Broaching method for high-pressure corrosion foil

Through the two-step pore reaming method, the pore size is controlled in the nitric acid solution by using organic acid and macromolecular corrosion inhibitor, which solves the problem of uneven pore type in the aluminum electrolytic capacitor, improves the specific capacitance and pore utilization, simplifies the process and reduces the The cost.

CN118969513APending Publication Date: 2024-11-15DONGGUAN DONGYANG SOLAR SCI RES & DEV CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411212422.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In existing aluminum electrolytic capacitors, the uneven pore type of corrosive foil leads to insufficient specific capacitance, and the traditional hole reaming process is costly, complex, and the aperture size cannot be accurately controlled, making the preparation of conical holes with small upper and large lower cannot be achieved.

Method used

The two-step hole expansion method is adopted. The first step is to use the first hole expansion corrosion solution to use organic acids such as phosphoric acid as corrosion inhibitors to expand the surface pore size under the action of current. The second step is to use macromolecular corrosion inhibitors such as polystyrene sulfonic acid, The internal pore size is expanded under the action of current to form conical tunnel holes with small upper and large lower lower, and all processes are based on nitric acid solution to reduce costs.

Benefits of technology

The specific capacitance of corrosive foil is improved, which avoids hole clogging and improves the utilization rate of internal holes. It has a simple process and low cost, and can accurately control the aperture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020637710000101
    Figure BDA0005020637710000101
  • Figure HDA0005020637720000011
    Figure HDA0005020637720000011
  • Figure HDA0005020637720000012
    Figure HDA0005020637720000012
Patent Text Reader

Abstract

The invention relates to the field of aluminum electrolytic capacitors, in particular to a chambering method for high-voltage corrosion foil, which comprises the following steps of: performing primary chambering corrosion treatment on the corrosion foil subjected to pitting corrosion by adopting first chambering corrosion liquid; carrying out secondary chambering corrosion treatment on the corrosion foil subjected to the primary chambering corrosion treatment by adopting a second chambering corrosion liquid; wherein the first reaming corrosive liquid comprises a first salpeter solution and a first corrosion inhibitor; the first corrosion inhibitor comprises at least one of organic acid, inorganic acid, organic acid salt and inorganic acid salt; the second reaming corrosive liquid comprises a second salpeter solution and a second corrosion inhibitor; the second corrosion inhibitor comprises at least one of polystyrolsulfon acid, polyacrylic acid, polyethylene glycol, polystyrene sulfonate and polyacrylate. Therefore, the hole pattern of the final corrosion foil is a big-end-down conical hole, the surface and internal hole diameters of the corrosion foil can be accurately controlled, the process is simple, the cost is low, and implementation is easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aluminum electrolytic capacitors, and in particular to a hole expansion method for high-voltage corrosion foil. Background Art

[0002] In recent years, aluminum electrolytic capacitors, as a basic electronic component, have been increasingly used in emerging fields such as new energy, in addition to being used in the traditional electronics industry. With social development and technological progress, the industry has also put forward higher requirements for the performance of aluminum electrolytic capacitors, among which miniaturization and higher specific capacitance anode foil have always been the goals pursued by the aluminum electrolytic capacitor industry.

[0003] As the basic material for manufacturing aluminum electrolytic capacitors, the performance of the etched foil determines the performance of the final aluminum electrolytic capacitor to a certain extent. According to the capacitor anode foil capacitance formula C = ε0ε r S / d, in the aluminum electrolytic capacitor industry, the key to improving the specific capacitance of the anode foil lies in manufacturing an etched foil with a higher specific surface area. The general etched foil manufacturing process includes four steps: pre-treatment, pore etching, hole expansion etching, and post-treatment. The role of the pre-treatment is to clean the surface of the plain foil, and it also has a certain pre-hole arrangement effect; the role of the pore etching is to etch a certain number and depth of etched holes on the plain foil; the role of the hole expansion corrosion is to expand the etched holes into tunnel holes with a specific aperture to prevent the subsequent formation steps from clogging the etched holes; the role of the post-treatment is to clean the residual chloride ions in the etched holes. These steps will have an impact on the performance of the etched foil.

[0004] In the manufacturing process of the corrosion foil, the most ideal state is that the corrosion holes formed in the hole-making step have uniform surfaces and consistent lengths of the corrosion holes. In the hole-expanding process, the corrosion holes are expanded into tunnel holes with consistent apertures on the upper and lower sides (foil surface and inside the foil), thereby obtaining the corrosion foil with the highest specific surface area. However, in reality, since the corrosion foil hole-making process is a process of continuous power-on for a certain period of time, the holes formed in the hole-making process are sequential, resulting in the problem of long and short holes in the final corrosion holes, and the hole density of different corrosion depths shows a trend of gradually decreasing. This is also a common technical difficulty and bottleneck in the industry, and there is no method to completely avoid it. In this case, the inventor of the present application found in the process development that controlling the hole shape of the final tunnel hole through the hole-expanding corrosion step so that the final corrosion hole presents a cone with a small top and a large bottom is more conducive to increasing the specific surface area of ​​the corrosion foil, thereby improving the performance of the corrosion foil. The advantage of this hole shape is that the number of corrosion holes on the surface of the corrosion foil can be maximized without merging holes, and since the density of the corrosion holes inside the corrosion foil is smaller than the surface, the expansion of its aperture will not cause merging holes, and the larger aperture also avoids the problem of corrosion hole blockage during the corrosion foil formation process.

[0005] At present, there are few reports on the preparation method of tapered holes in etching foil that are small at the top and large at the bottom. Most of them tend to prepare cylindrical tunnel holes with consistent apertures. However, in actual process production, due to the reduced hole density at different depths of the etching foil, the cylindrical tunnel hole cannot fully utilize the internal space of the etching foil and is not the most ideal etching hole type. In addition, the preparation method of tapered holes in etching foil that are small at the top and large at the bottom in the prior art has the following two shortcomings: first, two etching tank liquids are used in the hole expansion process, which increases certain production costs and complexity; second, this process can produce tunnel holes with small apertures at the top and large apertures at the bottom, but it cannot achieve precise control of the apertures on the surface and inside of the etching foil, which is insufficient for practical applications.

[0006] Therefore, it is urgent to develop a hole expansion process for high-voltage etching foil to solve the shortcomings of the hole shape in the traditional hole expansion process, so that the final hole shape of the etching foil presents a conical tunnel hole that is small at the top and large at the bottom, thereby improving the specific capacitance of the etching foil. The process should be simple and easy to implement, with low cost, and at the same time, it can achieve precise control of the surface pore size and internal pore size. Summary of the invention

[0007] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the present invention provides a method for expanding a hole of a high-pressure etching foil, so that the final hole shape of the etching foil presents a tapered hole with a small top and a large bottom, and the surface and internal pore diameters of the etching foil can be precisely controlled, the process is simple, the cost is low, and it is easy to implement.

[0008] To this end, the first aspect of the present invention provides a method for expanding a hole of a high-voltage corrosion foil, comprising:

[0009] The first hole enlarging etching liquid is used to perform a first hole enlarging etching treatment on the corroded foil that has undergone the hole enlarging etching;

[0010] Using a second hole-expanding etching solution to perform a second hole-expanding etching treatment on the etching foil that has undergone the first hole-expanding etching treatment;

[0011] Wherein, the first hole-expanding etching solution comprises a first nitric acid solution and a first corrosion inhibitor;

[0012] The first corrosion inhibitor includes at least one of an organic acid, an inorganic acid, an organic acid salt, and an inorganic acid salt;

[0013] The second hole enlarging etching solution includes a second nitric acid solution and a second corrosion inhibitor;

[0014] The second corrosion inhibitor includes at least one of polystyrene sulfonic acid, polyacrylic acid, polyethylene glycol, polystyrene sulfonate, and polyacrylic acid salt.

[0015] In order to solve the deficiencies in the prior art, the present invention provides a high-pressure etching foil hole expansion process, which includes a two-step hole expansion treatment, using two hole expansion etching solutions, wherein the first hole expansion etching solution contains a first corrosion inhibitor (at least one of an organic acid, an inorganic acid, an organic acid salt, and an inorganic acid salt) with a weak surface pore size protection ability, under the action of electric current, the pore size of the corrosion hole on the surface of the corrosion foil is rapidly expanded to an ideal size, while the pore size of the internal pore changes slightly, and at this time, the corrosion hole on the corrosion foil presents an inverted cone morphology with a large top and a small bottom; the second hole expansion etching solution contains a first corrosion inhibitor with a surface pore size protection ability A strong macromolecular second corrosion inhibitor (at least one of polystyrene sulfonic acid, polyacrylic acid, polyethylene glycol, polystyrene sulfonate, and polyacrylic acid salt) is used to place the corrosion foil that has undergone primary hole expansion corrosion treatment in the second hole expansion corrosion solution for secondary hole expansion corrosion treatment. Due to the presence of the macromolecular second corrosion inhibitor with strong surface pore protection ability, the surface pore size of the corrosion foil no longer changes significantly. Under the action of current, the internal pore size will mainly be enlarged. After a certain period of corrosion, the internal pore size of the corrosion hole is larger than the surface pore size, forming a tapered tunnel hole that is beneficial to the improvement of the specific capacitance of the corrosion foil. In addition, the above two hole expansion corrosion solutions are based on nitric acid solution, that is, there is no need to replace the basic tank liquid system, which is low in cost and easy to implement.

[0016] According to an embodiment of the present invention, the first corrosion inhibitor includes at least one of phosphoric acid, boric acid, silicic acid, phosphates, borates, and silicates.

[0017] According to an embodiment of the present invention, the concentration of the first corrosion inhibitor in the first hole-expanding etching solution is 0.001-10wt%; preferably 0.005-5wt%; preferably 0.01-1wt%.

[0018] According to an embodiment of the present invention, the concentration of nitric acid in the first nitric acid solution is 1-15 wt %, preferably 3-10 wt %.

[0019] According to an embodiment of the present invention, the second corrosion inhibitor includes at least one of polystyrene sulfonic acid, polyacrylic acid, polyethylene glycol, sodium polystyrene sulfonate, and sodium polyacrylate.

[0020] According to an embodiment of the present invention, the concentration of the second corrosion inhibitor in the second hole enlarging etching solution is 0.001-10wt%; preferably 0.005-5wt%; preferably 0.01-1wt%.

[0021] According to an embodiment of the present invention, the concentration of nitric acid in the second nitric acid solution is 1-15 wt %, preferably 3-10 wt %.

[0022] According to an embodiment of the present invention, in the first-stage hole enlargement corrosion treatment, the current density is controlled to be 0.10-1.0A / cm 2; preferably 0.10-0.60A / cm 2 ; preferably 0.20-0.60A / cm 2 .

[0023] According to an embodiment of the present invention, in the primary hole expansion corrosion treatment, the power-on time is 100-400s, preferably 150-350s.

[0024] According to an embodiment of the present invention, the temperature of the primary hole expansion corrosion treatment is 50-100°C, preferably 60-80°C.

[0025] According to an embodiment of the present invention, in the secondary hole enlargement corrosion treatment, the current density is controlled to be 0.10-1.0A / cm 2 ; preferably 0.10-0.60A / cm 2 ; preferably 0.20-0.60A / cm 2 .

[0026] According to an embodiment of the present invention, in the secondary hole expansion corrosion treatment, the power-on time is 100-600s, preferably 150-500s.

[0027] According to an embodiment of the present invention, the temperature of the secondary hole expansion corrosion treatment is 50-100°C, preferably 60-80°C.

[0028] According to an embodiment of the present invention, the hole expansion method further comprises:

[0029] The etched foil that has undergone the secondary hole expansion etching treatment is post-treated.

[0030] According to an embodiment of the present invention, the post-processing includes:

[0031] The corrosion foil which has undergone the secondary hole enlargement corrosion treatment is immersed in a nitric acid solution, cleaned, and dried to obtain the high-pressure corrosion foil.

[0032] A second aspect of the present invention provides a high voltage etching foil, wherein the high voltage etching foil is prepared by the hole expanding method described in the first aspect.

[0033] Compared with the traditional hole-type corrosion foil, the high-pressure corrosion foil provided by the present invention has a corrosion hole structure with small top and large bottom, and the internal corrosion hole utilization rate is higher, which can avoid the corrosion hole blockage during the sample formation process, and the sample performance is improved to a certain extent.

[0034] A third aspect of the present invention provides an aluminum electrolytic capacitor, comprising the high-voltage corrosion foil described in the second aspect.

[0035] This results in an aluminum electrolytic capacitor with a higher capacitance.

[0036] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood through the description of the embodiments in conjunction with the following drawings, in which:

[0038] Figure 1 The scanning electron microscope image of the sample surface polished to 10 μm in Example 1 of the present invention is shown;

[0039] Figure 2 The scanning electron microscope image of the sample of Example 1 of the present invention with a surface polished to 30 μm is shown;

[0040] Figure 3 shows a cross-sectional scanning electron microscope image of the sample of Example 1 of the present invention;

[0041] Figure 4 The scanning electron microscope image of the sample surface polished to 10 μm in Comparative Example 1 of the present invention is shown;

[0042] Figure 5 The scanning electron microscope image of the surface of the sample of comparative example 1 of the present invention polished to 30 μm is shown;

[0043] Figure 6 The cross-sectional scanning electron microscope image of the sample of Comparative Example 1 of the present invention is shown;

[0044] Figure 7 The scanning electron microscope image of the surface of the sample of comparative example 2 of the present invention with a polishing time of 10 μm is shown;

[0045] Figure 8 The scanning electron microscope image of the surface of the sample of comparative example 2 of the present invention polished to 30 μm is shown;

[0046] Fig. 9 The cross-sectional scanning electron microscope image of the sample of Comparative Example 2 of the present invention is shown. DETAILED DESCRIPTION

[0047] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be understood as limiting the present invention.

[0048] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Further, in the description of the present invention, unless otherwise specified, the meaning of "plurality" is two or more.

[0049] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0050] In order to make the present invention more easily understood, certain technical and scientific terms are specifically defined below. Unless otherwise clearly defined elsewhere in this document, all other technical and scientific terms used herein have the meanings commonly understood by those skilled in the art to which the present invention belongs.

[0051] In this document, the terms “include” or “comprising” are open expressions, that is, including the contents specified in the present invention but not excluding other contents.

[0052] As used herein, the terms "optionally", "optional" or "optionally" generally mean that the subsequently described event or circumstance may but need not occur, and that the description includes instances where the event or circumstance occurs and instances where it does not.

[0053] The existing hole expansion process has the following shortcomings: (1) It is mostly used to prepare cylindrical tunnel holes. Due to the phenomenon of long and short holes in the corrosion foil, the hole density of different depths is reduced, and the cylindrical tunnel hole cannot fully utilize the internal space of the foil, which is not conducive to the improvement of the specific capacitance of the corrosion foil; (2) Different hole expansion tank liquids are used in the hole expansion process, which increases the complexity of the process and production cost; (3) It is impossible to accurately control the upper and lower apertures of the tapered hole, and it is impossible to adjust the hole shape and aperture of the tunnel hole according to specific requirements, so as to achieve the best hole structure. To this end, the present invention provides a hole expansion method for high-voltage corrosion foil, which is completed in two parts. By using the different effects of corrosion inhibitors and the influence of hole expansion time on the aperture, the hole shape and aperture of the corrosion hole can be accurately controlled, so that the final state of the corrosion hole is kept optimal, the specific capacitance of the corrosion foil is improved, and the problem of the difficulty in improving the specific capacitance of the traditional cylindrical tunnel hole corrosion foil is solved. At the same time, although the hole expansion step is divided into two parts, the basic hole expansion tank liquid used is the same tank liquid, and only the type of corrosion inhibitor is different, which can reduce the production process changes to a certain extent, reduce costs, and the process is simple and easy.

[0054] According to an embodiment of the present invention, the present invention provides a method for expanding a hole of a high-voltage corrosion foil in a first aspect, comprising:

[0055] (1) A first hole enlarging etching solution is used to perform a first hole enlarging etching treatment on the etched foil that has undergone pore etching.

[0056] According to a specific embodiment of the present invention, the first hole-enlarging etching solution includes a first nitric acid solution and a first corrosion inhibitor; the first corrosion inhibitor includes at least one of an organic acid, an inorganic acid, an organic acid salt, and an inorganic acid salt. Among them, the first corrosion inhibitor is an acidic corrosion inhibitor with weak surface pore protection ability, which can rapidly expand the pore size of the corrosion holes on the surface of the corrosion foil to an ideal size, while the internal pore size changes slightly, and the corrosion holes present an inverted cone morphology with a large top and a small bottom. In addition, the hole-enlarging etching solution does not need to replace the existing basic etching solution system (i.e., nitric acid solution as the basic etching solution), and is low-cost and easy to implement.

[0057] According to a specific embodiment of the present invention, the first corrosion inhibitor is preferably phosphoric acid, boric acid, silicic acid, phosphate, borate, silicate, and more preferably phosphoric acid and boric acid. Its concentration in the first hole-expanding etching solution is not particularly limited, and those skilled in the art can make a reasonable selection according to actual needs. As some specific examples, the concentration of the first corrosion inhibitor in the first hole-expanding etching solution is 0.001-10wt%; preferably 0.005-5wt%; preferably 0.01-1wt%, for example 0.001wt%, 0.005wt%, 0.01wt%, 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt% %, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, etc. The amount of the corrosion inhibitor added is small, easy to operate in actual production, and will not increase the production cost.

[0058] According to a specific embodiment of the present invention, the concentration of the first nitric acid solution is not particularly limited, and those skilled in the art can make a reasonable selection according to actual needs. As some specific examples, the concentration of the first nitric acid solution may be 1-15wt%; preferably 3-10wt%, for example 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, etc.

[0059] According to a specific embodiment of the present invention, the first-stage hole enlargement corrosion treatment is carried out under constant direct current, and the current density in the first-stage hole enlargement corrosion treatment is preferably 0.10-1.0A / cm 2 ; preferably 0.10-0.60A / cm 2 ; preferably 0.20-0.60A / cm 2, for example 0.10A / cm 2 , 0.20A / cm 2 , 0.30A / cm 2 , 0.40A / cm 2 , 0.50A / cm 2 , 0.60A / cm 2 , 0.7A / cm 2 , 0.8A / cm 2 , 0.9A / cm 2 , 1.0A / cm 2 wait.

[0060] According to a specific embodiment of the present invention, in the first-stage hole expansion corrosion treatment, the power-on time can be used to adjust the pore size on the foil surface and inside, and the size of each pore size is controlled by the length of the power-on time, so as to accurately control the hole taper and each pore size according to actual needs. Personnel in this field can make reasonable choices according to actual needs. As some specific examples, in the first-stage hole expansion corrosion treatment, the power-on time is preferably 100-400s; preferably 150-350s, such as 100s, 150s, 200s, 250s, 300s, 350s, 400s, etc.

[0061] According to a specific embodiment of the present invention, the temperature of the first-level hole expansion corrosion treatment is not particularly limited, and those skilled in the art can make a reasonable choice based on actual needs. As some specific examples, the temperature of the first-level hole expansion corrosion treatment can be 50-100°C; preferably 60-80°C, for example 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc.

[0062] According to a specific embodiment of the present invention, the aluminum foil can be washed with pure water at room temperature after the primary hole expansion etching process. In addition, the hole formation method of the etched foil does not affect the subsequent hole expansion etching process, that is, the etched foil that has been etched with hole formation can be used in the present invention.

[0063] (2) using a second hole-expanding etching solution to perform a second hole-expanding etching treatment on the etching foil that has undergone the first hole-expanding etching treatment.

[0064] According to a specific embodiment of the present invention, the second hole-expanding etching solution includes a second nitric acid solution and a second corrosion inhibitor; the second corrosion inhibitor includes at least one of polystyrene sulfonic acid, polyacrylic acid, polyethylene glycol, polystyrene sulfonate, and polyacrylic acid. Among them, the second corrosion inhibitor is a macromolecular corrosion inhibitor with strong surface pore protection ability, which can prevent the surface pore size of the corrosion foil from changing significantly, and mainly changes the internal pore size. After a certain period of corrosion, the internal pore size is larger than the surface pore size, forming a conical tunnel hole that is beneficial to the improvement of the specific capacitance of the corrosion foil. At the same time, in addition, the hole-expanding etching solution does not need to replace the existing basic etching solution system (i.e., nitric acid as the basic etching solution), and the cost is low and easy to implement.

[0065] According to a specific embodiment of the present invention, the second corrosion inhibitor is preferably polystyrene sulfonic acid, polyacrylic acid, polyethylene glycol, sodium polystyrene sulfonate, sodium polyacrylate. Its concentration in the second hole-expanding etching solution is not particularly limited, and those skilled in the art can make a reasonable selection according to actual needs. As some specific examples, the concentration of the second corrosion inhibitor in the second hole-expanding etching solution is 0.001-10wt%; preferably 0.005-5wt%; preferably 0.01-1wt%, for example 0.001wt%, 0.005wt%, 0.01wt%, 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt% %, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, etc. The amount of the corrosion inhibitor added is small, easy to operate in actual production, and will not increase the production cost.

[0066] According to a specific embodiment of the present invention, the concentration of the second nitric acid solution is not particularly limited, and those skilled in the art can make a reasonable selection according to actual needs. As some specific examples, the concentration of the second nitric acid solution may be 1-15wt%; preferably 3-10wt%, for example 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, etc.

[0067] According to a specific embodiment of the present invention, the secondary hole enlargement corrosion treatment is carried out under constant direct current. In the secondary hole enlargement corrosion treatment, the current density is preferably 0.10-1.0 A / cm 2 ; preferably 0.10-0.60A / cm 2; preferably 0.20-0.60A / cm 2 , for example 0.01A / cm 2 , 0.20A / cm 2 , 0.30A / cm 2 , 0.40A / cm 2 , 0.50A / cm 2 , 0.60A / cm 2 , 0.7A / cm 2 , 0.8A / cm 2 , 0.9A / cm 2 , 1.0A / cm 2 wait.

[0068] According to a specific embodiment of the present invention, in the secondary hole expansion corrosion treatment, the power-on time can be used to adjust the aperture of the corrosion holes on the surface and inside of the corrosion foil, and the size of each aperture is controlled by the length of the power-on time, so as to accurately control the hole taper and each aperture according to actual needs. Personnel in this field can make reasonable choices according to actual needs. As some specific examples, in the secondary hole expansion corrosion treatment, the power-on time is preferably 100-600s; preferably 150-500s, such as 100s, 150s, 200s, 250s, 300s, 350s, 400s, 450s, 500s, 550s, 600s, etc.

[0069] According to a specific embodiment of the present invention, the temperature of the secondary hole expansion corrosion treatment is not particularly limited, and those skilled in the art can make a reasonable selection based on actual needs. As some specific examples, the temperature of the secondary hole expansion corrosion treatment may be 50-100°C; preferably 60-80°C, for example 50°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc.

[0070] According to a specific embodiment of the present invention, the aluminum foil may be washed with pure water at room temperature after the secondary hole expansion corrosion treatment.

[0071] According to a specific embodiment of the present invention, the method may further include a post-processing step, that is, post-processing the corrosion foil that has undergone secondary hole expansion corrosion treatment. The specific method is not particularly limited, and those skilled in the art can make a reasonable choice based on actual needs. As some specific examples, the corrosion foil that has undergone secondary hole expansion corrosion treatment can be immersed in a 50-75°C, 4-10wt% nitric acid solution for 30-180s, and the aluminum foil is washed with pure water at room temperature, and placed at 60-100°C to dry for 10-30min to obtain the high-voltage corrosion foil.

[0072] According to an embodiment of the present invention, a second aspect of the present invention provides a high voltage corrosion foil, which is prepared by the hole expansion method described in the first aspect.

[0073] Compared with the traditional hole-type corrosion foil, the high-pressure corrosion foil provided by the present invention has a corrosion hole structure with small top and large bottom, and the internal corrosion hole utilization rate is higher, which can avoid the corrosion hole blockage during the sample formation process, and the sample performance is improved to a certain extent.

[0074] According to an embodiment of the present invention, a third aspect of the present invention provides an aluminum electrolytic capacitor, comprising the high-voltage corrosion foil described in the second aspect.

[0075] Therefore, the aluminum electrolytic capacitor has better performance.

[0076] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer and are all conventional products that can be obtained commercially.

[0077] Example 1

[0078] The hole expansion process of the high-voltage corrosion foil provided in this embodiment includes the following steps:

[0079] (1) Primary hole expansion corrosion treatment:

[0080] The etched foil after the hole is placed in the first hole expansion etching solution for primary hole expansion etching treatment. The first hole expansion etching solution includes a first nitric acid solution and a first corrosion inhibitor. The concentration of the first nitric acid solution is 5wt%. The first corrosion inhibitor is phosphoric acid. The concentration of phosphoric acid in the first hole expansion etching solution is 0.01wt%. Constant current hole expansion etching is performed at a temperature of 70°C, and the current density used is 0.20A / cm 2 , the power-on time is 150s, and then the aluminum foil is washed with pure water at room temperature;

[0081] (2) Secondary hole expansion corrosion treatment:

[0082] The corroded foil treated in step (1) is placed in a second hole-expanding etching solution for secondary hole-expanding etching treatment. The second hole-expanding etching solution includes a second nitric acid solution and a second corrosion inhibitor. The concentration of the second nitric acid solution is 5wt%. The second corrosion inhibitor is sodium polystyrene sulfonate. The concentration of sodium polystyrene sulfonate in the second hole-expanding etching solution is 0.01wt%. Constant current hole-expanding etching is performed at a temperature of 70°C, and the current density used is 0.20A / cm 2 , the power-on time is 400s, and then the aluminum foil is washed with pure water at room temperature;

[0083] (3) Post-processing:

[0084] The corroded foil obtained by the step (2) is immersed in a 6.5 wt% nitric acid aqueous solution at 65° C. for 120 seconds, and then the aluminum foil is washed with pure water at room temperature;

[0085] (4) Drying treatment:

[0086] The etched foil obtained in step (3) is placed at 80° C. for drying for 20 minutes to obtain a high-voltage etched foil.

[0087] Example 2

[0088] The difference between this embodiment and embodiment 1 is that:

[0089] In step (1), the concentration of the first corrosion inhibitor in the first hole enlarging etching solution is 1wt%, and the power-on time is 350s;

[0090] In step (2), the concentration of the second corrosion inhibitor in the second hole enlarging etching solution is 1wt%, and the power-on time is 200s.

[0091] Example 3

[0092] The difference between this embodiment and embodiment 1 is that:

[0093] In step (1), the concentration of the first corrosion inhibitor in the first hole enlarging etching solution is 0.5wt%, and the power-on time is 200s;

[0094] In step (2), the concentration of the second corrosion inhibitor in the second hole enlarging etching solution is 0.5wt%, and the power-on time is 350s.

[0095] Example 4

[0096] The difference between this embodiment and embodiment 1 is that:

[0097] The first corrosion inhibitor in step (1) is boric acid.

[0098] Example 5

[0099] The difference between this embodiment and embodiment 1 is that:

[0100] The second corrosion inhibitor in step (2) is polyethylene glycol.

[0101] Comparative Example 1

[0102] The difference between this embodiment and embodiment 1 is that:

[0103] The conventional high-voltage foil hole enlargement corrosion process was adopted, and the hole enlargement corrosion treatment was carried out using a single-stage constant current. The etching solution included a nitric acid solution and a corrosion inhibitor. The concentration of the nitric acid solution was 5wt%, and the corrosion inhibitor added was phosphoric acid. The concentration of phosphoric acid in the etching solution was 0.01wt%. The constant current hole enlargement corrosion was carried out at a temperature of 70°C, and the current density used was 0.2A / cm 2 , the power-on time is 550s.

[0104] Comparative Example 2

[0105] The difference between this embodiment and embodiment 1 is that:

[0106] A single continuous hole enlargement corrosion treatment was adopted, the corrosion solution included a nitric acid solution and a corrosion inhibitor, the concentration of the nitric acid solution was 5wt%, the corrosion inhibitor added was sodium polystyrene sulfonate, the concentration of sodium polystyrene sulfonate in the corrosion solution was 0.01wt%, and the constant current hole enlargement corrosion was carried out at a temperature of 70°C, and the current density used was 0.2A / cm 2 , the power-on time is 550s.

[0107] Test example:

[0108] 1. Scanning electron microscope test:

[0109] The surface scanning electron microscope test and cross-sectional scanning electron microscope test were performed on the etched foils obtained in Example 1 and Comparative Examples 1-2, respectively. Figure 1-9 The surface SEM test is performed by polishing the sample surface to 10μm or 30μm before performing the SEM test.

[0110] The results show that: (1) a tapered tunnel hole with a small top and a large bottom is formed in the etched foil obtained in Example 1, and the two-step hole expansion controls the surface pore size and the internal pore size respectively, so that it reaches a relatively ideal pore size; the number of internal pores is smaller than the number of surface pores, and even if the internal pore size is larger, no pores will be formed inside the etched foil, but there are still many unetched areas. The larger internal pore size makes more effective use of the internal space of the aluminum foil;

[0111] (2) Comparative Example 1 forms a cylindrical tunnel hole with the same upper and lower apertures. After the number of internal holes is reduced, the relatively small aperture fails to fully utilize the internal space of the aluminum foil, resulting in more uncorroded areas being wasted;

[0112] (3) Comparative Example 2 adopts a single continuous hole expansion corrosion, and the corrosion inhibitor is a single sodium polystyrene sulfonate, which has a strong ability to protect the surface of the corrosion foil. The holes on the surface of the corrosion foil are difficult to expand during the hole expansion process. Therefore, with the same amount of electricity added, the pore size on the surface of the corrosion foil is too small, which will also affect the improvement of the comprehensive performance of the corrosion foil.

[0113] 2. Formation test:

[0114] The corrosion foil samples obtained in Examples 1-5 and Comparative Examples 1-2 were chemically processed respectively. The chemical processing conditions were: using 8 wt % boric acid, at 90 ° C, and a current of 5 A / dm 2 The electrode foil was formed under the conditions of Vfe=600V. The test results of the electrode foil after formation are shown in Table 1.

[0115] Table 1

[0116]

[0117]

[0118] Based on the performance of the etching foil obtained in Comparative Example 1 (set as 100%), a 600Vf etching foil was prepared using a 127μm thick plain foil. As shown in Table 1, compared with Comparative Example 1, the thickness and bending strength of the etching foils obtained in Examples 1-5 did not change significantly, and the electrostatic capacitance per unit area was effectively improved. The specific capacitance of the etching foils obtained in Examples 1-5 was better than that of the etching foil obtained in Comparative Example 1, and the specific capacitance was improved by 3.4%-5.2%, indicating that the use of the hole expansion process in Examples 1-5 can prepare etching foils with better performance. In addition, compared with Comparative Example 2, the specific capacitance of the etching foils obtained in Examples 1-5 is also higher, indicating that the use of the two-stage hole expansion process in Examples 1-5 can effectively improve the comprehensive performance of the etching foil.

[0119] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0120] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for expanding a hole in a high-voltage corrosion foil, characterized in that: include: The first hole enlarging etching liquid is used to perform a first hole enlarging etching treatment on the corroded foil that has undergone the hole enlarging etching; Using a second hole-expanding etching solution to perform a second hole-expanding etching treatment on the etching foil that has undergone the first hole-expanding etching treatment; Wherein, the first hole-expanding etching solution comprises a first nitric acid solution and a first corrosion inhibitor; The first corrosion inhibitor includes at least one of an organic acid, an inorganic acid, an organic acid salt, and an inorganic acid salt; The second hole enlarging etching solution includes a second nitric acid solution and a second corrosion inhibitor; The second corrosion inhibitor includes at least one of polystyrene sulfonic acid, polyacrylic acid, polyethylene glycol, polystyrene sulfonate, and polyacrylic acid salt.

2. The hole enlarging method according to claim 1, characterized in that: The first corrosion inhibitor includes at least one of phosphoric acid, boric acid, silicic acid, phosphates, borates, and silicates; Optionally, the concentration of the first corrosion inhibitor in the first hole-enlarging etching solution is 0.001-10wt%; preferably 0.005-5wt%; preferably 0.01-1wt%.

3. The hole enlarging method according to claim 1, characterized in that: The concentration of nitric acid in the first nitric acid solution is 1-15 wt %, preferably 3-10 wt %.

4. The hole enlarging method according to claim 1, characterized in that: The second corrosion inhibitor includes at least one of polystyrene sulfonic acid, polyacrylic acid, polyethylene glycol, sodium polystyrene sulfonate, and sodium polyacrylate; Optionally, the concentration of the second corrosion inhibitor in the second hole enlarging etching solution is 0.001-10wt%; preferably 0.005-5wt%; preferably 0.01-1wt%.

5. The hole enlarging method according to claim 1, characterized in that: The concentration of nitric acid in the second nitric acid solution is 1-15 wt %, preferably 3-10 wt %.

6. The hole enlarging method according to claim 1, characterized in that: In the first stage hole enlargement corrosion treatment, the current density is controlled to be 0.10-1.0A / cm 2 ; preferably 0.10-0.60A / cm 2 ; preferably 0.20-0.60A / cm 2 ; Optionally, in the primary hole expansion corrosion treatment, the power-on time is 100-400s; preferably 150-350s; Optionally, the temperature of the primary hole expansion corrosion treatment is 50-100°C; preferably 60-80°C.

7. The hole enlarging method according to claim 1, characterized in that: In the secondary hole enlargement corrosion treatment, the current density is controlled to be 0.10-1.0A / cm 2 ; preferably 0.10-0.60A / cm 2 ; preferably 0.20-0.60A / cm 2 ; Optionally, in the secondary hole expansion corrosion treatment, the power-on time is 100-600s; preferably 150-500s; Optionally, the temperature of the secondary hole expansion corrosion treatment is 50-100°C; preferably 60-80°C.

8. The hole enlarging method according to claim 1, characterized in that: The hole expansion method further comprises: Post-processing the corrosion foil after the secondary hole expansion corrosion treatment; Optionally, the post-processing comprises: The corrosion foil which has undergone the secondary hole enlargement corrosion treatment is immersed in a nitric acid solution, cleaned, and dried to obtain the high-pressure corrosion foil.

9. A high-voltage corrosion foil prepared by the hole expansion method according to any one of claims 1 to 8.

10. An aluminum electrolytic capacitor, characterized in that: The invention comprises the high voltage corrosion foil as claimed in claim 9.

Citation Information

Cited By

  • Anode foil, preparation method thereof and aluminum electrolytic capacitor

    CN119889934A

  • Anode foil and method of making same and aluminum electrolytic capacitor

    CN119889934B