Iron-silicon magnetic powder core and preparation method and application thereof
By grading and combining ferrosilicon magnetic powder in particle size and oxidizing and reducing treatment in a protective atmosphere, the problem of low magnetic permeability of the ferrosilicon magnetic powder core is solved, which significantly improves the magnetic permeability, expands the application range, and meets the requirements of the ferrosilicon magnetic powder core. Environmental protection and economic requirements.
Patent Information
- Application Number
- CN202411180263.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
AI Technical Summary
The existing ferrosilicon magnetic powder core has a low permeability, limiting its use in miniaturized and high permeability applications.
After particle size grading and combining the ferrosilicon magnetic powder, a first heat treatment is performed in a protective atmosphere to form an oxide film, and a reduction treatment is used to convert part or all of the oxide film into iron tetraoxide, thereby improving magnetic permeability.
It significantly improves the magnetic permeability of the ferrosilicon magnetic powder core, expands its application prospects, and uses non-toxic and low-cost raw materials to meet environmental protection requirements.
Smart Images

Figure BDA0005011922240000181 
Figure BDA0005011922240000191
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of magnetic powder cores, and relates to a method for preparing an iron silicon magnetic powder core, and in particular to an iron silicon magnetic powder core and a preparation method and application thereof. Background Art
[0002] In recent years, with the rapid development of high-tech fields such as new energy, photovoltaics and home appliances, the demand for inductors has evolved towards high efficiency, miniaturization and high current. As a result, the requirements for soft magnetic materials are low loss, high magnetic permeability and high saturation flux density. In addition to high magnetic permeability, high resistivity, low magnetostriction coefficient, low coercive force, low magnetocrystalline anisotropy coefficient and low power loss, magnetic powder core materials also have high magnetic saturation, that is, high Bs value, so they can meet the requirements of high current and high power.
[0003] As a type of magnetic powder core, iron silicon has a saturation flux density of up to 1.6T and good temperature stability. In addition, iron silicon magnetic powder cores also have excellent DC bias performance and low cost, so they have natural advantages in high current, high power and other fields. However, due to the limitations of the intrinsic properties of the material, the magnetic permeability of iron silicon magnetic powder cores is generally between 26 and 90. The low magnetic permeability limits the application of iron silicon in high permeability directions such as miniaturization and consumer electronics, which forces iron silicon magnetic powder cores to develop towards the goal of higher magnetic permeability and lower power consumption.
[0004] CN102303115A discloses a method for manufacturing an iron silicon material and a μ26 iron silicon magnetic powder core, including alloy smelting, powder making, powder reduction, powder classification, particle size ratio, powder passivation, insulation coating, compression molding, heat treatment and surface coating steps. A small amount of V and Nb elements are added during the alloy smelting process to improve the magnetic properties of the iron silicon alloy. The prepared powder is spherical and has a smooth surface, which is easy to be evenly coated. The obtained magnetic powder core has a high quality factor and excellent DC superposition characteristics.
[0005] CN116013678A discloses a method for preparing a low-loss iron silicon magnetic powder core material, which belongs to the technical field of magnetic materials. First, the invention uses an iron silicon alloy with a silicon content of 6.3-7.0% as a raw material, and prepares alloy powder by a gas atomization method, and then uses alkaline silica sol and polymethylphenylsiloxane to form an insulating coating liquid, and undergoes a gradient concentration treatment from low concentration, medium concentration to high concentration. The obtained iron silicon magnetic powder core has excellent physical properties and magnetic properties, and the insulating layer is effectively wrapped, which greatly reduces the magnetic loss of the magnetic powder core. The entire process is chromium-free and phosphorus-free, green and environmentally friendly, and has extremely high market application value.
[0006] The preparation methods of the iron silicon magnetic powder core disclosed in the prior art all have certain defects, and there is a problem that the magnetic permeability of the prepared iron silicon magnetic powder core is low. Therefore, it is very important to develop and design a new type of iron silicon magnetic powder core and its preparation method. Summary of the invention
[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide an iron silicon magnetic powder core and a preparation method and application thereof. The preparation method of the iron silicon magnetic powder core provided by the present invention comprises the following steps: grading the iron silicon magnetic powder into particles and then combining them; performing a first heat treatment in a protective atmosphere; performing an oxidation treatment to form an oxide film with high resistivity on the surface of the iron silicon magnetic powder; and performing a reduction treatment to partially or completely reduce the oxide film on the surface of the iron silicon magnetic powder to magnetic iron oxide, thereby improving the magnetic permeability of the obtained iron silicon magnetic powder core; therefore, the iron silicon magnetic powder core prepared by the preparation method has a higher magnetic permeability, and the obtained iron silicon magnetic powder core has a broader application prospect.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing an iron silicon magnetic powder core, the preparation method comprising:
[0010] The iron silicon magnetic powder is combined after being graded, and then subjected to a first heat treatment in a protective atmosphere, and then subjected to an oxidation treatment to form an oxide film, and then subjected to a reduction treatment to partially or completely reduce the oxide film to ferrosoferric oxide, and then subjected to a compression molding, and then subjected to a second heat treatment in a protective atmosphere to obtain an iron silicon magnetic powder core.
[0011] The preparation method of the iron silicon magnetic powder core provided by the present invention comprises the following steps: firstly subjecting the iron silicon magnetic powder to particle size classification and then combining the powder to obtain the optimal densely packed magnetic powder; then, subjecting the powder to a first heat treatment in a protective atmosphere, subjecting the powder to an oxidation treatment to form an oxide film with a high resistivity on the surface of the iron silicon magnetic powder; and then subjecting the powder to a reduction treatment to partially or completely reduce the oxide film on the surface of the iron silicon magnetic powder to magnetic iron oxide, thereby improving the magnetic permeability of the obtained iron silicon magnetic powder core; therefore, the iron silicon magnetic powder core prepared by the preparation method has a high magnetic permeability, and the obtained iron silicon magnetic powder core has a broader application prospect; in addition, the raw materials and reagents used in the preparation method are non-toxic and low in cost, and the preparation method has high economy and safety, and also meets the requirements of environmental protection.
[0012] Preferably, the particle size classification includes classifying the ferrosilicon magnetic powder into six levels according to the mesh number, the first level ferrosilicon magnetic powder is less than 120 mesh, the second level ferrosilicon magnetic powder is greater than or equal to 120 and less than 250 mesh, the third level ferrosilicon magnetic powder is greater than or equal to 250 mesh and less than 325 mesh, the fourth level ferrosilicon magnetic powder is greater than or equal to 325 and less than 500 mesh, the fifth level ferrosilicon magnetic powder is greater than or equal to 500 and less than 600 mesh, and the sixth level ferrosilicon magnetic powder is greater than or equal to 600 mesh.
[0013] Preferably, the combination is to combine the graded iron silicon magnetic powders to obtain combined iron silicon magnetic powders. Taking the mass of the combined iron silicon magnetic powders as 100%, the mass fraction of the first-grade iron silicon magnetic powders is 13-25%, the mass fraction of the second-grade iron silicon magnetic powders is 32%-45%, the mass fraction of the third-grade iron silicon magnetic powders is 25-34%, the mass fraction of the fourth-grade iron silicon magnetic powders is 7-15%, and the mass fraction of the fifth-grade iron silicon magnetic powders is 1-3%.
[0014] In the present invention, the mass fraction of the iron silicon magnetic powder after the combination is calculated as percent, and the mass fraction of the first-level iron silicon magnetic powder is 13-25%, for example, it can be 13%, 15%, 17%, 19%, 20%, 21%, 23% or 25%, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] In the present invention, the mass fraction of the iron silicon magnetic powder after the combination is calculated as 100%, and the mass fraction of the second-level iron silicon magnetic powder is 32-45%, for example, it can be 32%, 35%, 37%, 39%, 40%, 41%, 43% or 45%, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0016] In the present invention, the mass fraction of the iron silicon magnetic powder after the combination is calculated as percent, and the mass fraction of the third-level iron silicon magnetic powder is 25-34%, for example, it can be 25%, 27%, 29%, 30%, 32% or 34%, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] In the present invention, the mass fraction of the iron silicon magnetic powder after the combination is calculated as 100%, and the mass fraction of the fourth-level iron silicon magnetic powder is 7-15%, for example, it can be 7%, 9%, 10%, 11%, 12%, 14% or 15%, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] In the present invention, the mass fraction of the fifth-grade iron silicon magnetic powder is 1-3%, and the mass fraction of the fifth-grade iron silicon magnetic powder is 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8% or 3%. However, the above values are not limited to the above values, and other values not listed in the above value range are also applicable.
[0019] Preferably, the preparation method further comprises performing at least one shaping treatment on the ferrosilicon magnetic powder before the first heat treatment, wherein the shaping treatment comprises tableting, crushing and screening in sequence.
[0020] After the shaping process described in the present invention, the spherical iron silicon magnetic powder undergoes micro-deformation, which is beneficial to increasing the contact area between the iron silicon magnetic powders during the subsequent pressing and forming process, and improving the blank density and magnetic permeability of the iron silicon magnetic powder core.
[0021] Preferably, the iron silicon magnetic powder is prepared by a gas atomization method.
[0022] Preferably, the particle size of the iron silicon magnetic powder is not higher than 120 mesh, for example, it can be 120 mesh, 118 mesh, 115 mesh, 110 mesh, 105 mesh, 100 mesh, 95 mesh, 90 mesh, 80 mesh, 70 mesh or 60 mesh, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Preferably, based on the mass of the iron-silicon magnetic powder, the mass fraction of silicon in the iron-silicon magnetic powder is 3.5-6.5wt%, for example, it can be 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt% or 6.5wt%, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable, and the remainder is iron.
[0024] The preparation method provided by the present invention has certain universality, and no matter whether the silicon content in the iron silicon powder is low or high, the magnetic permeability of the prepared iron silicon magnetic powder is relatively high.
[0025] Preferably, the magnetic powder is subjected to three shaping treatments before the first heat treatment.
[0026] Preferably, the tableting pressure is 100-500T (tons), for example, it can be 100T, 150T, 200T, 250T, 300T, 350T, 400T, 450T or 500T, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable; when the tableting pressure in the present invention is too large (exceeding 500T), the hydraulic mechanical equipment used for tableting is greatly consumed, and the performance improvement is very small.
[0027] Preferably, the tableting is performed using a mechanical press.
[0028] Preferably, the first heat treatment includes a first temperature increase, a first temperature preservation and a first temperature decrease performed in sequence.
[0029] Preferably, the first heating rate is 2-10°C / min, and the end temperature is 600-900°C.
[0030] The first heating rate of the present invention is 2 to 10°C / min, for example, it can be 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] The terminal temperature of the first heating in the present invention is 600-900°C, for example, it can be 600°C, 650°C, 700°C, 750°C, 800°C, 850°C or 900°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the first insulation time is 0.5 to 3 hours, for example, 0.5 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the first cooling method includes natural cooling along with the furnace.
[0034] Preferably, the protective atmosphere comprises any one of hydrogen, nitrogen or an inert gas or a combination of at least two thereof, and typical but non-limiting combinations include a combination of hydrogen and nitrogen, a combination of nitrogen and an inert gas, or a combination of hydrogen, nitrogen and an inert gas.
[0035] Preferably, the oxidation treatment includes an oxidation heat treatment in an oxygen-containing atmosphere.
[0036] Preferably, the oxygen-containing atmosphere consists of oxygen and nitrogen and / or an inert gas.
[0037] Preferably, the oxygen content in the oxygen-containing atmosphere is 1-15%, for example, 1%, 3%, 5%, 7%, 9%, 11%, 13% or 15%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0038] The oxygen content in the oxygen-containing atmosphere in the present invention is the volume concentration of oxygen.
[0039] Preferably, the temperature of the oxidation heat treatment is 100-500° C., and the time is 10-180 min.
[0040] The temperature of the oxidation heat treatment in the present invention is 100-500°C, for example, it can be 100°C, 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C or 500°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] The time of the oxidative heat treatment of the present invention is 10 to 180 minutes, for example, it can be 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 100 minutes, 120 minutes, 140 minutes, 160 minutes or 180 minutes, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] Preferably, the preparation method further comprises a passivation treatment between the oxidation treatment and the reduction treatment.
[0043] The passivation treatment in the preparation method of the present invention can further oxidize the cracks between the oxide film formed on the surface of the iron silicon magnetic powder after the oxidation treatment, and can also further oxidize the iron silicon magnetic powder that has not been effectively oxidized in the re-oxidation treatment, thereby improving the density of the oxide film on the surface of the iron silicon magnetic powder and improving the resistivity of the final iron silicon magnetic powder core.
[0044] Preferably, the oxidation treatment and the passivation treatment also include passing through a 60-100 mesh sieve, for example, it can be 60 mesh, 65 mesh, 70 mesh, 75 mesh, 80 mesh, 85 mesh, 90 mesh, 95 mesh or 100 mesh, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0045] Preferably, the passivation treatment includes soaking in a passivating agent for 1 to 30 minutes, for example, 1 minute, 3 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes or 30 minutes, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0046] Preferably, the passivating agent comprises a hydrogen peroxide solution with a mass concentration of 5 to 20 wt%, for example, 5 wt%, 7 wt%, 9 wt%, 11 wt%, 13 wt%, 15 wt%, 17 wt% or 20 wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] Preferably, the soaking process is accompanied by stirring.
[0048] Preferably, the passivation treatment and the reduction treatment also include solid-liquid separation, drying and 60-100 mesh sieves, for example, 60 mesh, 65 mesh, 70 mesh, 75 mesh, 80 mesh, 85 mesh, 90 mesh, 95 mesh or 100 mesh, but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] Preferably, the drying temperature is 100-150° C. and the drying time is 30-120 min.
[0050] The drying temperature of the present invention is 100-150°C, for example, it can be 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0051] The drying time of the present invention is 30 to 120 minutes, for example, it can be 30 minutes, 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes, 110 minutes or 120 minutes, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0052] Preferably, the reduction treatment includes performing a reduction heat treatment in a reducing atmosphere containing a reducing gas.
[0053] Preferably, the reducing gas in the reducing atmosphere includes any one of hydrogen, carbon monoxide or methane or a combination of at least two of them. Typical but non-limiting combinations include a combination of hydrogen and carbon monoxide, a combination of carbon monoxide and methane, or a combination of hydrogen, carbon monoxide and methane.
[0054] Preferably, the reducing atmosphere consists of a reducing gas and nitrogen and / or an inert gas.
[0055] Preferably, the content of reducing gas in the reducing atmosphere is 5-15%, for example, it can be 1%, 3%, 5%, 7%, 9%, 11%, 13% or 15%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0056] The content of reducing gas in the reducing atmosphere in the present invention is the volume concentration of the reducing gas.
[0057] Preferably, the reduction heat treatment is carried out at a temperature of 100 to 500° C. and for a time of 10 to 180 minutes.
[0058] The temperature of the reduction heat treatment in the present invention is 100-500°C, for example, it can be 100°C, 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C or 500°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0059] The time of the reduction heat treatment in the present invention is 10 to 180 min, for example, it can be 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 100 min, 120 min, 140 min, 160 min or 180 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0060] Preferably, the reduction treatment and the pressing molding also include passing through a 60-100 mesh sieve, for example, it can be 60 mesh, 65 mesh, 70 mesh, 75 mesh, 80 mesh, 85 mesh, 90 mesh, 95 mesh or 100 mesh, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0061] Preferably, the reduction treatment and the pressing molding further include mixing the powder obtained from the reduction treatment with a demoulding powder.
[0062] Preferably, the demolding powder comprises any one of zinc stearate, aluminum stearate, mica powder or talc, or a combination of at least two of them. Typical but non-limiting combinations include a combination of zinc stearate and aluminum stearate, a combination of aluminum stearate and talc, or a combination of zinc stearate, aluminum stearate and talc.
[0063] Preferably, the mass ratio of the powder obtained by the reduction treatment to the demolding powder in the mixing is 100:(0.1-0.6), for example, it can be 100:0.1, 100:0.2, 100:0.3, 100:0.4, 100:0.5 or 100:0.6, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0064] Preferably, the mixing and the pressing molding also include passing through a 60-100 mesh sieve, for example, it can be 60 mesh, 65 mesh, 70 mesh, 75 mesh, 80 mesh, 85 mesh, 90 mesh, 95 mesh or 100 mesh, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0065] Preferably, the pressing pressure is 1800-2200 MPa, for example, it can be 1800 MPa, 1850 MPa, 1900 MPa, 1950 MPa, 2000 MPa, 2050 MPa, 2100 MPa, 2150 MPa or 2200 MPa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0066] Preferably, the second heat treatment further comprises a second temperature increase, a second temperature preservation and a second temperature decrease performed sequentially.
[0067] Preferably, the second heating rate is 5-15°C / min, and the end point temperature is 600-800°C.
[0068] The second heating rate in the present invention is 5 to 15°C / min, for example, it can be 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min or 15°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0069] The terminal temperature of the second heating in the present invention is 600-800°C, for example, it can be 600°C, 620°C, 640°C, 660°C, 680°C, 700°C, 720°C, 740°C, 760°C, 780°C or 800°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0070] Preferably, the second insulation time is 0.5 to 5 h, for example, it can be 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 45 h or 5 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0071] Preferably, the second cooling rate is 5 to 10°C / min, for example, it can be 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0072] Preferably, the protective atmosphere comprises any one of nitrogen and / or an inert gas or a combination of at least two of them.
[0073] In a second aspect, the present invention provides an iron silicon magnetic powder core, wherein the iron silicon magnetic powder core is obtained by the preparation method described in the first aspect.
[0074] In a third aspect, the present invention provides an application of the iron silicon magnetic powder core described in the second aspect, wherein the iron silicon magnetic powder core is used for new energy, photovoltaics and home appliances.
[0075] Compared with the prior art, the present invention has the following beneficial effects:
[0076] (1) In the preparation method of the iron silicon magnetic powder core provided by the present invention, the iron silicon magnetic powder is combined after particle size classification, which can achieve the optimal dense packing state. Under the same pressure, the magnetic ring has the maximum density, and the magnetic permeability of the iron silicon magnetic powder core is significantly improved;
[0077] (2) The method for preparing the iron silicon magnetic powder core provided by the present invention comprises the following steps: firstly subjecting the iron silicon magnetic powder to a first heat treatment in a protective atmosphere, and then subjecting the iron silicon magnetic powder to an oxidation treatment to form an oxide film with a high resistivity on the surface of the iron silicon magnetic powder, and then subjecting the iron silicon magnetic powder to a reduction treatment to partially or completely reduce the oxide film on the surface of the iron silicon magnetic powder to magnetic iron oxide, thereby improving the magnetic permeability of the obtained iron silicon magnetic powder core; therefore, the iron silicon magnetic powder core prepared by the preparation method has a higher magnetic permeability, and the obtained iron silicon magnetic powder core has a broader application prospect;
[0078] (3) The raw materials and reagents used in the preparation method of the iron silicon magnetic powder core provided by the present invention are non-toxic and low in cost. The preparation method has high economy and safety and meets environmental protection requirements;
[0079] (4) After the shaping treatment in the preparation method of the iron silicon magnetic powder core provided by the present invention, the spherical iron silicon magnetic powder undergoes micro-deformation, which is beneficial to increase the contact area between the iron silicon magnetic powders during the subsequent pressing and forming process, and improve the blank density and magnetic permeability of the iron silicon magnetic powder core;
[0080] (5) The passivation treatment in the preparation method of the iron silicon magnetic powder core provided by the present invention can further oxidize the cracks between the oxide film formed on the surface of the iron silicon magnetic powder after the oxidation treatment, and can also further oxidize the iron silicon magnetic powder that has not been effectively oxidized in the re-oxidation treatment, thereby improving the density of the oxide film on the surface of the iron silicon magnetic powder and improving the resistivity of the final iron silicon magnetic powder core. DETAILED DESCRIPTION
[0081] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0082] Example 1
[0083] This embodiment provides a method for preparing an iron silicon magnetic powder core, the preparation method comprising:
[0084] (1) The iron silicon magnetic powder (based on the mass of the iron silicon magnetic powder as 100%, the mass fraction of silicon in the iron silicon magnetic powder is 4.5wt%, and the remainder is iron) is classified into six grades according to the mesh size, the first grade iron silicon magnetic powder is less than 120 mesh, the second grade iron silicon magnetic powder is greater than or equal to 120 and less than 250 mesh, the third grade iron silicon magnetic powder is greater than or equal to 250 mesh and less than 325 mesh, the fourth grade iron silicon magnetic powder is greater than or equal to 325 and less than 500 mesh, the fifth grade iron silicon magnetic powder is greater than or equal to 500 and less than 600 mesh, and the sixth grade iron silicon magnetic powder is greater than or equal to 600 mesh;
[0085] The classified iron silicon magnetic powders are then combined to obtain combined iron silicon magnetic powders, wherein the mass fraction of the first-grade iron silicon magnetic powders is 20%, the mass fraction of the second-grade iron silicon magnetic powders is 40%, the mass fraction of the third-grade iron silicon magnetic powders is 30%, the mass fraction of the fourth-grade iron silicon magnetic powders is 8%, and the mass fraction of the fifth-grade iron silicon magnetic powders is 2% based on the mass of the combined iron silicon magnetic powders;
[0086] (2) performing three shaping processes on the first magnetic powder obtained in step (1) to obtain second magnetic powder;
[0087] The shaping process includes tableting, crushing and screening in sequence, the tableting pressure is 300T, and the screening is through an 80-mesh sieve;
[0088] (3) heating the second magnetic powder obtained in step (2) to 810° C. at a rate of 5° C. / min in a nitrogen atmosphere, maintaining the temperature for 1 hour, and then cooling the furnace to obtain a third magnetic powder;
[0089] (4) subjecting the third magnetic powder obtained in step (3) to an oxidation heat treatment at 300° C. for 120 min in an oxygen-containing atmosphere (oxygen content is 5%, nitrogen content is 95%), and after an oxide film is formed on the surface of the third magnetic powder, the third magnetic powder is sieved with an 80-mesh sieve to obtain a fourth magnetic powder;
[0090] (5) soaking the fourth magnetic powder obtained in step (4) in a hydrogen peroxide solution with a mass concentration of 10 wt% for 15 minutes to passivate the fourth magnetic powder, and drying and then passing through an 80-mesh sieve after solid-liquid separation to obtain a fifth magnetic powder;
[0091] (6) subjecting the fifth magnetic powder obtained in step (5) to a reduction heat treatment at 400° C. for 100 min in a reducing atmosphere (hydrogen content of 15% and nitrogen content of 85%) to reduce the oxide film on the surface of the fifth magnetic powder to ferroferric oxide, and then passing the sieve with 80 mesh to obtain a sixth magnetic powder;
[0092] (7) mixing the sixth magnetic powder obtained in step (6), zinc stearate and mica powder in a mass ratio of 100:0.3:0.05, passing through an 80-mesh sieve, and then pressing and molding at a pressure of 2200 MPa to obtain an embryo body;
[0093] (8) The embryo body obtained in step (7) is heated to 700° C. at a rate of 10° C. / min in a nitrogen atmosphere, kept at that temperature for 1 hour, and then cooled at a rate of 7° C. / min to obtain an iron silicon magnetic powder core.
[0094] Example 2
[0095] This embodiment provides a method for preparing an iron silicon magnetic powder core, the preparation method comprising:
[0096] (1) the iron silicon magnetic powder (based on the mass of the iron silicon magnetic powder as 100%, the mass fraction of silicon in the iron silicon magnetic powder is 3.5wt%, and the remainder is iron) is classified into six grades according to the mesh size, the first grade iron silicon magnetic powder is less than 120 mesh, the second grade iron silicon magnetic powder is greater than or equal to 120 and less than 250 mesh, the third grade iron silicon magnetic powder is greater than or equal to 250 mesh and less than 325 mesh, the fourth grade iron silicon magnetic powder is greater than or equal to 325 and less than 500 mesh, the fifth grade iron silicon magnetic powder is greater than or equal to 500 and less than 600 mesh, and the sixth grade iron silicon magnetic powder is greater than or equal to 600 mesh;
[0097] The classified iron silicon magnetic powders are then combined to obtain combined iron silicon magnetic powders, wherein the mass fraction of the first-grade iron silicon magnetic powders is 13%, the mass fraction of the second-grade iron silicon magnetic powders is 45%, the mass fraction of the third-grade iron silicon magnetic powders is 34%, the mass fraction of the fourth-grade iron silicon magnetic powders is 7%, and the mass fraction of the fifth-grade iron silicon magnetic powders is 1% based on the mass of the combined iron silicon magnetic powders;
[0098] (2) performing three shaping processes on the first magnetic powder obtained in step (1) to obtain second magnetic powder;
[0099] The shaping process includes tableting, crushing and screening in sequence, the tableting pressure is 100T, and the screening is through a 100-mesh sieve;
[0100] (3) heating the second magnetic powder obtained in step (2) to 600° C. at a rate of 2° C. / min in an argon atmosphere, maintaining the temperature for 3 h, and then cooling the furnace to obtain a third magnetic powder;
[0101] (4) subjecting the third magnetic powder obtained in step (3) to an oxidative heat treatment at 100° C. for 180 min in an oxygen-containing atmosphere (oxygen content is 15%, nitrogen content is 85%), and after an oxide film is formed on the surface of the third magnetic powder, the third magnetic powder is sieved with a 100-mesh sieve to obtain a fourth magnetic powder;
[0102] (5) soaking the fourth magnetic powder obtained in step (4) in a hydrogen peroxide solution with a mass concentration of 20 wt % for 1 minute to passivate the fourth magnetic powder, and drying and passing through a 100-mesh sieve after solid-liquid separation to obtain a fifth magnetic powder;
[0103] (6) subjecting the fifth magnetic powder obtained in step (5) to a reduction heat treatment at 100° C. for 180 min in a reducing atmosphere (hydrogen content of 10% and nitrogen content of 90%) to reduce the oxide film on the surface of the fifth magnetic powder to ferroferric oxide, and then passing the sieve through a 100-mesh sieve to obtain a sixth magnetic powder;
[0104] (7) mixing the sixth magnetic powder obtained in step (6) with zinc stearate in a mass ratio of 100:0.1, passing through a 100-mesh sieve, and then pressing and molding at a pressure of 1800 MPa to obtain an embryo body;
[0105] (8) The embryo body obtained in step (7) is heated to 800° C. at a rate of 15° C. / min in an argon atmosphere, kept at that temperature for 0.5 h, and then cooled at a rate of 10° C. / min to obtain an iron silicon magnetic powder core.
[0106] Example 3
[0107] This embodiment provides a method for preparing an iron silicon magnetic powder core, the preparation method comprising:
[0108] (1) the iron silicon magnetic powder (based on the mass of the iron silicon magnetic powder as 100%, the mass fraction of silicon in the iron silicon magnetic powder is 6.5wt%, and the remainder is iron) is classified into six grades according to the mesh size, the first grade iron silicon magnetic powder is less than 120 mesh, the second grade iron silicon magnetic powder is greater than or equal to 120 and less than 250 mesh, the third grade iron silicon magnetic powder is greater than or equal to 250 mesh and less than 325 mesh, the fourth grade iron silicon magnetic powder is greater than or equal to 325 and less than 500 mesh, the fifth grade iron silicon magnetic powder is greater than or equal to 500 and less than 600 mesh, and the sixth grade iron silicon magnetic powder is greater than or equal to 600 mesh;
[0109] The classified iron silicon magnetic powders are then combined to obtain combined iron silicon magnetic powders, wherein the mass fraction of the first-grade iron silicon magnetic powders is 25%, the mass fraction of the second-grade iron silicon magnetic powders is 32%, the mass fraction of the third-grade iron silicon magnetic powders is 25%, the mass fraction of the fourth-grade iron silicon magnetic powders is 15%, and the mass fraction of the fifth-grade iron silicon magnetic powders is 3% based on the mass of the combined iron silicon magnetic powders;
[0110] (2) performing three shaping processes on the first magnetic powder obtained in step (1) to obtain second magnetic powder;
[0111] The shaping process includes tableting, crushing and screening in sequence, the tableting pressure is 500T, and the screening is through a 60-mesh sieve;
[0112] (3) heating the second magnetic powder obtained in step (2) to 900° C. at a rate of 10° C. / min in a nitrogen atmosphere, maintaining the temperature for 0.5 h, and then cooling the furnace to obtain a third magnetic powder;
[0113] (4) subjecting the third magnetic powder obtained in step (3) to an oxidation heat treatment at 500° C. for 10 min in an oxygen-containing atmosphere (oxygen content is 1%, nitrogen content is 99%), and after an oxide film is formed on the surface of the third magnetic powder, the third magnetic powder is sieved with a 60-mesh sieve to obtain a fourth magnetic powder;
[0114] (5) soaking the fourth magnetic powder obtained in step (4) in a hydrogen peroxide solution with a mass concentration of 5 wt% for 30 minutes to passivate the fourth magnetic powder, and drying and then passing through a 60-mesh sieve after solid-liquid separation to obtain a fifth magnetic powder;
[0115] (6) subjecting the fifth magnetic powder obtained in step (5) to a reduction heat treatment at 500° C. for 10 min in a reducing atmosphere (hydrogen content of 5% and nitrogen content of 95%) to reduce the oxide film on the surface of the fifth magnetic powder to ferroferric oxide, and then passing the sieve through a 60-mesh sieve to obtain a sixth magnetic powder;
[0116] (7) mixing the sixth magnetic powder obtained in step (6) with aluminum stearate in a mass ratio of 100:0.6, passing the mixture through a 60-mesh sieve, and then pressing the mixture at a pressure of 2000 MPa to obtain an embryonic body;
[0117] (8) The embryo body obtained in step (7) is heated to 600° C. at a rate of 5° C. / min in a nitrogen atmosphere, kept at this temperature for 5 h, and then cooled at a rate of 5° C. / min to obtain an iron silicon magnetic powder core.
[0118] Example 4
[0119] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the pressure used for tableting in step (2) is 100 T.
[0120] Example 5
[0121] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the pressure used for tableting in step (2) is 500T.
[0122] Example 6
[0123] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the mass fraction of silicon in the iron silicon magnetic powder is 3.5wt% and the remainder is iron.
[0124] Example 7
[0125] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the mass fraction of silicon in the iron silicon magnetic powder is 5.5wt% and the remainder is iron.
[0126] Example 8
[0127] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the mass fraction of silicon in the iron silicon magnetic powder is 6.5wt% and the remainder is iron.
[0128] Example 9
[0129] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that step (2) is omitted.
[0130] Example 10
[0131] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the oxygen content in the oxygen-containing atmosphere in step (4) is 0.2% and the nitrogen content is 99.8%.
[0132] Embodiment 11
[0133] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the oxygen-containing atmosphere in step (4) is replaced by an air atmosphere.
[0134] Example 12
[0135] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of embodiment 1 except that the temperature of the oxidation heat treatment in step (4) is set to 80°C.
[0136] Example 13
[0137] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of embodiment 1 except that the temperature of the oxidation heat treatment in step (4) is set to 600°C.
[0138] Embodiment 14
[0139] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that step (5) is omitted.
[0140] Embodiment 15
[0141] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the hydrogen content in the reducing atmosphere in step (6) is 1% and the nitrogen content is 99%.
[0142] Example 16
[0143] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the hydrogen content in the reducing atmosphere in step (6) is 20% and the nitrogen content is 80%.
[0144] Embodiment 17
[0145] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the temperature of the reduction heat treatment in step (6) is 80°C.
[0146] Embodiment 18
[0147] This embodiment provides a method for preparing an iron silicon magnetic powder core, which is the same as that of Embodiment 1 except that the temperature of the reduction heat treatment in step (6) is 600°C.
[0148] Comparative Example 1
[0149] This comparative example provides a method for preparing an iron silicon magnetic powder core, which is the same as Example 1 except that step (1), i.e., the magnetic powder particle size classification combination, is omitted (the particle size combination of the original iron silicon magnetic powder is 11.3% <120 mesh, 23.6% 120-250 mesh, 32.3% 200-325 mesh, 18.6% 325-500 mesh, 9.1% 500-600 mesh, 5.1% >600 mesh).
[0150] Comparative Example 2
[0151] This comparative example provides a method for preparing an iron silicon magnetic powder core, which is the same as Example 1 except that step (4) is omitted.
[0152] Comparative Example 3
[0153] This comparative example provides a method for preparing an iron silicon magnetic powder core, which is the same as Example 1 except that step (6) is omitted.
[0154] The density of the iron silicon magnetic powder core obtained by the preparation method provided in the above embodiment and comparative example was tested by hydrostatic weighing method, and the density of the iron silicon magnetic powder core was shown in Table 1;
[0155] The iron silicon magnetic powder core prepared by the preparation method provided in the above embodiment and comparative example was subjected to inductance test. The test instrument was a CH3302 inductance tester with a test frequency and voltage of 100kHz / 1V and a test number of turns: 0.4mm 25Ts. The inductance of the iron silicon magnetic powder core obtained by the test was shown in Table 1.
[0156] Magnetic permeability (μ) is a measure of a material's ability to respond to a magnetic field. It describes the degree of magnetization of a material in a magnetic field. Magnetic permeability can be divided into absolute magnetic permeability (μ) and relative magnetic permeability (μr); absolute magnetic permeability refers to the degree of magnetization of a material under a unit magnetic field, while relative magnetic permeability refers to the magnetic permeability relative to a vacuum (or air); the relationship between inductance and magnetic permeability can be derived from the following formula: L = (μ0 × μr × A × N 2) / l, where L represents the inductance and μ0 is the magnetic permeability in a vacuum (approximately equal to 4π×10 -7 H / m), μr is the relative magnetic permeability, A is the cross-sectional area of the coil, N is the number of turns of the coil, l is the length of the magnetic path, and the magnetic permeability calculated from the inductance obtained by the test is shown in Table 1:
[0157] The magnetic loss test of the iron silicon magnetic powder core prepared by the preparation method provided in the above embodiment and comparative example was carried out. The testing instrument was a SY8219 power consumption tester. The testing conditions were 50kHz / 100mT. The number of test turns was 0.4mm 22×22Ts. The magnetic loss of the iron silicon magnetic powder core obtained by the test was shown in Table 1.
[0158] The resistivity of the iron silicon magnetic powder core prepared by the preparation method provided in the above embodiment and comparative example was tested by a four-probe method. The resistivity of the iron silicon magnetic powder core obtained by the test is shown in Table 1:
[0159] Table 1
[0160]
[0161]
[0162] From Table 1, we can get:
[0163] (1) The iron silicon magnetic powder core prepared by the preparation method provided in Examples 1 to 8 has a high magnetic permeability, a high density, a high inductance, a low magnetic loss and a high resistivity;
[0164] (2) By comparing Example 1 with Example 9, it can be seen that after the shaping treatment in the preparation method of the iron silicon magnetic powder core provided by the present invention, the spherical iron silicon magnetic powder undergoes micro-deformation, which is beneficial to increase the contact area between the iron silicon magnetic powders in the subsequent pressing process, and improve the blank density and magnetic permeability of the iron silicon magnetic powder core;
[0165] (3) By comparing Example 1 with Examples 10, 11 and Examples 12, 13, it can be seen that the oxygen content in the oxygen-containing atmosphere and the heat treatment temperature in the oxidation heat treatment of the preparation method of the present invention will affect the performance of the iron silicon magnetic powder core; when the oxygen content or the heat treatment temperature is too low, the resistivity of the iron silicon magnetic powder core will decrease and the magnetic loss will increase. This is because the low oxygen content cannot form a dense oxide layer on the surface of the magnetic powder, thereby reducing the resistivity of the iron silicon magnetic powder core and worsening the power consumption; when the oxygen content or the heat treatment temperature is too high, the density, inductance and magnetic permeability of the iron silicon magnetic powder core will decrease. This is because the excessively high oxygen content causes a loose and large-grained non-magnetic oxide layer to form quickly on the surface of the magnetic powder. The increase in the non-magnetic phase causes the magnetic permeability of the magnetic powder core to decrease sharply;
[0166] (4) By comparing Example 1 with Example 14, it can be seen that the passivation treatment in the preparation method of the iron silicon magnetic powder core provided by the present invention can further oxidize the cracks between the oxide film formed on the surface of the iron silicon magnetic powder after the oxidation treatment, and can also further oxidize the iron silicon magnetic powder that has not been effectively oxidized in the re-oxidation treatment, thereby improving the compactness of the oxide film on the surface of the iron silicon magnetic powder and improving the resistivity of the iron silicon magnetic powder core finally obtained;
[0167] (5) By comparing Example 1 with Examples 15, 16 and Examples 17, 18, it can be seen that the content of reducing gas in the reducing atmosphere and the heat treatment temperature in the reduction heat treatment of the preparation method of the present invention will affect the performance of the iron silicon magnetic powder core; when the content of reducing gas or the heat treatment temperature is too low, the density, inductance and magnetic permeability of the iron silicon magnetic powder core will be reduced. This is because the iron oxide on the surface of the iron silicon magnetic powder cannot be reduced to magnetic iron oxide due to the too low reducing gas content or heat treatment temperature, and the magnetic dilution in the magnetic powder core cannot be effectively contained, and the magnetic permeability cannot be improved; when the content of reducing gas or the heat treatment temperature is too high, the resistivity of the iron silicon magnetic powder core will be reduced and the magnetic loss will be worse. This is because the iron oxide layer is excessively reduced to iron due to the too high reducing gas content or heat treatment temperature, thereby reducing the resistivity of the iron silicon magnetic powder core and worsening the power consumption;
[0168] (6) By comparing Example 1 with Comparative Examples 1, 2 and 3, it can be seen that the preparation method of the iron silicon magnetic powder core provided by the present invention obtains the optimal densely packed magnetic powder by combining the iron silicon magnetic powder after particle size classification, and the obtained magnetic ring density is relatively high. The iron silicon magnetic powder is further subjected to a first heat treatment in a protective atmosphere, and then an oxidation treatment is performed to form an oxide film with a high resistivity on the surface of the iron silicon magnetic powder, and then a reduction treatment is performed to partially or completely reduce the oxide film on the surface of the iron silicon magnetic powder to magnetic iron oxide, thereby reducing magnetic dilution and improving the magnetic permeability of the obtained iron silicon magnetic powder core; therefore, the iron silicon magnetic powder core prepared by the preparation method has a higher magnetic permeability, and the obtained iron silicon magnetic powder core has a broader application prospect; in addition, the raw materials and reagents used in the preparation method of the iron silicon magnetic powder core provided by the present invention are non-toxic and low in cost, and the preparation method has high economy and safety, and also meets environmental protection requirements.
[0169] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing an iron silicon magnetic powder core, characterized in that: The preparation method comprises: The iron silicon magnetic powder is combined after being graded, and then subjected to a first heat treatment in a protective atmosphere, and then subjected to an oxidation treatment to form an oxide film, and then subjected to a reduction treatment to partially or completely reduce the oxide film to ferrosoferric oxide, and then subjected to a compression molding, and then subjected to a second heat treatment in a protective atmosphere to obtain an iron silicon magnetic powder core.
2. The preparation method according to claim 1, characterized in that: The particle size classification includes classifying the iron silicon magnetic powder into six levels according to the mesh number, the first level iron silicon magnetic powder is less than 120 mesh, the second level iron silicon magnetic powder is greater than or equal to 120 and less than 250 mesh, the third level iron silicon magnetic powder is greater than or equal to 250 mesh and less than 325 mesh, the fourth level iron silicon magnetic powder is greater than or equal to 325 and less than 500 mesh, the fifth level iron silicon magnetic powder is greater than or equal to 500 and less than 600 mesh, and the sixth level iron silicon magnetic powder is greater than or equal to 600 mesh; Preferably, the combination is to combine the graded iron silicon magnetic powders to obtain the combined iron silicon magnetic powders, and based on the mass of the combined iron silicon magnetic powders, the mass fraction of the first-grade iron silicon magnetic powders is 13-25%, the mass fraction of the second-grade iron silicon magnetic powders is 32-45%, the mass fraction of the third-grade iron silicon magnetic powders is 25-34%, the mass fraction of the fourth-grade iron silicon magnetic powders is 7-15%, and the mass fraction of the fifth-grade iron silicon magnetic powders is 1-3%; Preferably, the preparation method further comprises performing at least one shaping process on the iron silicon magnetic powder before the first heat treatment, wherein the shaping process comprises tableting, crushing and screening in sequence; Preferably, based on the mass of the iron silicon magnetic powder, the mass fraction of silicon in the iron silicon magnetic powder is 3.5-6.5wt%, and the remainder is iron; Preferably, the particle size of the iron silicon magnetic powder is not higher than 120 mesh; Preferably, the magnetic powder is subjected to three shaping treatments before the first heat treatment; Preferably, the tabletting pressure is 100-500T.
3. The preparation method according to claim 1 or 2, characterized in that: The first heat treatment includes a first temperature increase, a first temperature preservation and a first temperature decrease performed in sequence; Preferably, the first heating rate is 2-10°C / min, and the end temperature is 600-900°C; Preferably, the first insulation time is 0.5 to 3 hours; Preferably, the first cooling method includes natural cooling along with the furnace.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The oxidation treatment includes performing an oxidation heat treatment in an oxygen-containing atmosphere; Preferably, the oxygen content in the oxygen-containing atmosphere is 1 to 15%; Preferably, the temperature of the oxidation heat treatment is 100-500° C., and the time is 10-180 min.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The preparation method further comprises a passivation treatment between the oxidation treatment and the reduction treatment; Preferably, the passivation treatment comprises soaking in a passivating agent for 1 to 30 minutes; Preferably, the passivating agent comprises a hydrogen peroxide solution with a mass concentration of 5 to 20 wt%.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The reduction treatment comprises performing a reduction heat treatment in a reducing atmosphere containing a reducing gas; Preferably, the reducing gas in the reducing atmosphere includes any one of hydrogen, carbon monoxide or methane, or a combination of at least two thereof; Preferably, the content of reducing gas in the reducing atmosphere is 5-15%; Preferably, the reduction heat treatment is carried out at a temperature of 100 to 500° C. and for a time of 10 to 180 minutes.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The reduction treatment and the pressing molding further include mixing the powder obtained by the reduction treatment with the demoulding powder; Preferably, the mass ratio of the powder obtained by reduction treatment to the demolding powder in the mixing is 100:(0.1-0.6); Preferably, the compression molding pressure is 1800-2200 MPa.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The second heat treatment further includes a second temperature increase, a second temperature preservation and a second temperature decrease performed sequentially; Preferably, the second heating rate is 5-15°C / min, and the end temperature is 600-800°C; Preferably, the second insulation time is 0.5 to 5 hours; Preferably, the second cooling rate is 5-10°C / min.
9. An iron silicon magnetic powder core, characterized in that: The iron silicon magnetic powder core is obtained by the preparation method according to any one of claims 1 to 8.
10. An application of the iron silicon magnetic powder core according to claim 9, characterized in that: The iron silicon magnetic powder core is used in new energy, photovoltaics and home appliances.
Citation Information
Patent Citations
Composite soft magnetic powder core and preparation method thereof
CN101996723A
Preparation method for low-loss FeSi6.5 soft magnetic composite powder core
CN106409461A
Preparation method for low loss iron silicon aluminum magnetic powder core
CN108777227A
Fe-based soft magnetic composite material and preparation method thereof
CN109727745A
Method of manufacturing oxide-coated soft magnetic powder, oxide-coated soft magnetic powder, dust core, and magnetic element
JP2009088502A
Cited By
Preparation method of low-loss high-direct-current-superposition iron-silicon / iron-nickel composite magnetic powder core