating and drying to obtain pretreated cashmere fiber;
[0046] (2) immersing the pretreated pure cashmere fiber into an antistatic agent solution with a mass concentration of 5%, wherein the bath ratio of the pretreated wool fiber to the antistatic agent solution is 1:50; reacting at 40° C. for 4 hours, and drying after the reaction to obtain the antistatic cashmere fiber;
[0047] (3) Antistatic cashmere fiber is added in a mass ratio of 10% and uniformly mixed with dyed cashmere fiber, and the mixture is processed into cashmere yarn with antistatic function through a strip making machine, a drawing machine, a roving machine, a spinning machine, and a bobbin winder; the cashmere yarn with antistatic function is processed into cashmere grey cloth with antistatic function through warping, reeding, and weaving; the cashmere grey cloth with antistatic function is processed into cashmere fabric with antistatic function through washing, shrinking, washing, drying, raising, smoothing, ironing, shearing, and steaming.
[0048] The difference between this comparative example and Example 1 is that the antistatic cashmere fiber is prepared by treatment with an antistatic agent.
[0049] Comparative Example 2:
[0050] (1) pure cashmere fiber is processed through wool blending, combing, slivering, roving, spun yarn, winding, warping, reeding and weaving to prepare pure cashmere grey cloth; the pure cashmere grey cloth is processed through washing, shrinking, washing and drying to prepare semi-finished pure cashmere fabric to be dyed and finished; the semi-finished pure cashmere fabric is placed in a penetrant JFC solution (1% mass concentration), washed at 55° C. for 20 minutes, dehydrated and dried to obtain a pre-treated semi-finished pure cashmere fabric;
[0051] (2) immersing the pretreated semi-finished pure wool fabric into an antistatic agent solution with a mass concentration of 2%, wherein the bath ratio of the pretreated wool fiber and the antistatic agent solution is 1:50; reacting at 40° C. for 4 hours, and drying after the reaction to obtain an antistatic cashmere fabric;
[0052] (3) The anti-static cashmere fabric is made into a finished anti-static functional cashmere fabric through dyeing, raising, smoothing, ironing, shearing and steaming processes.
[0053] The difference between this comparative example and Example 2 is that the antistatic cashmere fabric is prepared by treatment with an antistatic agent.
[0054] Comparative Example 3:
[0055] (1) pure cashmere fiber is processed through wool blending, combing, slivering, roving, spun yarn, winding, warping, reeding and weaving to prepare pure cashmere grey cloth; the pure cashmere grey cloth is processed through washing, shrinking, washing and drying to prepare semi-finished pure cashmere fabric to be dyed and finished; the semi-finished pure cashmere fabric is placed in a penetrant JFC solution (1% mass concentration), washed at 55° C. for 20 minutes, dehydrated and dried to obtain a pre-treated semi-finished pure cashmere fabric;
[0056] (2) immersing the pretreated semi-finished pure wool fabric into a silver nitrate solution with a mass concentration of 2%, wherein the bath ratio of the pretreated semi-finished pure wool fabric to the silver nitrate solution is 1:50; reacting at 40° C. for 4 hours, and drying after the reaction to obtain a cashmere fabric with metal ions;
[0057] (3) immersing the cashmere fabric with metal ions obtained in step (2) into a sulfide-reducing solution with a mass concentration of 4%, wherein the bath ratio of the cashmere fabric with metal ions to the sulfide-reducing solution is 1:50;
[0058] The solute of the sulfide reduction solution is composed of sodium sulfide and sodium sulfate in a mass ratio of 1:1, and the solvent is water; the solution is reacted at 80°C for 4 hours, and after cooling, the solution is taken out, rinsed and dried to obtain an antistatic cashmere fabric;
[0059] (4) The anti-static cashmere fabric is made into a finished anti-static functional cashmere fabric through dyeing, raising, smoothing, ironing, shearing and steaming processes.
[0060] The difference between this comparative example and Example 2 is that silver nitrate solution is used instead of the metal ion solution in Example 2.
[0061] Comparative Example 4:
[0062] (1) pure cashmere fiber is processed through wool blending, combing, slivering, roving, spun yarn, winding, warping, reeding and weaving to prepare pure cashmere grey cloth; the pure cashmere grey cloth is processed through washing, shrinking, washing and drying to prepare semi-finished pure cashmere fabric to be dyed and finished; the semi-finished pure cashmere fabric is placed in a penetrant JFC solution (1% mass concentration), washed at 55° C. for 20 minutes, dehydrated and dried to obtain a pre-treated semi-finished pure cashmere fabric;
[0063] (2) immersing the pretreated semi-finished pure wool fabric into a copper sulfate solution with a mass concentration of 2%, wherein the bath ratio of the pretreated semi-finished pure wool fabric to the copper sulfate solution is 1:50; reacting at 40° C. for 4 hours, and drying after the reaction to obtain a cashmere fabric with metal ions;
[0064] (3) immersing the cashmere fabric with metal ions obtained in step (2) into a sulfide-reducing solution with a mass concentration of 4%, wherein the bath ratio of the cashmere fabric with metal ions to the sulfide-reducing solution is 1:50;
[0065] The solute of the sulfide reduction solution is composed of sodium sulfide and sodium sulfate in a mass ratio of 1:1, and the solvent is water; the solution is reacted at 80°C for 4 hours, and after cooling, the solution is taken out, rinsed and dried to obtain an antistatic cashmere fabric;
[0066] (4) The anti-static cashmere fabric is made into a finished anti-static functional cashmere fabric through dyeing, raising, smoothing, ironing, shearing and steaming processes.
[0067] The difference between this comparative example and Example 2 is that copper sulfate solution is used instead of the metal ion solution in Example 2.
[0068] Comparative Example 5:
[0069] (1) pure cashmere fiber is processed through wool blending, combing, slivering, roving, spun yarn, winding, warping, reeding and weaving to prepare pure cashmere grey cloth; the pure cashmere grey cloth is processed through washing, shrinking, washing and drying to prepare semi-finished pure cashmere fabric to be dyed and finished; the semi-finished pure cashmere fabric is placed in a penetrant JFC solution (1% mass concentration), washed at 55° C. for 20 minutes, dehydrated and dried to obtain a pre-treated semi-finished pure cashmere fabric;
[0070] (2) immersing the pretreated semi-finished pure cashmere fabric into a nickel sulfate solution with a mass concentration of 2%, wherein the bath ratio of the pretreated semi-finished pure cashmere fabric to the nickel sulfate solution is 1:50; reacting at 40° C. for 4 hours, and drying after the reaction to obtain a cashmere fabric with metal ions;
[0071] (3) immersing the cashmere fabric with metal ions obtained in step (2) into a sulfide-reducing solution with a mass concentration of 4%, wherein the bath ratio of the cashmere fabric with metal ions to the sulfide-reducing solution is 1:50;
[0072] The solute of the sulfide reduction solution is composed of sodium sulfide and sodium sulfate in a mass ratio of 1:1, and the solvent is water; the solution is reacted at 80°C for 4 hours, and after cooling, the solution is taken out, rinsed and dried to obtain an antistatic cashmere fabric;
[0073] (4) The anti-static cashmere fabric is made into a finished anti-static functional cashmere fabric through dyeing, raising, smoothing, ironing, shearing and steaming processes.
[0074] The difference between this comparative example and Example 2 is that nickel sulfate solution is used instead of the metal ion solution in Example 2.
[0075] Comparative Example 6:
[0076] (1) preparing pure cashmere fabric by wool blending, combing, drawing, roving, spun yarn, winding, warping, reeding and weaving pure cashmere fiber, and preparing semi-finished pure cashmere fabric to be dyed and finished by washing, shrinking, washing and drying the pure cashmere fabric;
[0077] (2) The semi-finished pure cashmere fabric is made into the finished pure cashmere fabric through dyeing, raising, smoothing, ironing, shearing and steaming processes.
[0078] The difference between this comparative example and Example 2 is that the pure cashmere fabric is prepared by conventional process without antistatic treatment.
[0079] Test example:
[0080] 1. Refer to "GB / T12703.2-2021 Test method for electrostatic properties of textiles Part 2: Manual friction method" to test the charge surface density of Examples 1-2 and Comparative Examples 1-6;
[0081] 2. After washing 100 times according to GB / T8629-2017 "Household Washing and Drying Procedure for Textile Testing", the charge surface density of Examples 1-2 and Comparative Examples 1-6 was tested again according to GB / T12703.2-2021 Test Method for Electrostatic Properties of Textiles Part 2: Manual Friction Method;
[0082] The size of the test samples in each treatment group was (350±1) mm×(250±1) mm. The test results are shown in Table 1.
[0083] Table 1 Charge surface density after different treatments, friction and washing
[0084]
[0085] It can be seen from Table 1 that the charge surface density of the antistatic functional cashmere fabrics of Examples 1 and 2 of the present application is significantly lower than that of other treatment groups, and the antistatic effect is significant. In addition, Comparative Examples 1 and 2 are cashmere fabrics with added antistatic finishing agents. After washing 100 times, the charge surface density increases significantly, which is basically consistent with the charge surface density of the pure wool fabric without antistatic treatment in Comparative Example 6, and the antistatic functional cashmere fabrics of Examples 1 and 2 still have good antistatic effects.
[0086] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. An antistatic wool velvet fiber, characterized in that: Prepared by the following method: (1) immersing the pretreated pure wool fiber in a metal ion solution, reacting at 20-60° C. for 3-5 hours, and drying after the reaction to obtain wool fiber with metal ions; (2) immersing the wool plush fiber with metal ions obtained in step (1) into a sulfide reduction solution, reacting at 60-100° C. for 3-5 hours, cooling down, taking out, rinsing and drying, to obtain an antistatic wool plush fiber; In step (1), the mass concentration of the metal ion solution is 1-10%, the solute is a mixture of silver nitrate, copper sulfate and nickel sulfate in a mass ratio of (0.5-1.5): (1-2): (0.4-0.6), and the solvent is water.
2. The antistatic wool velvet fiber according to claim 1, characterized in that: In step (1), the pretreatment method is: putting the pure wool velvet fiber into a penetrant, washing it at 50-60° C. for 20 minutes, dehydrating and drying it to obtain the pretreated pure wool velvet fiber.
3. The antistatic wool velvet fiber according to claim 1, characterized in that: The pure wool fiber is one or more of cashmere fiber and wool fiber.
4. The antistatic wool velvet fiber according to claim 1, characterized in that: In step (1), the bath ratio of the pretreated wool fibers to the metal ion solution is 1:(10-50).
5. The antistatic wool velvet fiber according to claim 1, characterized in that: In step (2), the mass concentration of the sulfide-reducing solution is 2-20%, the solute is one or more of sodium sulfide, sodium thiosulfate, and sodium sulfate, and the solvent is water.
6. The antistatic wool velvet fiber according to claim 1, characterized in that: In step (2), the bath ratio of the wool fibers with metal ions to the sulfide reduction solution is 1:(10-50).
7. Use of the antistatic wool plush fiber according to any one of claims 1 to 6 in the preparation of antistatic wool plush products.
8. The use according to claim 7, characterized in that: The antistatic wool plush product is an antistatic wool plush fabric. 9.An antistatic wool velvet fabric, characterized in that: Prepared by the following method: The antistatic wool velvet fiber according to any one of claims 1 to 6 is added in a mass ratio of 1% to 10% and mixed evenly with wool velvet fibers that have not been treated with antistatic treatment, and the antistatic functional wool velvet fabric is obtained through blending, weaving, dyeing and finishing; Or immerse the pretreated semi-finished pure wool plush fabric into a metal ion solution for reaction to obtain a wool plush fabric with metal ions; immerse the wool plush fabric with metal ions into a sulfide reduction solution for reaction to obtain an antistatic wool plush fabric; the mass concentration of the metal ion solution is 1-10%, the solute is a mixture of silver nitrate, copper sulfate, and nickel sulfate in a mass ratio of (0.5-1.5): (1-2): (0.4-0.6), and the solvent is water; The pretreatment method comprises: placing the semi-finished pure wool velvet fabric into a penetrant, washing it at 50-60° C. for 20 minutes, dehydrating and drying it to obtain the pretreated semi-finished pure wool velvet fabric.
10. The antistatic wool velvet fabric according to claim 9, characterized in that: The semi-finished pure wool plush fabric is made of pure wool plush fiber through wool blending, combing, drawing, roving, spun yarn, winding, warping, reeding and weaving to make pure wool plush grey cloth, and the pure wool plush grey cloth is washed, shrunk, washed and dried to make the semi-finished pure wool plush fabric to be dyed and finished.