Paper pulp composition, paperboard composition and preparation method and application thereof
By using a specific pulp composition, including reinforcing agents and retention and filtration aids, in the cardboard composition, the interfiber bonding force is enhanced, solving the problem of low internal bonding strength in black core cardboard. This enables the preparation of cardboard with high internal bonding strength and folding endurance, and reduces production costs.
Patent Information
- Application Number
- CN202411147822.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-15
AI Technical Summary
The existing black core cardboard has low internal bonding strength and insufficient folding endurance, which makes it easy to delaminate and deform during use, making it difficult to meet the requirements of high-end cardboard.
A paperboard composition with high internal bond strength and folding endurance is prepared by using a pulp composition, including papermaking pulp, reinforcing agents such as corn cationic starch and cassava cationic starch, internal sizing agents and retention and filtration aids. The binding force between fibers is enhanced by hydrogen bonding, and the retention effect of fine fibers is improved by using water-soluble branched organic polymers.
It improves the internal bonding strength and folding endurance of the cardboard composition, ensures shape stability during use, prevents delamination and deformation, extends service life, and reduces production costs.
Smart Images

Figure CN118958033A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of papermaking, and in particular to a pulp slurry composition, a cardboard composition, and a preparation method and application thereof. Background Art
[0002] As a new type of cardboard, black core cardboard needs to have folding resistance, internal bonding strength, flexibility and elasticity. It has a wide range of applications in high-end playing cards, scratch cards, game cards and other products.
[0003] At present, the method often used is to apply black core coating on base paper to make black core base paper, and then sandwich a layer of black core paper between two layers of paper and laminate them by machine to make black core cardboard. However, the process of this method is relatively complicated, and the internal bonding strength between the layers is low. It is easy to delaminate and deform during use, and it is difficult to meet the requirements of high-end black core cardboard. Summary of the invention
[0004] The object of the present invention is to provide a pulp slurry composition, a cardboard composition and a preparation method and application thereof, so as to prepare a cardboard composition with higher internal bonding strength and folding endurance.
[0005] In a first aspect, in order to achieve the above-mentioned object, the present invention provides a pulp slurry composition, comprising:
[0006] Papermaking pulp, a first reinforcing agent, a second reinforcing agent, an internal sizing agent and a retention and drainage aid; wherein the first reinforcing agent comprises at least one of corn cationic starch and cassava cationic starch; and / or the second reinforcing agent comprises at least one of corn starch and cassava starch; in terms of weight parts, the papermaking pulp is 90 to 110 parts, the first reinforcing agent is 1 to 2 parts, the second reinforcing agent is 3 to 6 parts, and the retention and drainage aid is 0.225 to 0.385 parts.
[0007] Compared with the prior art, the pulp slurry composition provided in the embodiment of the present invention includes papermaking pulp, a first reinforcing agent, a second reinforcing agent, an internal sizing agent and a retention and drainage aid. Among them, the first reinforcing agent includes at least one of corn cationic starch and cassava cationic starch, and the second reinforcing agent includes at least one of corn starch and cassava starch. In the pulp slurry composition provided in the embodiment of the present invention, since the cellulose molecules contained in the papermaking pulp have more hydroxyl groups on their surfaces, and the reinforcing agent contains more hydrogen bond forming groups, when 1 to 2 parts of the first reinforcing agent, 3 to 6 parts of the second reinforcing agent and 90 to 110 parts of the papermaking pulp are mixed by weight, they can "chemically hydrate" with the cellulose molecules, promote the hydrogen bond forming groups contained in the first reinforcing agent and the second reinforcing agent to form hydrogen bonds with the cellulose molecules of the papermaking pulp, enhance the bonding force between the fibers, and facilitate the preparation of a cardboard composition with high internal bonding strength and folding resistance. At the same time, although the two reinforcing agents are derived from the same or two different starches, they have similar properties, so they can be better combined during the mixing process with the paper pulp, evenly dispersed between the fibers of the pulp, increase the binding sites between the fibers, and improve the retention rate of fine fibers, which is conducive to the preparation of a cardboard composition with high binding strength. In addition, since the cost of the first reinforcing agent is higher than that of the second reinforcing agent, and the cost of the second reinforcing agent is lower than that of the paper pulp, by limiting the mass fractions of the first reinforcing agent, the second reinforcing agent and the paper pulp to the above range, it can not only ensure full combination with the pulp, but also reduce the production cost of the pulp slurry composition, which is conducive to the large-scale production of the pulp slurry composition.
[0008] In addition, the retention and drainage aid provided by the embodiment of the present invention is a water-soluble branched organic polymer. When the retention and drainage aid in the pulp slurry composition is 0.225 to 0.385 parts, it can have an excellent retention effect on fine fibers, which is not only conducive to the prepared cardboard composition having a higher internal bonding strength, but also conducive to the prepared cardboard composition having a higher folding resistance. At the same time, the pulp slurry composition provided by the embodiment of the present invention also includes an internal sizing agent, which has a hydrophilic group and a hydrophobic group, and can orient the outer side of the fiber surface of the papermaking pulp to a hydrophobic group, which is conducive to the prepared cardboard composition having hydrophobicity and resistance to fluid penetration, so that the prepared cardboard composition is not easy to be affected by moisture and mildew, and the service life is extended.
[0009] In a second aspect, the present invention further provides a cardboard composition, comprising: a coating and the above-mentioned pulp slurry composition.
[0010] In a third aspect, the present invention further provides a method for preparing a cardboard composition, comprising:
[0011] Step 1, mixing bleached chemical coniferous wood pulp and bleached chemical hardwood wood pulp to obtain papermaking pulp;
[0012] Step 2, adding a toner, a first reinforcing agent, a second reinforcing agent, an internal sizing agent and a retention and drainage aid to the papermaking slurry to obtain a pretreated slurry;
[0013] Step three, dehydrating and forming the pretreated slurry to obtain a wet paper sheet; performing a dehydration treatment, a first drying treatment, a first sizing with a surface sizing agent, a second drying treatment and a first calendering treatment on the wet paper sheet, and rolling up to obtain a paper base;
[0014] Step 4: forming a coating on one surface of the paper base, and performing a second sizing on the other surface of the paper base using a sizing material to obtain a cardboard composition.
[0015] In a fourth aspect, the present invention further provides an application of the above-mentioned pulp slurry composition or the above-mentioned cardboard composition or the preparation method of the above-mentioned cardboard composition in the preparation of black core cardboard.
[0016] Compared with the prior art, the beneficial effects of a cardboard composition and a preparation method and application thereof provided in the embodiment of the present invention are the same as the beneficial effects of the pulp slurry composition, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0018] Figure 1 The flowchart of the method for preparing the cardboard composition provided in the embodiment of the present invention is shown. DETAILED DESCRIPTION
[0019] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0020] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.
[0021] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "front", "back", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present disclosure.
[0022] It should be noted that, in the present invention, words such as "exemplary" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "exemplary" or "for example" in the present disclosure should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "exemplary" or "for example" is intended to present related concepts in a specific way.
[0023] In the present invention, "at least one" means one or more, and "plurality" means two or more. "And / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone, where A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items. For example, at least one of a, b or c can mean: a, b, c, the combination of a and b, the combination of a and c, the combination of b and c, or the combination of a, b and c, where a, b, c can be single or multiple.
[0024] In view of the problems of low internal bonding strength and low folding resistance of black core cardboard in the prior art, and easy delamination and deformation during use, an embodiment of the present invention provides a pulp slurry composition to prepare a cardboard composition with high internal bonding strength and folding resistance. The pulp slurry composition includes: papermaking pulp, a first reinforcing agent, a second reinforcing agent, an internal sizing agent and a retention and drainage aid. Among them, the first reinforcing agent includes at least one of corn cationic starch and cassava cationic starch. The second reinforcing agent includes at least one of corn starch and cassava starch.
[0025] In terms of weight percentage, the pulp slurry composition provided in the embodiment of the present invention includes 90 to 110 parts of papermaking pulp, 1 to 2 parts of a first reinforcing agent, 3 to 6 parts of a second reinforcing agent, and 0.225 to 0.385 parts of a retention and drainage aid.
[0026] It is understandable that, since the cellulose molecules contained in the paper pulp have more hydroxyl groups on their surfaces, and the reinforcing agent contains more hydrogen bond forming groups, when 1 to 2 parts of the first reinforcing agent and 3 to 6 parts of the second reinforcing agent react with 90 to 110 parts of the paper pulp, they can "chemically hydrate" with the cellulose molecules, prompting the hydrogen bond forming groups contained in the first reinforcing agent and the second reinforcing agent to form hydrogen bonds with the cellulose molecules of the paper pulp, thereby enhancing the binding force between the fibers, and facilitating the preparation of a cardboard composition with higher internal bonding strength and folding resistance. Since the cardboard composition has a higher internal bonding strength, its shape is stable during use, and it is not easy to delaminate and deform, which is conducive to extending the service life of the cardboard composition. At the same time, although these two reinforcing agents are derived from the same or two different starches, they have similar properties, so they can be better combined during the mixing process with the paper pulp, evenly dispersed in the pulp, increase the binding sites between the fibers, and improve the retention rate of fine fibers, which is conducive to the preparation of a cardboard composition with higher internal bonding strength and folding resistance. When the first reinforcing agent includes cassava cationic starch, at least one of cassava cationic starch XW8841, cassava cationic starch Statcat C26 and cassava cationic starch MICROCAT 600 can be selected. When the first reinforcing agent includes corn cationic starch, at least one of corn cationic starch FUYANG and corn cationic starch XINGMAO can be selected.
[0027] It should be understood that the sources of corn starch and cassava starch included in the second reinforcing agent provided in the embodiment of the present invention can be adjusted according to actual conditions and are not limited here. Since the cost of the first reinforcing agent is higher than that of the second reinforcing agent, and the cost of the second reinforcing agent is lower than that of the papermaking pulp, by limiting the mass fractions of the first reinforcing agent, the second reinforcing agent and the papermaking pulp to the above range, it can not only ensure full combination with the pulp, but also reduce the production cost of the pulp slurry composition, which is conducive to the large-scale production of the pulp slurry composition.
[0028] At the same time, the retention and drainage aid provided by the embodiment of the present invention is a water-soluble branched organic polymer, and at least one of cationic polyacrylamide, anionic polyacrylamide, cationic starch and bentonite can be selected. When the pulp slurry composition includes 0.225 to 0.385 parts of the retention and drainage aid, it can have an excellent retention effect on fine fibers, which is not only conducive to the prepared cardboard composition having a strong internal bonding strength, but also conducive to the prepared cardboard composition having a good folding resistance.
[0029] At the same time, the pulp slurry composition provided by the embodiment of the present invention also includes an intra-slurry sizing agent, which has a hydrophilic group and a hydrophobic group, and can orient the outer side of the fiber surface of the papermaking pulp into a hydrophobic group, which is beneficial for the prepared cardboard composition to have hydrophobicity and resistance to fluid permeability, so that the prepared cardboard composition is not easily affected by moisture and mildew, thereby extending the service life.
[0030] Exemplarily, the internal sizing agent in the pulp slurry composition provided in the embodiment of the present invention includes at least one of alkyl ketene dimer, alkenyl succinic anhydride, and cationic dispersed rosin size. The internal sizing agent is 0.1 to 2 parts by weight. Within this range, the internal sizing agent can fully react with the papermaking slurry, so that the prepared cardboard composition has a certain water resistance and is not easily wetted by water or aqueous solution to a certain extent.
[0031] Exemplarily, the papermaking pulp in the pulp slurry composition provided in the embodiment of the present invention includes bleached chemical coniferous pulp and bleached chemical hardwood pulp, both of which are derived from whole wood pulp, which can effectively utilize forest resources and improve carbon sequestration capacity. Among them, in terms of mass parts, the present invention limits the bleached chemical coniferous pulp to 30 to 40 parts, and the bleached chemical hardwood pulp to 60 to 70 parts, which is beneficial to improve the strength of the prepared paper. When the chemical coniferous pulp is less than 30 parts, it will affect the internal bonding strength of the prepared cardboard composition, reduce the flexibility of the paper, and thus reduce the folding resistance of the paper. When the chemical coniferous pulp is higher than 40 parts, the production cost is high, and the strength of the prepared paper cannot be significantly improved.
[0032] In an optional manner, the pulp slurry composition provided by the embodiment of the present invention also includes a toner, which includes at least one of a whitening agent, a blue dye and a purple dye. Wherein, the whitening agent can adjust the whiteness of the papermaking pulp, and the mixture of the blue dye and the purple dye can adjust the hue of the papermaking pulp. Specifically, the whitening agent used in the present invention includes at least one of a disulfonic acid liquid whitening agent, a tetrasulfonic acid liquid whitening agent, and a hexasulfonic acid liquid whitening agent. The whitening agent of the above type has good water solubility and stable performance, which is conducive to preparing a cardboard composition with stable color. In addition, the blue dye and the purple dye used in the present invention are liquid dyes, which replace traditional solid dyes, and reduce the probability of dye spots and uneven coloring in the papermaking pulp due to the inability of the solid dye to be completely dissolved. Wherein, the blue dye includes at least one of blue dye 3R-EVliq, blue dye Lrgalite Blue RL and blue dye PT-21. The purple dye includes at least one of purple dye 3B-Fliq, purple dye Lrgalite Violet BL, purple dye PVA and purple dye PA-11. The liquid dye is a water-soluble anionic dye. The reactive groups in the dye molecules can combine with the cellulose molecules in the papermaking pulp by van der Waals forces and hydrogen bonds, which is beneficial for preparing a cardboard composition with high color uniformity.
[0033] Exemplarily, the pulp slurry composition provided by the embodiment of the present invention includes 0.1 to 0.6 parts of a whitening agent, 0 to 0.02 parts of a blue dye, and 0 to 0.04 parts of a purple dye, by weight. Within the above range, when the toner reacts with the papermaking slurry, it is beneficial to prepare a paperboard composition with a stable color and high uniformity. It should be understood that in order to save costs, dyes can be added in other papermaking processes, which can be adjusted according to actual needs and are not limited here.
[0034] The embodiment of the present invention also provides a cardboard composition, which includes a coating and the above-mentioned pulp slurry composition. The mass ratio of the coating to the pulp is (13-16):70. Within this range, the coating can completely cover the paper prepared from the pulp, so that the cardboard composition can have better physical and optical properties.
[0035] In an optional manner, the coating in the embodiment of the present invention includes a primer and a top coat, wherein the primer has a weight of 8 g / m 2 ~14g / m 2 The weight of the top coating is 8g / m 2 ~14g / m 2 .
[0036] Exemplarily, the primer layer in the embodiment of the present invention includes calcium carbonate, latex, defoamer, dispersant, coating starch, whitening agent, water repellent, lubricant, pH regulator and thickener. According to the mass parts, the cardboard composition includes: calcium carbonate is 90 parts to 100 parts, latex is 8 parts to 15 parts, defoamer is 0.2 parts to 0.5 parts, dispersant is 0.1 parts to 0.5 parts, coating starch is 2 parts to 5 parts, whitening agent is 0.1 parts to 0.3 parts, water repellent is 0.2 parts to 0.3 parts, lubricant is 0.2 parts to 0.3 parts, pH regulator is 0.01 parts to 0.05 parts and thickener is 0.1 parts to 0.3 parts. The cardboard composition of the embodiment of the present invention can ensure that the solid matter of the base coating is evenly distributed under the joint action of calcium carbonate, latex, defoaming agent, dispersant, coating starch, brightener, water repellent, lubricant, pH regulator and thickener, and each formula has good compatibility, thereby ensuring that the cardboard composition is not prone to phase separation during use, thereby extending the service life of the cardboard composition.
[0037] Specifically, the calcium carbonate in the embodiment of the present invention includes at least one of 65-grade ground calcium carbonate, 95-grade ground calcium carbonate and A40 reactive calcium carbonate, which has a relatively small and uniform particle size, stable chemical properties, is not easy to react with acids and alkalis, will not undergo oxidation or reduction, is insoluble or not easily soluble in water, has a large hiding power, refractive index and scattering coefficient, can not only improve the opacity of paper, make the cardboard printing details clear, but also improve the flatness and uniformity of paper. The latex in the embodiment of the present invention is an imported latex, including at least one of BASF's styrene butadiene latex Styronal 316CN, carboxylated styrene butadiene latex Styronal 300D CN and carboxylated styrene butadiene latex Styronal 302G, which can improve the coating strength of paper. The defoamer provided in the embodiment of the present invention includes at least one of nonionic organosilicon emulsion, dimethyl silicone oil and fumed silica to inhibit and eliminate the foam formed by various factors in the papermaking process. The dispersant in the embodiment of the present invention includes at least one of sodium polyacrylate, alkylphenol polyoxyethylene ether and phosphate (such as sodium hexametaphosphate) to reduce the viscosity of high-concentration coating so that it has good rheological properties. The coating starch in the embodiment of the present invention includes at least one of phosphate coating starch XC6225 and carboxymethyl coating starch CMS to enhance the film-forming property of the primer. The water-repellent in the embodiment of the present invention includes at least one of amino resin, zirconium salt (such as zirconium sulfate amine, zirconium carbonate amine), modified polyamide polyamine epichlorohydrin resin, and polyamide polyurea resin to improve the water resistance of the coating, so that the cardboard composition has mildew resistance. The lubricant in the embodiment of the present invention includes at least one of metal soap lubricant (such as calcium stearate), fluorine lubricant (such as perfluoropolyether), sulfated oil and sulfonated oil to reduce interfacial tension, improve the smoothness and fluidity of the wet coating surface, and make it easy to level and spread on paper, improve the coating adaptability of the coating, and improve the finished product performance of the coating by reducing or eliminating fuzzing and powdering. The pH regulator in the embodiment of the present invention includes at least one of sodium hydroxide, potassium hydroxide and ammonium hydroxide, so as to adjust the pH in the coating to an appropriate range, which is conducive to enhancing the compatibility between the various components. The thickener in the embodiment of the present invention includes at least one of polyacrylamide, polyvinyl alcohol and carboxymethyl cellulose, which can change the rheological properties of the coating and increase the viscosity and consistency of the coating.
[0038] Exemplarily, the topcoat in the embodiment of the present invention includes calcium carbonate, china clay, latex, defoamer, dispersant, brightener, dye, water repellent, lubricant, pH regulator, thickener and rheological agent. Wherein, according to the mass parts, the cardboard composition includes: calcium carbonate is 70 parts to 90 parts, china clay is 7 parts to 30 parts, latex is 10 parts to 20 parts, defoamer is 0.1 parts to 0.5 parts, dispersant is 0.1 parts to 0.3 parts, brightener is 0.05 parts to 0.8 parts, dye is 0.002 parts to 0.06 parts, water repellent is 0.1 parts to 0.3 parts, lubricant is 0.1 parts to 0.3 parts, pH regulator is 0.2 parts to 0.4 parts, thickener is 0.03 parts to 0.07 parts and rheological agent is 0.1 parts to 0.3 parts. Wherein, the calcium carbonate in the embodiment of the present invention includes at least one of 97-grade ground calcium carbonate, 95-grade ground calcium carbonate and reactive calcium carbonate A40, and its particle size is finer and more uniform than the calcium carbonate in the primer coating, and its adhesion in the coating is stronger. The porcelain clay in the embodiment of the present invention includes at least one of Brazilian porcelain clay KAOLIN AMAZON PREMIUMSD and American porcelain clay SNOW*TEX 45, which replaces a part of the calcium carbonate to further enhance the glossiness of the cardboard composition, preferably 7 to 15 parts. The latex in the embodiment of the present invention includes at least one of styrene butadiene latex Styronal 316CN, carboxylated styrene butadiene latex Styronal 300D CN and carboxylated styrene butadiene latex Styronal302G to improve the coating strength of the cardboard composition and enhance the surface properties of the cardboard composition. When 14 to 20 parts of latex are used in the topcoat, it is more conducive to improving the surface properties of the cardboard composition. The dye in the embodiment of the present invention includes a blue dye and a purple dye, wherein the blue dye is 0.001 to 0.02 parts, and the purple dye is 0.001 to 0.04 parts. The rheological agent in the embodiment of the present invention includes at least one of hydroxyethyl cellulose, polyvinyl alcohol and polyacrylate, so that the coating maintains a high viscosity, maintains the stability of the coating system, and prevents the precipitation of the dye. The water repellent in the embodiment of the present invention includes at least one of glyoxal urea polymer 1671, glyoxal urea polymer DD-2 and polyamide polyamine epichlorohydrin resin NCC-1695, which reduces the water solubility of the coating adhesive to provide maximum wet friction resistance and wet pick strength, preferably 0.05 to 0.09 parts.
[0039] In practical applications, the whiteness of the cardboard composition can be adjusted according to actual needs. When the whiteness requirement of the cardboard composition is high, the top coating of the cardboard composition can include, by weight, 70 to 90 parts of calcium carbonate, 10 to 30 parts of china clay, 10 to 20 parts of latex, 0.1 to 0.5 parts of defoaming agent, 0.1 to 0.3 parts of dispersant, 0.5 to 0.8 parts of whitening agent, 0.01 to 0.02 parts of blue dye, 0.01 to 0.04 parts of purple dye, 0.1 to 0.3 parts of water repellent, 0.1 to 0.3 parts of lubricant, 0.2 to 0.4 parts of pH regulator, 0.03 to 0.07 parts of thickener and 0.1 to 0.3 parts of rheological agent.
[0040] When the whiteness requirement of the cardboard composition is low, the top coating of the cardboard composition may include, by weight: 70 to 90 parts of calcium carbonate, 10 to 30 parts of china clay, 10 to 20 parts of latex, 0.1 to 0.5 parts of defoaming agent, 0.1 to 0.3 parts of dispersant, 0.05 to 0.49 parts of whitening agent, 0.001 to 0.009 parts of blue dye, 0.001 to 0.009 parts of purple dye, 0.1 to 0.3 parts of water repellent, 0.1 to 0.3 parts of lubricant, 0.2 to 0.4 parts of pH regulator, 0.03 to 0.07 parts of thickener and 0.1 to 0.3 parts of rheological agent. It can be seen that the embodiment of the present invention can be freely adjusted according to actual needs.
[0041] In an optional manner, the cardboard composition provided by the embodiment of the present invention also includes a surface sizing agent, which includes at least one of an alkyl ketene dimer and a styrene acrylic copolymer dispersion. When the cardboard composition includes 0.1 to 2 parts of the surface sizing agent by weight, it replaces the limitation of adding only alkyl ketene dimer or a ternary polymer composed of acrylonitrile, styrene, and acrylic rubber in the pulp, so as to form a layer of liquid-resistant film on the surface of the cardboard composition, further improving the water resistance of the paper. Under the joint action of the sizing agent in the pulp and the surface sizing agent, not only can the moisture-proof performance of the cardboard composition be improved, but also the strength and stiffness of the cardboard composition can be increased, the printing performance of the cardboard composition can be improved, the friction resistance and durability of the cardboard composition can be improved, and the probability of hair loss and powder loss of the cardboard composition can be reduced.
[0042] The invention also provides a method for preparing the cardboard composition. Figure 1 FIG. 2 is a flow chart showing a method for preparing a cardboard composition provided in an embodiment of the present invention. Figure 1 As shown, the preparation method of the cardboard composition comprises:
[0043] Step 1: Mix bleached chemical coniferous wood pulp and bleached chemical hardwood wood pulp to obtain papermaking pulp.
[0044] Exemplarily, the bleached chemical coniferous pulp can be first crushed and deslagging, and then refined to separate the fibers of the coniferous pulp and improve the bonding strength between paper fibers. Next, the bleached chemical hardwood pulp can be crushed and deslagging, and then refined to separate the fibers of the hardwood pulp and improve the bonding strength between paper fibers. Finally, after the above two pulps are mixed, further refining is performed to fully mix the fibers of the coniferous pulp and the fibers of the hardwood pulp, and the mixed fibers are de-cluttered, cut and separated to improve the bonding strength between paper fibers, folding endurance, tensile strength and paper uniformity. After the above operations are completed, they enter the pre-copying pool for standby.
[0045] In practical applications, after the softwood pulp is broken by the pulper, it is removed by a high-concentration cleaner, and then it is initially refined by a softwood cylindrical mill, and then it is refined by two large-taper refiners in series. The main function of the refiner is to cut and separate the fibers. Compared with refining equipment such as double-disc mills, it has low energy consumption and low maintenance costs. After the hardwood pulp is broken by the pulper, it is removed by a high-concentration cleaner, and then it is refined by two groups of two parallel large-taper refiners. The grinding tooth width and tooth groove width of the hardwood refiner are narrower than those of the coniferous refiner, and the refining effect is obvious. It can separate the fibers and improve the bonding force between paper fibers. At the same time, the taper refiner has low energy consumption for refining, which is conducive to reducing energy consumption. Then, the above two pulps are mixed according to the pulping requirements and then enter the mixing pulp tank for uniform mixing, and then refined by the leveling refiner to de-clutter, cut and separate the mixed fibers.
[0046] It is worth mentioning that the large-taper refiner is used for continuous beating of long-fiber pulp (such as coniferous wood pulp and hardwood pulp) or uniform beating of waste paper recycled pulp after defibrination. Defibrination refers to the process of separating plant raw materials into fine fibers, the purpose of which is to make fiber pulp. Fiberization refers to the phenomenon of fluffing, tearing, fiberization, and fiberization of the fiber cell wall after pulping in pulping and papermaking production. It should be understood that the model of the mechanical device used in this step can be adjusted according to actual needs and is not limited here.
[0047] Exemplarily, in step one, the disintegration concentration of the papermaking pulp is 4.5% to 5.0%. Increasing the disintegration concentration of the papermaking pulp is beneficial to improving the quality of subsequent pulping, ensuring that the disintegration concentration of the papermaking pulp meets expectations, and reducing the adverse effects on the production capacity of the paper machine caused by the low disintegration concentration of the papermaking pulp. At the same time, the beating degree of coniferous pulp is 34°SR to 42°SR, the beating degree of broadleaf pulp is 27°SR to 35°SR, and the beating degree of the papermaking pulp obtained after mixing is 31°SR to 39°SR. Within this range, the bonding force between fibers increases with the increase of the beating degree, which is beneficial to the preparation of a more delicate, good feel, high folding resistance, high internal bonding strength, and good uniformity cardboard composition. The pre-papermaking pool is the pulp pool before the pulp enters the paper machine flow system, also called the pulping pool. The pulp fiber ratio and concentration in the pre-papermaking pool are already quite stable and meet the papermaking requirements.
[0048] Step 2: Add a colorant, a first reinforcing agent, a second reinforcing agent, an internal sizing agent and a retention and drainage aid into the papermaking pulp to obtain a pretreated pulp.
[0049] In practical applications, in order to obtain pre-treated pulp, the papermaking pulp needs to be first transferred from the pre-cutting pool to the first stage desander pump (also called a first stage flushing pump) through the sizing pump. At this time, the first reinforcing agent can be added to the papermaking pulp at the inlet of the sizing pump. By using at least one of corn cationic starch and cassava cationic starch as the first reinforcing agent, a stable generation amount can be provided, and the continuous cooking effect is good. In addition, in the process of combining with the papermaking pulp, it can better "chemically hydrate" with the cellulose molecules, so that the hydrogen bond forming groups contained in the first reinforcing agent form hydrogen bonds with the cellulose molecules of the papermaking pulp, which enhances the bonding force between the fibers and is conducive to the preparation of a cardboard composition with high internal bonding strength and folding resistance. Then, the papermaking pulp is mixed and pumped to the first stage desander through a first stage desander pump. In this process, a colorant can be added to the inlet of the first stage desander pump, and a second reinforcing agent and an internal sizing agent can be added to the inlet of the second stage flushing pump. In the process of pumping by the first stage desander pump, the blue dye, purple dye and whitening agent included in the colorant can be fully mixed with the paper pulp and attached to the fibers of the paper pulp by chemical bonds, so that the optical properties such as the uniformity of paper coloring are greatly improved. The second reinforcing agent replaces the currently commonly used method of adding cationic starch, which can reduce costs while enhancing the bonding force between fibers, which is conducive to the preparation of a cardboard composition with high internal bonding strength and folding resistance. The internal sizing agent uses at least one of alkyl ketene dimer, alkenyl succinic anhydride and cationic dispersed rosin glue, replacing the currently commonly used method of adding alkyl ketene dimer, so that the paper has good water resistance and less system hydrolysis products. In addition, retention and filtration aids can be added at the inlet and outlet of the paper machine screen, and fully mixed with the papermaking pulp containing other chemical additives to form a pre-treated pulp, which can have an excellent retention effect on fine fibers and calcium carbonate fillers, not only conducive to the prepared cardboard composition having a strong internal bonding strength, but also conducive to the prepared cardboard composition having a good folding resistance. Finally, the impurities in the pre-treated pulp are screened out, and the filtered pre-treated pulp is used as a standby before papermaking.
[0050] It is understandable that in the process of pumping the mixed papermaking pulp to the paper machine screen by using the pre-tank pulp pump, it is necessary to remove sand and gas to reduce the impurities and air content in the prepared pre-treated pulp. The desander used in this process is a five-stage desander, and the flushing pump used is a two-stage flushing pump.
[0051] Specifically, when the pulp in the fore-papermaking pool is sent to the first-stage flushing pump via the external white water tank, a toner can be added to the inlet of the first-stage flushing pump to make the toner and the papermaking pulp fully mixed and uniform. Subsequently, the papermaking pulp is sequentially desanded through the first to fifth desanders. The first desander is used to desand the pulp sent by the first-stage flushing pump, and the tail pulp is sent to the second desander. Starting from the second desander, the good pulp after desanding in each desander can be returned to the upper desander for re-desanding, and the tail pulp is sent to the next desander for further desanding until the papermaking pulp is separated from the heavy impurities therein. At this time, the impurities will be discharged into the impurity treatment place (such as: ditch) by the fifth desander, and the good papermaking pulp after the heavy impurities are removed will be sent to the degasser by the first desander to remove the gas brought by the papermaking pulp and the gas generated during the pulping and transportation process, so as to reduce the probability of bubbles in the manufactured paperboard composition. Next, the papermaking slurry is sent from the degasser to the second-stage flushing pump. At this time, the second reinforcing agent and the sizing agent in the slurry can be added at the inlet of the second-stage flushing pump, so that the above-mentioned additives are fully mixed with the papermaking slurry in the second-stage flushing pump to increase the bonding force and water resistance between fibers. Finally, the pretreated slurry is screened out of impurities in the pretreated slurry through the paper machine screen. The filtered pretreated slurry is used as a standby before papermaking, and a flow aid is added at the inlet and outlet of the paper machine screen. After being fully mixed into the pretreated slurry, it enters the paper machine headbox.
[0052] It is worth noting that the pressure of the slurry fed in this step is the feed pressure, the pressure of the slurry filtered out without impurities or with less impurities in this step is the good pulp pressure, and the pressure of the slurry filtered out with more impurities in this step is the tailing pulp pressure. In step 2 of the embodiment of the present invention, the feed pressure, good pulp pressure and tailing pulp pressure in the first stage desander can all be determined by the two-stage sizing pump, which is not limited here. The feed pressure in the second stage desander to the fourth stage desander is 120kPa~210kPa, and the pressure difference between the feed pressure and the good pulp pressure is 15kPa~120kPa, and the tailing pulp pressure is 5kPa~60kPa. The fifth stage deslagging device can appropriately adjust the feed pressure and the good pulp pressure depending on the cleanliness of the papermaking pulp to ensure that the paper pulp has a higher cleanliness. The feed pressure of the screen before the paper machine is 200kPa~700kPa, and the pressure difference between the feed pressure and the good pulp pressure is 0~50kPa.
[0053] It is worth noting that the off-machine white water tank in this step refers to the tank containing the white water filtered by the papermaking wire, which can save water resources and reduce production costs. The working principle of the paper machine screen in this step is: using the pressure difference on both sides of the paper machine screen to make the qualified fibers in the pre-treated slurry flow through the sieve holes (or sieve slits) to the next section, and the remaining impurities are discharged under the pressure of the slurry and the push of the rotor.
[0054] Step three, dehydrating the pretreated pulp to form a wet paper sheet; dehydrating the wet paper sheet, performing a first drying process, performing a first sizing process using a surface sizing agent, performing a second drying process and a first calendering process, and rolling up to obtain a paper base.
[0055] Exemplarily, this step includes: first dehydrating and forming the pretreated slurry to obtain a wet paper sheet. Specifically, the filtered pretreated slurry is sent to a headbox and then dehydrated on the screen. The headbox in the embodiment of the present invention adopts a dilution water headbox method, that is, the white water used by the paper machine is filtered through multiple discs and then reused, thereby achieving the purpose of clean production and facilitating the improvement of the uniformity of the paper. Among them, the concentration of the slurry on the screen is 0.9% to 1.5%, and the pulp-to-net speed ratio is 0.99 to 1.01 to ensure the stability of the quality of the cardboard composition. The proportion of dilution water is 10% to 15% to reduce the quantitative banner difference and ensure the quality of the paper sheet. In addition, the horizontal lip opening in the headbox is 9.00mm to 14.00mm, and the vertical lip opening is 11.00mm to 16.00mm to adjust the amount of slurry and pressure head sprayed onto the forming net by the pretreated slurry in the headbox. Then, the pretreated slurry is dehydrated and formed using the bottom and top net formers. The top net former has three chambers, the vacuum degree of the first chamber is -2kPa to -5kPa, the vacuum degree of the second chamber is -6kPa to -12kPa, and the vacuum degree of the third chamber is -15kPa to -25kPa. In the bottom net dehydration vacuum box, the vacuum degree of the bottom net high vacuum box is -15kPa to -25kPa, the vacuum degree of the bottom net low vacuum box is 0kPa to -15kPa, the vacuum degree of the top net former wet suction box is 0 to -35kPa, the vacuum degree of the vacuum roller low vacuum zone is 0 to -63kPa, and the vacuum degree of the high vacuum zone is 0 to -65kPa. There are four pressure bars, among which the pressure of the first pressure bar to the third pressure bar is 0 to 250mbar, and the pressure of the fourth pressure bar is 0 to 200mbar.
[0056] Then, the wet paper sheet is subjected to a dehydration process, a first drying process, a surface sizing process using a surface sizing agent, a second drying process and a first calendering process, and is wound up to obtain a paper base.
[0057] Specifically, the wet paper sheets formed by dehydration are dehydrated. During this process, the wet paper sheets can be pressed three times using a four-roller three-pressure zone device including a shoe press device. The line pressure of the first pressing is 50kN / m to 60kN / m, the line pressure of the second pressing is 60kN / m to 80kN / m, and the line pressure of the third pressing is 0 to 1000kN / m. Then, a vacuum pressing roller is used for further pressing, wherein the vacuum degree of the low vacuum zone of the vacuum pressing roller is -20kPa to -45kPa, the vacuum degree of the high vacuum zone is -40kPa to -65kPa, and the dryness of the wet paper sheets out of the pressing section is 48% to 53%. Then, the wet paper sheets after dehydration are dried for the first time, and after drying, a sizing machine is used for surface sizing. After sizing, a second drying process is performed, wherein the pressure between the metering rod and the sizing roller is 30kPa to 250kPa. Finally, the dried paper base is sent to a hard calender for the first calendering. The surface temperature of the hot roller of the calender is not higher than 150°C, and the pressure of the nip zone is 10kN / m to 150kN / m. The paper base is then rolled up to finally obtain the paper base.
[0058] Exemplarily, in order to dry the paper base, a multi-stage steam system is used. The characteristic is that the drying cylinders of the multi-cylinder drying section are divided into several groups (a total of 7 to 9 groups, 1 to 5 groups or 1 to 7 groups for the first drying, 6-7 groups or 8 to 9 groups for the second drying), and the new steam from the boiler is divided into three stages of steam supply. Generally, the main steam of the three stages is introduced into the drying cylinders included in each stage, the residual steam of the third stage is sent to the drying cylinders included in the second stage, and the residual steam generated in the second stage is sent to the drying cylinders included in the first stage. If the steam consumption is insufficient after the residual steam is used up by the second stage drying cylinder and the first stage drying cylinder, it is introduced from the main steam of each stage. The condensed water generated by the three-stage air supply is sent from the condensed water tank of the third stage to the condensed water tank of the second stage, from the condensed water tank of the second stage to the condensed water tank of the first stage, and the condensed water of the condensed water tank of the first stage is sent to the main condensed water tank, and then sent to the thermal power plant for recycling.
[0059] In each steam group in the embodiment of the present invention, the pressure difference between the steam inlet and the drain is ≥15kPa (when the steam inlet valve of the drying cylinder of a steam group is closed, the pressure difference is not required), and the pressure difference between the steam inlets of each steam group is ≥30kPa. Calculation method of steam pressure of each steam group: P x =N x +F x ×(P x1 -N x1 ). x represents the steam pressure of steam group x, N x Indicates the minimum steam pressure of steam group x, F x Indicates the pressure increase factor of steam group x, P x1 Indicates the steam pressure of the adjacent high steam pressure group, N x1Indicates the minimum steam pressure of adjacent high steam pressure groups. In actual production, during the first drying, the third steam group and the moisture of the Honeywell quality control system are interlocked to automatically control the steam pressure of the drying cylinder, and the steam pressure of the other steam groups in the previous drying is automatically calculated by the above formula. During the second drying, the fifth steam group and the moisture of the Honeywell quality control system are interlocked to control the steam pressure of the drying cylinder, and the steam pressure of the other steam groups is calculated by the above formula.
[0060] It is worth noting that the quality control system of Valmet of Finland is widely used in the papermaking industry. The system includes a complete set of online sensors with fast scanning and data processing speeds, which can provide accurate and high-resolution measurement data. It can measure the moisture content according to the difference in the attenuation of infrared rays at two locations. Experiments have shown that there is a definite proportional relationship between the weight of moisture per unit area in paper and the measured ratio. After certain corrections, it can be directly used to calculate the weight of moisture per unit area of paper. Based on this, the temperature of the first drying process and the temperature of the second drying process in the embodiment of the present invention can be adjusted according to actual conditions, and are not limited here.
[0061] Exemplarily, step three also includes a broken paper recovery step. The broken paper recovery step includes: first, making the broken paper generated in the paper base into broken paper pulp. Specifically, the broken paper generated in the papermaking process is pulped and concentrated to obtain broken paper pulp. Then the broken paper pulp is added to the papermaking pulp in step two. Specifically, the broken paper screen can be used to screen out the broken paper pulp with qualified fiber length, and then add it to the papermaking pulp in step two. In this process, the amount of broken paper pulp added is appropriately added according to the amount generated during the actual production operation. It should be understood that the broken paper can come from the dehydration step, the dehydration and molding step, the surface sizing treatment step, the winding step and other steps, which can be adjusted according to the actual situation. In addition, whether the fiber length is qualified can also be adjusted according to the actual situation, which is not limited here.
[0062] In addition, step three also includes a fiber recovery step. The fiber recovery step includes: filtering the white water produced in step three to obtain pulp fibers. The fibers are then added to the papermaking pulp in step two, thereby improving pulp utilization and reducing production costs.
[0063] Step 4: forming a coating on one surface of the paper base, and performing a second sizing on the other surface of the paper base using a sizing material to obtain a cardboard composition.
[0064] Exemplarily, step 4 includes: firstly mixing calcium carbonate, latex, defoamer, dispersant, coating starch, brightener, water repellent, lubricant, pH regulator and thickener to obtain a primer. Then, the primer is applied on a surface of the paper base to form a primer. Under the joint action of the above-mentioned auxiliary agents, the solid matter of the primer can be guaranteed to be evenly distributed, and each formula has good compatibility, thereby ensuring that after coating, the paperboard composition is not prone to phase separation during use, and the service life of the paperboard composition is extended. At the same time, since a water repellent is added to the primer, the water resistance of the coating can be improved, so that the paperboard composition has mildew resistance.
[0065] Subsequently, calcium carbonate, porcelain clay, latex, defoamer, dispersant, brightener, dye, water repellent, lubricant, pH regulator, thickener and rheological agent are mixed to obtain a topcoat. The topcoat is applied on the primer to form a topcoat. Since latex is added to the topcoat, the coating strength of the cardboard composition can be improved and the surface properties of the cardboard composition can be enhanced. At the same time, a water repellent is also added to the topcoat to improve the water resistance of the coating, so that the cardboard composition has mildew resistance.
[0066] It is worth noting that the color of the dye contained in the top coating can be blue, purple, or brown, and cardboard compositions of different hues can be prepared according to actual conditions, which is not limited here.
[0067] Finally, the sizing material may be used to apply sizing to the other surface of the paper base to obtain a cardboard composition.
[0068] In practical applications, the second sizing can also be omitted on the other surface of the paper base (i.e., the uncoated surface) to obtain a cardboard composition. The sizing material used in the above process can be a boiled starch solution for sizing the surface of the paper machine as the sizing material for the uncoated surface, with a solid content of 10-19.0%, a starch solution temperature of 40-95°C, a viscosity of 6-21cp, and a pH value of 7.00-7.12. When the cardboard composition is processed into other products, the anti-counterfeiting sizing material is applied to the uncoated surface to compound the two layers of the cardboard composition, which can improve the opacity and composite strength between the paper bases of the cardboard composition.
[0069] Exemplarily, step 4 in the embodiment of the present invention further includes a post-processing step. The post-processing step includes:
[0070] The cardboard composition is subjected to a second calendering treatment. The vehicle speed of the second calendering treatment is 600m / min to 900m / min, the line pressure of the second calendering treatment is 90kN / m to 180kN / m, the temperature of the second calendering treatment is 90℃ to 120℃, and the bulk thickness of the paper after the second calendering treatment is 0.95cm3 / g~1.05cm 3 Within the above parameter range, the glossiness, surface smoothness, elasticity and fineness of the paper can be improved, and the thickness of the final paper can be improved, thereby achieving the quality control stability of the cardboard composition.
[0071] The present invention also provides an application of the above-mentioned pulp slurry composition or the above-mentioned cardboard composition or the preparation method of the above-mentioned cardboard composition in the preparation of black core cardboard.
[0072] Compared with the existing process that requires producing a large number of layers of base paper, gluing and coating, the production process is complicated and the interlayer bonding strength is low, making it difficult to meet the requirements of high-end black core cardboard. The preparation method of the cardboard composition in this application is relatively simple and the production cost is relatively low. It only requires copying two paper bases and coating them. After gluing, black core cardboard with stable hue, high folding resistance, high bonding strength, clear printing details, durability and good anti-counterfeiting performance can be prepared, which is conducive to being put into industrial large-scale production.
[0073] In order to verify the effect of the method for preparing the cardboard composition provided in the embodiment of the present invention, the embodiment of the present invention is demonstrated by using examples and comparative examples.
[0074] Embodiment 1
[0075] Step 1: According to the weight proportion, 30 parts of bleached chemical coniferous pulp and 70 parts of bleached chemical hardwood pulp are respectively crushed, deslagging and pulped, and then the bleached chemical coniferous pulp and the bleached chemical hardwood pulp are mixed and pulped to obtain papermaking pulp.
[0076] The beating degree of the bleached chemical coniferous pulp is 34°SR, the beating degree of the bleached chemical hardwood pulp is 27°SR, and the crushing concentration of the papermaking pulp is 4.5%.
[0077] Step 2: According to the mass fraction, 1 part of corn cationic starch, 0.01 part of blue dye 3R-EVliq, 0.01 part of purple dye 3B-Fliq and 0.01 part of tetrasulfonic acid liquid brightener are mixed with 100 parts of papermaking pulp, and after impurity removal and degassing, 3 parts of corn starch, 0.1 part of alkenyl succinic anhydride, 0.015 part of cationic polyacrylamide, 0.035 part of anionic polyacrylamide and 0.2 part of bentonite are mixed with the papermaking pulp to obtain pre-treated pulp. Finally, the impurities in the pre-treated pulp are screened out using a paper machine screen, and the filtered pre-treated pulp is used as a standby before papermaking.
[0078] Among them, impurities need to be removed through five-stage desanders. The pulp inlet pressure of the second to fourth desanders is 120kPa, the good pulp pressure is 105kPa, and the tail pulp pressure is 5kPa; the pulp inlet pressure of the paper machine screen is 200kPa, and the good pulp pressure is 190kPa.
[0079] Step 3: The filtered pre-treated pulp is sent to the headbox, and then dehydrated on the net. Then, the pre-treated pulp is dehydrated and formed by a stacked net former composed of a top net and a bottom net. Then, the wet paper sheet that has been dehydrated and formed is dehydrated in the press section and dried for the first time. After drying, the surface is sized by the sizing machine, and then dried for the second time. Finally, the dried paper base is sent to the hard calender for the first calendering and winding, and finally the paper base is obtained.
[0080] Among them, the concentration of the pulp on the net is 0.900%, the pulp-net speed ratio is 0.990, the proportion of dilution water is 10.0%, the horizontal lip opening in the headbox is 9.00mm, and the vertical lip opening is 11.00mm. In the top net former, the vacuum degree of the first chamber is -2kPa, the vacuum degree of the second chamber is -6kPa, the vacuum degree of the third chamber is -15kPa, the vacuum degree of the bottom net high vacuum box is -15kPa, the vacuum degree of the bottom net low vacuum box is 0kPa, the vacuum degree of the top net former wet suction box is -35kPa, the vacuum degree of the vacuum chamber of the low vacuum zone of the vacuum roller is -63kPa, and the vacuum degree of the vacuum chamber of the high vacuum zone is -65kPa, the first pressure to the third pressure of the pressure bar are 250mba, and the fourth pressure is 200mbar. Next, the wet paper can be pressed three times using a four-roll three-pressure zone device composed of a shoe press. The line pressure for the first pressing is 50kN / m, the line pressure for the second pressing is 60kN / m, and the line pressure for the third pressing is 800kN / m. The vacuum degree of the vacuum chamber in the low vacuum zone of the vacuum pressing roller is -20kPa, and the vacuum degree of the vacuum chamber in the high vacuum zone is -40kPa. The dryness of the wet paper out of the pressing section is 48%. When applying glue on the surface, the pressure between the metering rod and the glue roller is 100kPa. During the first calendering, the surface temperature of the hard calendering hot roller is 140°C, the line pressure of the pressure zone is 13kN / m, and the bulk thickness of the paper base is 1.05cm. 3 / g. If there is broken paper during papermaking, the broken paper is pulped to obtain broken paper pulp, and the broken paper pulp is added to the papermaking slurry. Similarly, if there is pulp fiber in the white water during papermaking, the pulp fiber is filtered out and added to the papermaking slurry.
[0081] Step 4: first, by weight, 90 parts of 65-grade ground calcium carbonate, 10 parts of carboxylic acid styrene butadiene latex Styronal 300D CN, 0.2 parts of dimethyl silicone oil, 0.1 parts of sodium polyacrylate, 2 parts of coating starch, 0.1 parts of disulfonic acid liquid brightener, 0.2 parts of amino resin, 0.2 parts of calcium stearate, 0.01 parts of sodium hydroxide and 0.1 parts of polyamide polyamine epichlorohydrin resin NCC-1695 are mixed to obtain a primer coating. Then, the primer coating is applied on one surface of the paper base to form a primer layer. Next, 70 parts of 95-grade ground calcium carbonate, 15 parts of porcelain clay KAOLIN AMAZON PREMIUMSD, 10 parts of styrene-butadiene latex Styronal 316CN, 0.1 parts of dimethyl silicone oil, 0.1 parts of sodium polyacrylate, 0.5 parts of tetrasulfonic acid liquid brightener, 0.01 parts of blue dye 3R-EVliq, 0.01 parts of purple dye PVA, 0.1 parts of polyamide polyamine epichlorohydrin resin, 0.1 parts of calcium stearate, 0.2 parts of sodium hydroxide, 0.03 parts of polyvinyl alcohol and 0.1 parts of hydroxyethyl cellulose are mixed to obtain a top coating. The top coating is applied on the primer to form a top coating. Finally, the boiled corn starch solution for paper machine surface sizing is used as the sizing material for another surface, with a solid content of 18.2%, a temperature of 45°C, a viscosity of 20.2cp, and a pH value of 7.08. The size is used to apply size to the other surface of the paper base (ie, the uncoated surface) to obtain a cardboard composition.
[0082] The coating amount of the primer and topcoat is 10.5g / m 2 The sizing amount of corn starch on the other surface is 2.0g / m 2 .
[0083] Embodiment 2
[0084] Step 1: According to the weight proportion, 40 parts of bleached chemical coniferous pulp and 60 parts of bleached chemical hardwood pulp are respectively crushed, deslagging and pulped, and then the bleached chemical coniferous pulp and the bleached chemical hardwood pulp are mixed and pulped to obtain papermaking pulp.
[0085] Among them, the beating degree of bleached chemical softwood pulp is 42°SR, and the beating degree of bleached chemical hardwood pulp is 35°SR.
[0086] The disintegration concentration of the papermaking pulp is 5%.
[0087] Step 2: According to the mass fraction, 2 parts of cassava cationic starch, 0.001 parts of blue dye 3R-EVliq, 0.001 parts of purple dye 3B-Fliq and 0.1 parts of disulfonic acid liquid brightener are mixed with 100 parts of papermaking pulp, and after impurity removal and degassing, 5 parts of cassava starch, 0.15 parts of alkenyl succinic anhydride, 0.015 parts of cationic polyacrylamide, 0.035 parts of anionic polyacrylamide and 0.2 parts of bentonite are mixed with the papermaking pulp to obtain pre-treated pulp. Finally, the impurities in the pre-treated pulp are screened out by a paper machine, and the filtered pre-treated pulp is used as a standby before papermaking.
[0088] Among them, impurities need to be removed through five-stage desanders. The pulp inlet pressure of the second to fourth desanders is 210kPa, the good pulp pressure is 100kPa, and the tail pulp pressure is 10kPa; the pulp inlet pressure of the paper machine screen is 700kPa, and the good pulp pressure is 650kPa.
[0089] Step 3: The filtered pre-treated pulp is sent to the headbox, and then dehydrated on the net. Then, the pre-treated pulp is dehydrated and formed by using a stack former composed of a top net and a bottom net. Then, the wet paper sheet that has been dehydrated and formed is dehydrated in the press section and dried for the first time. After drying, the surface is sized by a sizing machine, and then dried for the second time. Finally, the dried paper base is sent to the hard calender for the first calendering and winding, and finally the paper base is obtained.
[0090] Among them, the concentration of the pulp on the net is 0.900%, the pulp-net speed ratio is 0.990, the proportion of dilution water is 10.0%, the horizontal lip opening in the headbox is 9.00mm, and the vertical lip opening is 11.00mm. In the top net former, the vacuum degree of the first chamber is -2kPa, the vacuum degree of the second chamber is -6kPa, the vacuum degree of the third chamber is -15kPa, the vacuum degree of the bottom net high vacuum box is -15kPa, the vacuum degree of the bottom net low vacuum box is 0kPa, the vacuum degree of the top net former wet suction box is -35kPa, the vacuum degree of the vacuum chamber of the low vacuum zone of the vacuum roller is -43kPa, and the vacuum degree of the vacuum chamber of the high vacuum zone is -60kPa, the first pressure to the third pressure of the pressure bar are 250mba, and the fourth pressure is 200mbar. Next, the wet paper can be pressed three times using a four-roller three-pressure zone device composed of a shoe press. The line pressure for the first pressing is 45kN / m, the line pressure for the second pressing is 58kN / m, and the line pressure for the third pressing is 830kN / m. Next, a vacuum pressing roller is used for further pressing. The vacuum degree in the low vacuum zone is -45kpa, and the vacuum degree in the high vacuum zone is -65kpa. The dryness of the wet paper out of the pressing section is 51%. When applying glue on the surface, the pressure between the metering rod and the glue roller is 100kPa. During the first calendering, the surface temperature of the hard calendering hot roller is 140°C, the line pressure in the pressure zone is 20kN / m, and the bulk thickness of the paper base is 0.96cm. 3 / g. If there is broken paper during papermaking, the broken paper is pulped to obtain broken paper pulp, and the broken paper pulp is added to the papermaking slurry. Similarly, if there is pulp fiber in the white water during papermaking, the pulp fiber is filtered out and added to the papermaking slurry.
[0091] Step 4: first, by weight, 95 parts of 65-grade ground calcium carbonate, 11 parts of carboxylic acid styrene butadiene latex Styronal 300D CN, 0.5 parts of dimethyl silicone oil, 0.5 parts of sodium polyacrylate, 5 parts of coating starch, 0.3 parts of disulfonic acid liquid brightener, 0.3 parts of amino resin, 0.3 parts of calcium stearate, 0.05 parts of sodium hydroxide and 0.3 parts of polyamide polyamine epichlorohydrin resin are mixed to obtain a primer coating. Then, the primer coating is applied to one surface of the paper base to form a primer layer. Next, 90 parts of 95-grade ground calcium carbonate, 15 parts of porcelain clay KAOLIN AMAZON PREMIUM SD, 10 parts of carboxylic acid styrene butadiene latex Styronal 316CN, 0.1 parts of dimethyl silicone oil, 0.1 parts of sodium polyacrylate, 0.8 parts of disulfonic acid liquid brightener, 0.02 parts of blue dye 3R-EVliq, 0.04 parts of purple dye PVA, 0.1 parts of water repellent, 0.1 parts of calcium stearate, 0.2 parts of sodium hydroxide, 0.03 parts of polyamide polyamine epichlorohydrin resin and 0.1 parts of hydroxyethyl cellulose are mixed to obtain a top coating. The top coating is applied on the primer to form a top coating. Finally, the boiled corn starch solution for paper machine surface sizing is used as the sizing material for another surface, with a solid content of 18.2%, a temperature of 52°C, a viscosity of 19.0cp, and a pH value of 7.09. The other surface of the paper base (ie, the uncoated surface) is sized by using a size compound to obtain a cardboard composition.
[0092] The coating amount of the primer and topcoat is 10.0g / m 2 The sizing amount of tapioca starch in the other surface is 3.0g / m 2 .
[0093] Embodiment 3
[0094] Step 1: According to the weight proportion, 35 parts of bleached chemical coniferous pulp and 65 parts of bleached chemical hardwood pulp are respectively crushed, deslagging and pulped, and then the bleached chemical coniferous pulp and the bleached chemical hardwood pulp are mixed and pulped to obtain papermaking pulp.
[0095] The beating degree of the bleached chemical coniferous pulp is 40°SR, the beating degree of the bleached chemical hardwood pulp is 30°SR, and the crushing concentration of the papermaking pulp is 4.8%.
[0096] Step 2: According to the mass fraction, 1.5 parts of cassava cationic starch and 0.04 parts of hexasulfonic acid liquid brightener are mixed with 100 parts of papermaking pulp, and after impurities and degassing, 5 parts of cassava starch, 0.15 parts of alkenyl succinic anhydride, 0.015 parts of cationic polyacrylamide, 0.035 parts of anionic polyacrylamide, and 0.25 parts of bentonite are mixed with the papermaking pulp to obtain a pre-treated pulp. Finally, the impurities in the pre-treated pulp are screened out using a paper machine screen, and the filtered pre-treated pulp is used as a standby before papermaking.
[0097] Among them, impurities need to be removed through five-stage desanders. The pulp inlet pressure of the second to fourth desanders is 210kPa, the good pulp pressure is 100kPa, and the tail pulp pressure is 10kPa; the pulp inlet pressure of the paper machine screen is 700kPa, and the good pulp pressure is 650kPa.
[0098] Step 3: The filtered pre-treated pulp is sent to the headbox, and then dehydrated on the net. Then, the pre-treated pulp is dehydrated and formed by a stacked net former composed of a top net and a bottom net. Then, the wet paper sheet that has been dehydrated and formed is dehydrated in the press section and dried for the first time. After drying, the surface is sized by the sizing machine, and then dried for the second time. Finally, the dried paper base is sent to the hard calender for the first calendering and winding, and finally the paper base is obtained.
[0099] Among them, the concentration of the pulp on the net is 0.900%, the pulp-to-net speed ratio is 0.998, the proportion of dilution water is 10%, the horizontal lip opening in the headbox is 9.00mm, and the vertical lip opening is 11.00mm. In the top net former, the vacuum degree of the first chamber is -2kPa, the vacuum degree of the second chamber is -6kPa, the vacuum degree of the third chamber is -15kPa, the vacuum degree of the bottom net high vacuum box is -15kPa, the vacuum degree of the bottom net low vacuum box is 0kPa, the vacuum degree of the top net former wet suction box is -35kPa, the vacuum degree of the vacuum chamber in the low vacuum zone of the vacuum roller is -53kPa, and the vacuum degree of the vacuum chamber in the high vacuum zone is -65kPa, the first pressure to the third pressure of the pressure bar are 250mba, and the fourth pressure is 200mbar. Next, the wet paper can be pressed three times using a shoe press and a four-roll three-pressure zone device. The line pressure for the first pressing is 60kN / m, the line pressure for the second pressing is 80kN / m, and the line pressure for the third pressing is 850kN / m. Next, a vacuum pressing roller is used for further pressing. The vacuum degree in the low vacuum zone is -45kpa, the vacuum degree in the high vacuum zone is -65kpa, and the dryness of the wet paper out of the pressing section is 53%. When applying glue on the surface, the pressure between the metering rod and the glue roller is 250kPa. During the first calendering, the surface temperature of the hard calendering hot roller is 140°C, the line pressure in the pressure zone is 15kN / m, and the bulk thickness of the paper base is 0.99cm. 3 / g. If there is broken paper during papermaking, the broken paper is pulped to obtain broken paper pulp, and the broken paper pulp is added to the papermaking slurry. Similarly, if there is pulp fiber in the white water during papermaking, the pulp fiber is filtered out and added to the papermaking slurry.
[0100] Step 4: first, by weight, 90 parts of 65-grade ground calcium carbonate, 11 parts of carboxylic acid styrene butadiene latex Styronal 300D CN, 0.5 parts of dimethyl silicone oil, 0.5 parts of sodium polyacrylate, 5 parts of coating starch, 0.3 parts of tetrasulfonic acid liquid brightener, 0.3 parts of amino resin, 0.3 parts of calcium stearate, 0.05 parts of sodium hydroxide and 0.3 parts of polyvinyl alcohol are mixed to obtain a primer coating. Then, the primer coating is applied on the paper base to form a primer layer. Next, 80 parts of 95-grade ground calcium carbonate, 20 parts of porcelain clay KAOLIN AMAZON PREMIUM SD, 14 parts of styrene-butadiene latex Styronal 316CN, 0.3 parts of dimethyl silicone oil, 0.2 parts of sodium polyacrylate, 0.6 parts of tetrasulfonic acid liquid brightener, 0.015 parts of blue dye PT-30, 0.03 parts of purple dye PA-30, 1 part of water repellent, 0.1 parts of calcium stearate, 0.2 parts of sodium hydroxide, 0.03 parts of polyvinyl alcohol and 0.1 parts of hydroxyethyl cellulose are mixed to obtain a top coating. The top coating is applied on the primer to form a top coating. Finally, the boiled cassava starch solution for paper machine surface sizing is used as the sizing material for another surface, with a solid content of 18.0%, a temperature of 50°C, a viscosity of 18.0cp and a pH value of 7.02. The other surface of the paper base (ie, the uncoated surface) is sized with a size to obtain a cardboard composition.
[0101] The coating weight of the primer and topcoat is 11.0 g / m 2 The sizing amount of tapioca starch in the other surface is 1.6g / m 2 .
[0102] Embodiment 4
[0103] Step 1: According to the weight proportion, 30 parts of bleached chemical coniferous pulp and 70 parts of bleached chemical hardwood pulp are respectively crushed, deslagging and pulped, and then the bleached chemical coniferous pulp and the bleached chemical hardwood pulp are mixed and pulped to obtain papermaking pulp.
[0104] The beating degree of the bleached chemical coniferous pulp is 34°SR, the beating degree of the bleached chemical hardwood pulp is 27°SR, and the crushing concentration of the papermaking pulp is 4.5%.
[0105] Step 2: According to the mass fraction, 1 part of corn cationic starch, 0.01 part of blue dye 3R-EVliq, 0.01 part of purple dye 3B-Fliq and 0.2 part of disulfonic acid liquid brightener are mixed with 100 parts of papermaking pulp, and after removing impurities and degassing, 3 parts of corn starch, 0.1 part of alkenyl succinic anhydride, 0.025 parts of cationic polyacrylamide, 0.035 parts of anionic polyacrylamide and 0.2 parts of bentonite are mixed with the papermaking pulp to obtain pre-treated pulp. Finally, the impurities in the pre-treated pulp are screened out using a paper machine screen, and the filtered pre-treated pulp is used as a standby before papermaking.
[0106] Among them, impurities need to be removed through five-stage desanders. The pulp inlet pressure of the second to fourth desanders is 120kPa, the good pulp pressure is 105kPa, and the tail pulp pressure is 5kPa; the pulp inlet pressure of the screen before the paper machine is 200kPa, and the pressure of the good pulp is 190kPa.
[0107] Step 3: The filtered pre-treated pulp is sent to the headbox, and then dehydrated on the net. Then, the pre-treated pulp is dehydrated and formed by a stacked net former composed of a top net and a bottom net. Then, the wet paper sheet that has been dehydrated and formed is dehydrated in the press section and dried for the first time. After drying, the surface is sized by the sizing machine, and then dried for the second time. Finally, the dried paper base is sent to the hard calender for the first calendering and winding, and finally the paper base is obtained.
[0108] Among them, the concentration of the pulp on the net is 0.918%, the pulp-to-net speed ratio is 1.002, the proportion of dilution water is 10%, the horizontal lip opening in the headbox is 9.00mm, and the vertical lip opening is 11.00mm. In the top net former, the vacuum degree of the first chamber is -2kPa, the vacuum degree of the second chamber is -6kPa, the vacuum degree of the third chamber is -15kPa, the vacuum degree of the bottom net high vacuum box is -15kPa, the vacuum degree of the bottom net low vacuum box is 0kPa, the vacuum degree of the top net former wet suction box is -35kPa, the vacuum degree of the vacuum chamber in the low vacuum area of the vacuum roller is -53kPa, the vacuum degree of the vacuum chamber in the high vacuum area is -65kPa, the first pressure to the third pressure of the pressure bar are 250mba, and the fourth pressure is 200mbar. Next, the wet paper can be pressed three times using a four-roller three-pressure zone device composed of a shoe press. The line pressure for the first pressing is 50kN / m, the line pressure for the second pressing is 60kN / m, and the line pressure for the third pressing is 860kN / m. Next, a vacuum pressing roller is used for further pressing. The vacuum degree in the low vacuum zone is -20kpa, and the vacuum degree in the high vacuum zone is -40kpa. The dryness of the wet paper out of the pressing section is 48%. When applying glue on the surface, the pressure between the metering rod and the glue roller is 30kPa. During the first calendering, the surface temperature of the hard calendering hot roller is 140°C, the line pressure in the pressure zone is 13kN / m, and the bulk thickness of the paper base is 1.05cm. 3 / g. If there is broken paper during papermaking, the broken paper is pulped to obtain broken paper pulp, and the broken paper pulp is added to the papermaking slurry. Similarly, if there is pulp fiber in the white water during papermaking, the pulp fiber is filtered out and added to the papermaking slurry.
[0109] Step 4: first, by weight, 90 parts of 65-grade ground calcium carbonate, 10 parts of carboxylic acid styrene butadiene latex Styronal 300D CN, 0.2 parts of dimethyl silicone oil, 0.1 parts of sodium polyacrylate, 2 parts of coating starch, 0.1 parts of disulfonic acid liquid brightener, 0.2 parts of amino resin, 0.2 parts of calcium stearate, 0.01 parts of sodium hydroxide and 0.1 parts of polyamide polyamine epichlorohydrin resin are mixed to obtain a primer coating. Then, the primer coating is applied on one surface of the paper base to form a primer layer. Next, 70 parts of 95-grade ground calcium carbonate, 15 parts of porcelain clay KAOLIN AMAZON PREMIUM SD, 10 parts of carboxylic acid styrene butadiene latex Styronal 316CN, 0.1 parts of dimethyl silicone oil, 0.1 parts of sodium polyacrylate, 0.05 parts of tetrasulfonic acid liquid brightener, 0.001 parts of blue dye 3R-EVliq, 0.001 parts of purple dye PA-30, 0.1 parts of water repellent, 0.1 parts of calcium stearate, 0.2 parts of sodium hydroxide, 0.03 parts of polyvinyl alcohol and 0.1 parts of hydroxyethyl cellulose are mixed to obtain a top coating. The top coating is applied on the primer to form a top coating. Finally, the boiled starch solution for sizing the paper machine surface is used as the sizing material for another surface, with a solid content of 18.5%, a temperature of 52°C, a viscosity of 22.0cp, and a pH value of 7.11. The other surface of the paper base (ie, the uncoated surface) is sized with a size to obtain a cardboard composition.
[0110] The coating amount of the primer and topcoat is 10.5g / m 2 , the amount of corn starch applied on the other surface <24P02261CN>
[0111] 2.1g / m 2 .
[0112] Embodiment 5
[0113] Step 1: According to the weight proportion, 40 parts of bleached chemical coniferous pulp and 60 parts of bleached chemical hardwood pulp are respectively crushed, deslagging and pulped, and then the bleached chemical coniferous pulp and the bleached chemical hardwood pulp are mixed and pulped to obtain papermaking pulp.
[0114] The beating degree of the bleached chemical coniferous pulp is 42°SR, the beating degree of the bleached chemical hardwood pulp is 35°SR, and the crushing concentration of the papermaking pulp is 5.0%.
[0115] Step 2: According to the mass fraction, 2 parts of cassava cationic starch, 0.01 parts of blue dye 3R-EVliq, 0.01 parts of purple dye 3B-Fliq and 0.6 parts of disulfonic acid liquid brightener are mixed with 100 parts of papermaking pulp, and after impurity removal and degassing, 6 parts of cassava starch, 0.14 parts of alkenyl succinic anhydride, 0.015 parts of cationic polyacrylamide, 0.035 parts of anionic polyacrylamide and 0.3 parts of bentonite are mixed with the papermaking pulp to obtain pre-treated pulp. Finally, the impurities in the pre-treated pulp are screened out using a paper machine screen, and the filtered pre-treated pulp is used as a standby before papermaking.
[0116] Among them, impurities need to be removed through five-stage desanders. The pulp inlet pressure of the second to fourth desanders is 210kPa, the good pulp pressure is 100kPa, and the tail pulp pressure is 10kPa; the pulp inlet pressure of the screen before the paper machine is 700kPa, and the pressure of the good pulp is 650kPa.
[0117] Step 3: The filtered pre-treated pulp is sent to the headbox, and then dehydrated on the net. Then, the pre-treated pulp is dehydrated and formed by a stacked net former composed of a top net and a bottom net. Then, the wet paper sheet after dehydration and forming is dehydrated and dried for the first time. After drying, the surface is sizing treated by a sizing machine, and then dried for the second time. Finally, the dried paper base is sent to a hard calender for the first calendering and winding, and finally the paper base is obtained.
[0118] Among them, the concentration of the pulp on the net is 0.924%, the pulp-net speed ratio is 1.004, the proportion of dilution water is 10.5%, the horizontal lip opening in the headbox is 9.00mm, and the vertical lip opening is 11.00mm. In the top net former, the vacuum degree of the first chamber is -2kPa, the vacuum degree of the second chamber is -6kPa, the vacuum degree of the third chamber is -15kPa, the vacuum degree of the bottom net high vacuum box is -15kPa, the vacuum degree of the bottom net low vacuum box is 0kPa, the vacuum degree of the top net former wet suction box is -35kPa, the vacuum degree of the vacuum chamber of the low vacuum zone of the vacuum roller is -43kPa, and the vacuum degree of the vacuum chamber of the high vacuum zone is -63kPa, the first pressure to the third pressure of the pressure bar are 250mba, and the fourth pressure is 200mbar. Next, the wet paper can be pressed three times using a shoe press. The line pressure for the first pressing is 60kN / m, the line pressure for the second pressing is 80kN / m, and the line pressure for the third pressing is 810kN / m. Next, a vacuum pressing roller is used for further pressing. The vacuum degree in the low vacuum zone is -45kpa, the vacuum degree in the high vacuum zone is -65kpa, and the dryness of the wet paper out of the pressing section is 53%. When applying glue on the surface, the pressure between the metering rod and the glue roller is 250kPa. During the first calendering, the surface temperature of the hard calendering hot roller is 140°C, the line pressure in the pressing zone is 20kN / m, and the bulk thickness of the paper base is 0.98cm. 3 / g. If there is broken paper during papermaking, the broken paper is pulped to obtain broken paper pulp, and the broken paper pulp is added to the papermaking slurry. Similarly, if there is pulp fiber in the white water during papermaking, the pulp fiber is filtered out and added to the papermaking slurry.
[0119] Step 4: first, by weight, 95 parts of 65-grade ground calcium carbonate, 11 parts of carboxylic acid styrene butadiene latex Styronal 300D CN, 0.5 parts of dimethyl silicone oil, 0.5 parts of sodium polyacrylate, 5 parts of coating starch, 0.3 parts of disulfonic acid liquid brightener, 0.3 parts of amino resin, 0.3 parts of calcium stearate, 0.05 parts of sodium hydroxide and 0.3 parts of polyamide polyamine epichlorohydrin resin are mixed to obtain a primer coating. Then, the primer coating is applied on one surface of the paper base to form a primer layer. Next, 90 parts of 95-grade ground calcium carbonate, 15 parts of porcelain clay KAOLIN AMAZON PREMIUM SD, 10 parts of carboxylic acid styrene butadiene latex Styronal 316CN, 0.1 parts of dimethyl silicone oil, 0.1 parts of sodium polyacrylate, 0.49 parts of disulfonic acid liquid brightener, 0.009 parts of blue dye 3R-EVliq, 0.009 parts of purple dye PA-30, 1 part of water repellent, 0.1 parts of calcium stearate, 0.2 parts of sodium hydroxide, 0.03 parts of polyamide polyamine epichlorohydrin resin and 0.1 parts of hydroxyethyl cellulose are mixed to obtain a top coating. The top coating is applied on the primer to form a top coating. Finally, the boiled starch solution for sizing the paper machine surface is used as the sizing material for another surface, with a solid content of 18.0%, a temperature of 50°C, a viscosity of 18.0cp, and a pH value of 7.02. The other surface of the paper base (ie, the uncoated surface) is sized with a size to obtain a cardboard composition.
[0120] The coating amount of the primer and topcoat is 10g / m 2 The sizing amount of tapioca starch in the other surface is 3.0g / m 2 .
[0121] Embodiment 6
[0122] Step 1: According to the weight proportion, 30 parts of bleached chemical coniferous pulp and 70 parts of bleached chemical hardwood pulp are respectively crushed, deslagging and pulped, and then the bleached chemical coniferous pulp and the bleached chemical hardwood pulp are mixed and pulped to obtain papermaking pulp.
[0123] The beating degree of the bleached chemical coniferous pulp is 40°SR, the beating degree of the bleached chemical hardwood pulp is 30°SR, and the crushing concentration of the papermaking pulp is 4.8%.
[0124] Step 2: According to the mass fraction, 1.5 parts of cassava cationic starch and 0.004 parts of hexasulfonic acid liquid brightener are mixed with 100 parts of papermaking pulp, and after removing impurities and degassing, 5 parts of cassava starch, 0.13 parts of alkenyl succinic anhydride, 0.020 parts of cationic polyacrylamide, 0.030 parts of anionic polyacrylamide, and 0.25 parts of bentonite are mixed with the papermaking pulp to obtain a pre-treated pulp. Finally, the impurities in the pre-treated pulp are screened out using a paper machine screen, and the filtered pre-treated pulp is used as a standby before papermaking.
[0125] Among them, impurities need to be removed through five-stage desanders. The pulp inlet pressure of the second to fourth desanders is 210kPa, the good pulp pressure is 100kPa, and the tail pulp pressure is 10kPa; the pulp inlet pressure of the screen before the paper machine is 700kPa, and the pressure of the good pulp is 650kPa.
[0126] Step 3: The filtered pre-treated pulp is sent to the headbox, and then dehydrated on the net. Then, the pre-treated pulp is dehydrated and formed by a stacked net former composed of a top net and a bottom net. Then, the wet paper sheet that has been dehydrated and formed is dehydrated in the press section and dried for the first time. After drying, the surface is sized by the sizing machine, and then dried for the second time. Finally, the dried paper base is sent to the hard calender for the first calendering and winding, and finally the paper base is obtained.
[0127] Among them, the concentration of the pulp on the net is 0.905%, the pulp-to-net speed ratio is 0.999, the proportion of dilution water is 10.0%, the horizontal lip opening in the headbox is 9.00mm, and the vertical lip opening is 11.00mm. In the top net former, the vacuum degree of the first chamber is -2kPa, the vacuum degree of the second chamber is -6kPa, the vacuum degree of the third chamber is -15kPa, the vacuum degree of the bottom net high vacuum box is -15kPa, the vacuum degree of the bottom net low vacuum box is 0kPa, the vacuum degree of the top net former wet suction box is -35kPa, the vacuum degree of the vacuum chamber of the low vacuum zone of the vacuum roller is -43kPa, the vacuum degree of the vacuum chamber of the high vacuum zone is -65kPa, the first pressure to the third pressure of the pressure bar are 250mba, and the fourth pressure is 200mbar. Next, the wet paper can be pressed three times using a four-roller three-pressure zone device composed of a shoe press. The line pressure for the first pressing is 60kN / m, the line pressure for the second pressing is 80kN / m, and the line pressure for the third pressing is 880kN / m. Next, a vacuum pressing roller is used for further pressing. The vacuum degree in the low vacuum zone is -45kpa, the vacuum degree in the high vacuum zone is -65kpa, and the dryness of the wet paper out of the pressing section is 53%. When applying glue on the surface, the pressure between the metering rod and the glue roller is 250kPa. During the first calendering, the surface temperature of the hard calendering hot roller is 140°C, the line pressure in the pressure zone is 15kN / m, and the bulk thickness of the paper base is 1.00cm. 3 / g. If there is broken paper during papermaking, the broken paper is pulped to obtain broken paper pulp, and the broken paper pulp is added to the papermaking slurry. Similarly, if there is pulp fiber in the white water during papermaking, the pulp fiber is filtered out and added to the papermaking slurry.
[0128] Step 4: first, by weight, 90 parts of 65-grade ground calcium carbonate, 11 parts of carboxylic acid styrene butadiene latex Styronal 300D CN, 0.5 parts of dimethyl silicone oil, 0.5 parts of sodium polyacrylate, 5 parts of coating starch, 0.3 parts of disulfonic acid liquid brightener, 0.3 parts of amino resin, 0.3 parts of calcium stearate, 0.05 parts of sodium hydroxide and 0.3 parts of polyamide polyamine epichlorohydrin resin are mixed to obtain a primer coating. Then, the primer coating is applied on the paper base to form a primer layer. Next, 80 parts of 95-grade ground calcium carbonate, 20 parts of porcelain clay KAOLIN AMAZON PREMIUM SD, 14 parts of carboxylic acid styrene butadiene latex Styronal 316CN, 0.3 parts of dimethyl silicone oil, 0.2 parts of sodium polyacrylate, 0.2 parts of hexasulfonic acid liquid brightener, 0.005 parts of blue dye 3R-EVliq, 0.005 parts of purple dye PA-30, 0.1 parts of water repellent, 0.1 parts of calcium stearate, 0.2 parts of sodium hydroxide, 0.03 parts of polyvinyl alcohol and 0.1 parts of hydroxyethyl cellulose are mixed to obtain a top coating. The top coating is applied on the primer to form a top coating. Finally, the boiled starch solution for sizing the paper machine surface is used as the sizing material for another surface, with a solid content of 19.0%, a temperature of 55°C, a viscosity of 19cp, and a pH value of 7.12. The other surface of the paper base (ie, the uncoated surface) is sized with a size to obtain a cardboard composition.
[0129] The coating weight of the primer and topcoat is 11.2 g / m 2 The sizing amount of tapioca starch in the other surface is 1.6g / m 2 .
[0130] Comparative Example 1
[0131] Provide a piece of commercially available and common black core card stock.
[0132] In order to further verify the effect of the preparation method of the cardboard composition provided in the embodiment of the present invention, the present invention compares the optical properties and physical properties of the cardboard compositions prepared in comparative example 1 with those prepared in embodiments 1 to 6 of the present invention, and tests are performed by the following methods.
[0133] 1. Whiteness test: Blue light whiteness is a single-band whiteness formula, which measures the diffuse reflection factor of blue light in the short-wave band of 457nm, expressed as R457.
[0134] (1) D65 brightness: ISO2470 specifies the use of an integrating sphere instrument for measurement. 2470-2 measures R457 under D65 light source under outdoor daylight conditions, which is called D65 brightness.
[0135] (2) CIE whiteness
[0136] CIE whiteness is widely used in various industries. It is consistent with the whiteness formula after ASTM E313-95. It works under D65 and C light sources and is used in the textile industry, building materials, non-metallic mineral products and paper industry. ISO11475 is the CIE whiteness measurement of cardboard compositions under indoor light (C / 2°) conditions.
[0137] 2. Smoothness test: Place the paperboard combination on a glass plate, apply a specific pressure to create a semi-vacuum, thereby sucking in air and passing it through the contact surface, and measure the time required for the vacuum degree to change within a specified range, usually expressed in seconds. The higher the smoothness of the paper surface, the longer the time for air to flow in; conversely, the lower the smoothness, the shorter the time for air to flow in.
[0138] 3. Internal bonding strength measurement: It is the measurement of the tensile strength of the paperboard composite surface when it withstands uniformly distributed tensile force until it is destroyed. It is the ratio of the maximum destructive tensile force perpendicular to the sample surface to the sample area.
[0139] 4. Folding resistance test: The folding resistance of paper is measured by the number of folds required for the paper to break after being stretched by a certain force and then folded back and forth. It is expressed in times, and the unit is double folding times. The result of the longitudinal cutting test is the longitudinal folding resistance, and the result of the transverse cutting test is the transverse folding resistance.
[0140] 5. Water absorption test: The international standard ISO 535 "Paper and paperboard - Determination of water absorption (Cobb method)" is adopted to determine the surface water absorption capacity of paper or paperboard using a Cobb absorber.
[0141] The following are the performance test results of the cardboard compositions prepared in Examples 1 to 6.
[0142] Table 1 Optical performance test results of this embodiment
[0143]
[0144] Table 2 Physical properties test results of this embodiment
[0145]
[0146] 1. It can be seen from Table 1 that, compared with Comparative Example 1, the hue of the cardboard compositions prepared in Examples 1 to 6 is more stable, indicating that the whitening agent and the dye have good water solubility, stable performance, and strong fiber binding ability with the pulp. Under their synergistic effect, a cardboard composition with stable hue can be prepared.
[0147] 2. As shown in Table 2, compared with the comparative example 1, the smoothness, internal bonding strength and water resistance of the cardboard composition prepared by the present embodiments 1 to 6 are all excellent, indicating that under the joint action of papermaking pulp, the first reinforcing agent, the second reinforcing agent, the internal sizing agent and the retention and drainage aid, it is possible to prepare a cardboard composition with high internal bonding strength, water resistance and folding resistance. At the same time, since the cardboard composition has a high internal bonding strength, it is stable in form during use, not easy to be delaminated and deformed, which is conducive to extending the service life of the cardboard composition. In addition, since these two reinforcing agents are all derived from the same or different kinds of starch, the properties are similar, so they can be better matched in the process of combining with papermaking pulp, and are evenly distributed with the fibers in the pulp, increasing the binding sites between the fibers, and improving the retention rate of fine fibers, which is conducive to preparing a cardboard composition with high bonding strength, clear printing details, durable and good anti-counterfeiting performance.
[0148] 3. Compared with the existing process that requires the production of a large number of layers of base paper and reduces bonding and coating, the production process is complicated and the interlayer bonding strength is low, which makes it difficult to meet the requirements of high-end black core cardboard. The preparation method of the cardboard composition used in Examples 1 to 6 is relatively simple and has a relatively low production cost. It only requires the manufacture of two paper bases and coating them. After bonding, a cardboard composition with stable hue, high bonding strength, clear printing details, durability, and good anti-counterfeiting performance can be prepared, which is conducive to being put into industrial large-scale production.
[0149] 4. It can be seen from Table 2 that, through the combined action of the internal sizing agent and the surface sizing agent, the cardboard composition has hydrophobicity and fluid penetration resistance, is not easily affected by moisture and mildew, and has a longer service life.
[0150] 5. As shown in Table 2, the smoothness and glossiness of the paperboard composition can be significantly increased by the combined effect of the above-mentioned pulp slurry composition, coating and calendering step, so that the paperboard composition has a better feel and improves the use process <24P02261CN>
[0151] Comfort in.
[0152] The above is only a specific embodiment of the present invention. Obviously, various modifications and combinations can be made without departing from the spirit and scope of the present invention. Accordingly, this specification and the drawings are only exemplary illustrations of the present invention as defined by the attached claims, and are deemed to have covered any and all modifications, changes, combinations or equivalents within the scope of the present invention. Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is intended to include these changes and variations. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be covered within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope of protection of the claims.
Claims
1. A pulp slurry composition, characterized in that: include: Papermaking pulp, a first reinforcing agent, a second reinforcing agent, an internal sizing agent and a retention and drainage aid; wherein the first reinforcing agent comprises at least one of corn cationic starch and cassava cationic starch; and / or the second reinforcing agent comprises at least one of corn starch and cassava starch; in terms of weight parts, the papermaking pulp is 90 to 110 parts, the first reinforcing agent is 1 to 2 parts, the second reinforcing agent is 3 to 6 parts, and the retention and drainage aid is 0.225 to 0.385 parts.
2. The pulp slurry composition according to claim 1, characterized in that The papermaking pulp comprises bleached chemical coniferous wood pulp and bleached chemical broadleaf wood pulp; in terms of weight percentage, the chemical coniferous wood pulp accounts for 30 to 40 parts, and the broadleaf wood pulp accounts for 60 to 70 parts.
3. A cardboard composition, characterized in that: include: The coating and the pulp slurry composition according to any one of claims 1 to 2, wherein the mass ratio of the coating to the pulp is (13-16):
70.
4. The cardboard composition according to claim 3, characterized in that: The coating comprises a primer and a top coat, wherein the primer has a weight of 8 g / m 2 ~14g / m 2 The weight of the top coating is 8 g / m 2 ~14g / m 2 .
5. The cardboard composition according to claim 4, characterized in that: The base coating layer includes calcium carbonate, latex, defoamer, dispersant, coating starch, whitening agent, water repellent, lubricant, pH regulator and thickener; in terms of mass parts, the cardboard composition includes: 90 to 100 parts of calcium carbonate, 8 to 15 parts of latex, 0.2 to 0.5 parts of defoamer, 0.1 to 0.5 parts of dispersant, 2 to 5 parts of coating starch, 0.1 to 0.3 parts of whitening agent, 0.2 to 0.3 parts of water repellent, 0.2 to 0.3 parts of lubricant, 0.01 to 0.05 parts of pH regulator and 0.1 to 0.3 parts of thickener.
6. The cardboard composition according to claim 4, characterized in that: The top coating layer includes calcium carbonate, china clay, latex, defoamer, dispersant, brightener, dye, water repellent, lubricant, pH adjuster, thickener and rheological agent; in terms of mass parts, the cardboard composition includes: 70 to 90 parts of calcium carbonate, 10 to 30 parts of china clay, 10 to 20 parts of latex, 0.1 to 0.5 parts of defoamer, 0.1 to 0.3 parts of dispersant, 0.05 to 0.8 parts of brightener, 0.002 to 0.06 parts of dye, 0.1 to 0.3 parts of water repellent, 0.1 to 0.3 parts of lubricant, 0.2 to 0.4 parts of pH adjuster, 0.03 to 0.07 parts of thickener, and 0.1 to 0.3 parts of rheological agent.
7. The cardboard composition according to claim 3, characterized in that: The card paper composition further comprises a surface sizing agent, which is an alkyl ketene dimer or a styrene acrylic copolymer dispersion.
8. A method for preparing the cardboard composition according to any one of claims 3 to 7, characterized in that: <24P02261CN> The preparation method comprises: Step 1, mixing bleached chemical coniferous wood pulp and bleached chemical hardwood wood pulp to obtain papermaking pulp; Step 2, adding a toner, a first reinforcing agent, a second reinforcing agent, an internal sizing agent and a retention and drainage aid to the papermaking slurry to obtain a pretreated slurry; Step three, dehydrating and forming the pretreated slurry to obtain a wet paper sheet; performing a dehydration treatment, a first drying treatment, a first sizing with a surface sizing agent, a second drying treatment and a first calendering treatment on the wet paper sheet, and rolling up to obtain a paper base; Step 4: forming a coating on one surface of the paper base, and performing a second sizing on the other surface of the paper base using a sizing material to obtain a cardboard composition.
9. The method for preparing the cardboard composition according to claim 8, characterized in that: The step 4 also includes a post-processing step; the post-processing step includes: The cardboard composition is subjected to a second calendering treatment; the vehicle speed of the second calendering treatment is 600m / min to 900m / min, the line pressure of the second calendering treatment is 90kN / m to 180kN / m, and the temperature of the second calendering treatment is 90℃ to 120℃.
10. Use of a preparation method comprising the pulp slurry composition according to any one of claims 1 to 2, the cardboard composition according to any one of claims 3 to 7, or the cardboard composition according to any one of claims 8 to 9 in preparing black core cardboard.
Citation Information
Patent Citations
Method for improving performance of paper stock in retention and drainage aiding
CN101634120A
Coated white cardboard and production process thereof
CN114277607A
High-whiteness coated white cardboard and preparation method thereof
CN116043612A
Soft color art paper and preparation method thereof
CN116289292A
Preparation method of base paper for waterproof and oilproof coating paperboard
CN117779516A
Cited By
Papermaking method of high-performance digital paper
CN119287696A
Electronic paper carrier tape body paper and surface sizing production method thereof
CN119686175A