Dry-method pole piece, preparation method thereof and secondary battery
By etching inverted triangle grooves on the surface of the first dry diaphragm of the dry diaphragm and converting them into gaps during winding, the reduction of polarity, poor electrolyte wetting and rolling in the existing dry diaphragm is solved. The problem of high surround stress improves the charging speed, rate performance and cycle life of lithium-ion batteries, and reduces internal resistance.
Patent Information
- Application Number
- CN202411068985.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
The existing dry electrode sheets in lithium-ion batteries have reduced polarity, reduced intermolecular force, and poor hydrophilicity, which affects the wetting properties of the electrolyte and lithium ion transport. , and the stress generated during winding leads to increased internal resistance, damage to safety performance and cycle life.
Design a dry electrode sheet, using a current collector to combine with the first and second dry diaphragms, the surface of the first dry diaphragm is etched into an inverted triangle groove, increasing the surface area and electrolyte wetting, and in the roll When winding, the grooves are converted into gaps to buffer stress and reduce local stress.
It improves the transmission speed of lithium ions in the active substance, shortens the charging and discharging time, improves the charging speed and rate performance of the secondary battery, extends the cycle life, reduces the internal resistance, and enhances the safety performance of the battery.
Smart Images

Figure CN118969956A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of dry-process electrodes, and in particular to a dry-process electrode sheet and a preparation method thereof, and a secondary battery. Background Art
[0002] Lithium-ion batteries have high energy density, long cycle life and good safety performance, and are widely used in modern society. At present, improving energy density is still one of the important directions of battery development. Large-sized, high-load, and high-density thick electrodes help to increase the proportion of active substances in single cells, which is of great significance for improving the energy density of lithium-ion batteries.
[0003] Compared with the traditional wet process, the dry process is to mix the active material, conductive agent and binder powder, form a dry film under the fibrillation effect of the binder, and then combine it with the current collector to form a dry electrode. This process can increase the thickness of the electrode, which is conducive to obtaining an electrode with a high proportion of active materials in the single cell, thereby helping to improve the energy density of lithium-ion batteries. However, the current dry process usually uses polytetrafluoroethylene (PTFE) as a binder. The inert fluoride ions in the PTFE molecule have strong electronegativity, which usually leads to a decrease in the polarity of the dry electrode, a decrease in the intermolecular force, and poor hydrophilicity. Moreover, the thicker electrode itself is not conducive to its wettability to the electrolyte, and it will also cause the transmission of lithium ions to be blocked, which is not conducive to the charge and discharge rate of the battery.
[0004] During the production process of lithium-ion batteries, the pole pieces also need to be wound. The stress generated during the winding process inevitably creates the risk of bending, wrinkling, and even breaking of the pole pieces. It also causes the internal resistance of the pole pieces to increase and the heat to increase, which has adverse effects on the safety performance and cycle life of the power battery. Summary of the invention
[0005] In view of this, the present application provides a dry electrode to solve at least one of the above technical problems.
[0006] To achieve the above-mentioned objectives, the present application provides a dry electrode, comprising a current collector, a first dry membrane and a second dry membrane, the current collector being arranged between the first dry membrane and the second dry membrane, a plurality of grooves being arranged on the surface of the first dry membrane facing away from the current collector, and when observed along the width direction of the dry electrode, the groove is triangular and one of the vertices of the groove is arranged toward the current collector, the groove does not penetrate the first dry membrane along the thickness direction of the dry electrode, and a plurality of the grooves are arranged at intervals along the length direction of the first dry membrane.
[0007] In some possible implementations, along the length direction, the maximum width of the groove is 55 μm to 80 μm; and the depth of the groove is 20 μm to 50 μm.
[0008] In some possible implementations, the groove does not penetrate the first dry film along the width direction of the dry electrode, and along the width direction, a distance between an edge of the groove and an edge of the dry film is 1 mm to 3 mm.
[0009] The present application also provides a secondary battery, including an electrode assembly, the electrode assembly is a winding structure and includes a dry electrode sheet, the dry electrode sheet includes a current collector, a first dry membrane sheet and a second dry membrane sheet, the current collector is arranged between the first dry membrane sheet and the second dry membrane sheet, the first dry membrane sheet is arranged toward the winding center axis of the electrode assembly, and a plurality of gaps are provided on the surface of the first dry membrane sheet facing away from the current collector, the gaps do not penetrate the first dry membrane sheet along the thickness direction of the dry electrode sheet, and the plurality of gaps are arranged at intervals along the length direction of the first dry membrane sheet.
[0010] In some possible implementations, the gap includes a first end and a second end that are arranged opposite to each other, the first end is closer to the winding center axis than the second end, and the spacing between the second ends of two adjacent gaps is 1 mm to 2 mm.
[0011] The present application also provides a method for preparing the dry-process electrode, comprising:
[0012] A current collector is provided, and a first dry film and a second dry film are respectively arranged on the two surfaces of the current collector; a plurality of grooves are etched on the surface of the first dry film away from the current collector using a laser to obtain the dry electrode; wherein, when observed along the width direction of the dry electrode, the groove is triangular and one of the vertices of the groove is arranged toward the current collector, the groove does not penetrate the first dry film along the thickness direction of the dry electrode, and the plurality of grooves are arranged at intervals along the length direction of the first dry film.
[0013] In some possible implementations, the etching includes: setting the spot diameter of the laser to d1, and performing one etching along the laser scanning path; setting the spot diameter of the laser to d2, and performing two etchings along the laser scanning path; setting the spot diameter of the laser to d3, and performing three etchings along the laser scanning path; wherein d1>d2>d3.
[0014] In some possible implementations, the spot diameter d1 of the laser is 50 μm to 60 μm, and d3 is 20 μm to 35 μm.
[0015] In some possible implementations, the power of the laser is 10 W to 70 W, or the pulse frequency of the laser is 50 kHz to 60 kHz.
[0016] In some possible implementations, the distance between any two adjacent laser scanning paths is 1 mm to 2 mm.
[0017] In the dry-process electrode of the present application, a groove having an inverted triangle shape is formed on the surface of the dry-process membrane, which can increase the surface area of the dry-process electrode with relatively less loss of active material, help to accelerate the transmission of lithium ions in the active material, and shorten the charge and discharge time. Therefore, when the dry-process electrode is prepared into a secondary battery, it helps to increase the charging speed of the secondary battery; moreover, the increase in surface area improves the electrolyte wettability of the dry-process electrode, reduces the electrolyte standing time of the dry-process electrode during the aging process, and helps to improve the rate performance and capacity release of the secondary battery, thereby facilitating the inhibition of lithium dendrites and improving the cycle life of the secondary battery. When the dry-process electrode of the present application is wound to form a secondary battery, the groove on the surface of the dry-process membrane is converted into a gap, so the groove can provide a buffer space for the dry-process electrode when it is wound, thereby effectively reducing the local stress generated by the winding, reducing the internal resistance, and helping to release the capacity of the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 A three-dimensional schematic diagram of a dry electrode provided in one embodiment of the present application.
[0019] Figure 2 for Figure 1 The schematic cross-sectional view of the thickness direction of the dry electrode is shown.
[0020] Figure 3 for Figure 2 A partial enlarged view of the dry electrode is shown.
[0021] Figure 4 A schematic cross-sectional view of the structure of a secondary battery provided in one embodiment of the present application.
[0022] Figure 5 for Figure 4 A partial enlarged view of the secondary battery shown.
[0023] Main component symbols
[0024] Dry electrode 100
[0025] Current Collectors 101
[0026] The first dry film 102
[0027] The second dry film 103
[0028] Groove 110
[0029] Secondary battery 200
[0030] Winding center axis 10
[0031] Positive electrode 11
[0032] Negative electrode 12
[0033] Isolation film 13
[0034] Gap 120
[0035] First end 121
[0036] Second end 122 DETAILED DESCRIPTION
[0037] The embodiments of the present application are described in detail below. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application; it should be noted that, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by technicians in the technical field of the present application; in the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other; many specific details are elaborated in the following description to facilitate a full understanding of the present application, and the described embodiments are only part of the embodiments of the present application, not all of the embodiments.
[0038] In the embodiments of the present application, for the convenience of description and not to limit the present application, the term "connection" used in the patent application specification and claims of the present application is not limited to physical or mechanical connection, whether direct or indirect. "Up", "down", "above", "below", "left", "right", etc. are only used to indicate relative position relationship. When the absolute position of the described object changes, the relative position relationship also changes accordingly.
[0039] Although the dry process can increase the thickness of the electrode and the content of active substances, the current dry process usually uses PTFE as a binder. The inert fluoride ions in the PTFE molecules have strong electronegativity, which usually leads to a decrease in the polarity of the dry electrode, a decrease in the intermolecular force, and poor hydrophilicity. In addition, the thicker electrode itself is not conducive to its wettability to the electrolyte, and it will also cause the transmission of lithium ions to be blocked, which is not conducive to the charge and discharge rate of the battery.
[0040] An embodiment of the present application provides a dry electrode 100, see Figure 1 and Figure 2, comprising a current collector 101, a first dry film 102 and a second dry film 103, wherein the current collector 101 is disposed between the first dry film 102 and the second dry film 103, and a plurality of grooves 110 are disposed on a surface of the first dry film 102 away from the current collector 101, see Figure 2 , observed along the width direction of the dry electrode 100, the groove 110 is triangular and one of the vertices of the groove 110 is set toward the current collector 101, the groove 110 does not penetrate the first dry membrane 102 along the thickness direction of the dry electrode 100, and the plurality of grooves 110 are arranged at intervals along the length direction of the first dry membrane 102.
[0041] The present application provides a groove 110 having an inverted triangle shape on the surface of the first dry-process membrane 102, which loses relatively little active material, and on this basis increases the surface area of the dry-process electrode 100, which helps to accelerate the transmission of lithium ions in the active material and shorten the charging and discharging time. Therefore, when the dry-process electrode 100 is prepared as a secondary battery, it is beneficial to increase the charging speed of the secondary battery. Moreover, the increase in surface area further promotes the electrolyte wettability of the dry-process electrode 100, reduces the electrolyte standing time of the dry-process electrode 100 during the aging process, and helps to improve the rate performance and capacity release of the secondary battery, thereby helping to inhibit lithium dendrites and improve the cycle life of the secondary battery.
[0042] In some embodiments, see Figure 3 , along the length direction, the maximum width g of the groove 110 is 55μm to 80μm. For example, the maximum width g can be 55μm, 60μm, 65μm, 70μm, 75μm, 80μm or any value within the range formed by any two of the above values. In the present application, the width of the groove 110 gradually decreases along the thickness direction of the dry diaphragm (that is, as the depth of the depression deepens), so the maximum width g refers to the opening width of the groove 110 on the surface of the first dry diaphragm 102. Controlling the maximum width within the range is beneficial to improving the surface area and electrolyte wettability of the dry electrode 100 on the basis of relatively less active material loss.
[0043] In some embodiments, see Figure 3, the depth h of the groove 110 is 20μm to 50μm. For example, the depth h can be 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm or any value within the range formed by any two of the above values. In the present application, since the cross-section of the groove 110 is an inverted triangle, it has different depression depths at different depression sites. The depth h is the distance between the inverted triangle vertex at the bottom of the depression and the surface of the first dry film 102. Controlling the depth within the range ensures that the groove 110 does not penetrate the first dry film 102 in the thickness direction, avoiding damage to the current collector 101. On the other hand, it is beneficial to control the surface area and electrolyte wettability of the dry electrode 100 on the basis of relatively less active material loss.
[0044] In some embodiments, the groove 110 does not penetrate the first dry film 102 along the width direction of the dry electrode 100, and the distance between the edge of the groove 110 and the edge of the first dry film 102 along the width direction is 1 mm to 3 mm. Controlling the distance within the above range can ensure that the groove 110 does not penetrate the first dry film 102 in the width direction, thereby preventing electrolyte leakage, and can form enough grooves 110 to improve the surface area of the dry electrode 100 and the electrolyte wettability.
[0045] An embodiment of the present application further provides a secondary battery 200, see Figure 4 and Figure 5 , including an electrode assembly, the electrode assembly is a winding structure and includes a positive electrode sheet 11, a negative electrode sheet 12 and a separator 13. The separator 13 is provided between the positive electrode sheet 11 and the negative electrode sheet 12 to prevent the positive electrode sheet 11 and the negative electrode sheet 12 from contacting and short-circuiting. Among them, any one of the positive electrode sheet 11 and the negative electrode sheet 12 can adopt the above-mentioned dry electrode sheet 100, and the dry electrode sheet 100 includes a current collector 101, a first dry film sheet 102 and a second dry film sheet 103. The current collector 101 is arranged between the first dry film sheet 102 and the second dry film sheet 103. The first dry film sheet 102 is arranged toward the winding center axis 10 of the electrode assembly. A plurality of gaps 120 are provided on the surface of the first dry film sheet 102 away from the current collector 101. The gaps 120 do not penetrate the first dry film sheet 102 along the thickness direction of the dry electrode sheet 100, and the plurality of gaps 120 are arranged at intervals along the length direction of the first dry film sheet 102.
[0046] In the related art, the stress generated during the winding process of the pole piece creates the risk of bending, wrinkling, and even breaking of the pole piece, and also causes the internal resistance of the pole piece to increase and the heat to intensify, which has a significant impact on the safety performance and cycle life of the power battery. In the present application, an inverted triangular groove 110 is formed on the surface of the first dry film 102, and the groove 110 is converted into a gap 120 after the dry pole piece 100 is wound. Therefore, the groove 110 can provide a buffer space during the winding process of the dry pole piece 100, which can effectively reduce the local stress generated by the winding, reduce the internal resistance, and help release the capacity of the secondary battery 200.
[0047] In some embodiments, see Figure 5 The slit 120 includes a first end 121 and a second end 122 that are arranged opposite to each other, the first end 121 is closer to the winding center axis 10 than the second end 122, and the spacing between the second ends 122 of two adjacent slits 120 is 1 mm to 2 mm. For example, the spacing can be 1 mm, 1.2 mm, 1.4 mm, 1.5 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2 mm, or any value within the range formed by any two of the above values. Controlling the spacing within the above range is conducive to releasing the internal stress generated when the pole piece is wound.
[0048] Another embodiment of the present application provides a method for preparing the dry electrode 100, comprising:
[0049] The first step is to provide a current collector 101 , and to arrange a first dry-process membrane 102 and a second dry-process membrane 103 on two surfaces of the current collector 101 .
[0050] In some embodiments, the current collector 101 includes one of a carbon-coated current collector and a perforated current collector.
[0051] In some embodiments, when preparing the positive electrode sheet 11, the first dry film 102 or the second dry film 103 includes a positive electrode active material, a conductive agent and an adhesive. In other embodiments, when preparing the negative electrode sheet 12, the first dry film 102 or the second dry film 103 includes a negative electrode active material, a conductive agent and an adhesive. The positive electrode active material includes one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide and lithium cobalt oxide. The negative electrode active material includes one or more of graphite, soft carbon, hard carbon, and mesophase carbon microspheres; the conductive agent includes one or more of conductive carbon black, carbon nanotubes, graphene, carbon fiber, acetylene black and Ketjen black. The adhesive includes PTFE.
[0052] In some embodiments, in the first dry film 102 or the second dry film 103, the mass percentage of the positive electrode active material or the negative electrode active material is 80% to 98%, the mass percentage of the conductive agent is 1% to 10%, and the mass percentage of the adhesive is 1% to 10%. For example, the mass percentage of the positive electrode active material or the negative electrode active material can be 80%, 82%, 83%, 85%, 87%, 90%, 92%, 95%, 96%, 97%, 98%, or any value within the range of any two of the above values. The mass percentage of the conductive agent can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10, or any value within the range of any two of the above values. The mass percentage of the adhesive can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10, or any value within the range of any two of the above values.
[0053] Based on the dry process, the first dry diaphragm 102 or the second dry diaphragm 103 is mixed by the above materials, fiberized into a film under the action of the adhesive PTFE, and formed by calendering. In some embodiments, the thickness of the first dry diaphragm 102 or the second dry diaphragm 103 is 200μm to 500μm. For example, the thickness can be 200μm, 250μm, 300μm, 350μm, 400μm, 450μm, 500μm or any value within the range composed of any two of the above values. The dry electrode 100 is obtained by compounding the first dry diaphragm 102, the second dry diaphragm 103 with the collector 101. In some embodiments, the thickness of the dry electrode 100 is 210μm to 510μm.
[0054] Step 2: Use laser to etch a plurality of grooves 110 on the surface of the first dry film 102 away from the current collector 101 to obtain the dry electrode 100; wherein, when observed along the width direction of the dry electrode 100, the groove 110 is triangular and one of the vertices of the groove 110 is set toward the current collector 101, the groove 110 does not penetrate the first dry film 102 along the thickness direction of the dry electrode 100, and the plurality of grooves 110 are arranged at intervals along the length direction of the first dry film 102.
[0055] In some embodiments, the etching includes: setting the spot diameter of the laser to d1, and performing one etching along the laser scanning path; setting the spot diameter of the laser to d2, and performing two etchings along the laser scanning path; setting the spot diameter of the laser to d3, and performing three etchings along the laser scanning path; wherein d1>d2>d3.
[0056] As the spot diameter of the laser gradually decreases at the same etching position, an inverted triangular groove 110 recessed in the thickness direction of the dry electrode 100 may be formed on the surface of the first dry film 102. It can be understood that by repeating the above process on multiple laser scanning paths, multiple grooves 110 may be formed on the surface of the first dry film 102, and the multiple laser scanning paths are arranged at intervals along the length direction of the first dry film 102.
[0057] In some embodiments, the spot diameter d1 of the laser is 50 μm to 60 μm, and d3 is 20 μm to 35 μm. For example, the spot diameter d1 can be 50 μm, 51 μm, 52 μm, 53 μm, 54 μm, 55 μm, 56 μm, 57 μm, 58 μm, 59 μm, 60 μm, or any value within the range formed by any two of the above values. The spot diameter d3 can be 20 μm, 22 μm, 23 μm, 25 μm, 26 μm, 28 μm, 30 μm, 31 μm, 33 μm, 34 μm, 35 μm, or any value within the range formed by any two of the above values. It can be understood that after determining d1 and d3, d2 can select any value that meets the relationship based on the relationship of d1>d2>d3.
[0058] In some embodiments, the power of the laser is 10W to 70W, or the pulse frequency of the laser is 50kHZ to 60kHZ. The power or pulse frequency of the laser is controlled within the above range, thereby controlling the energy of the laser and realizing the use of the laser to perform etching exceeding the damage threshold of the dry film. The material composition, compaction density, surface density, etc. of the etching object constitute the damage resistance of the etching object. Controlling the power and pulse frequency of the laser within the above range can ensure that damage can be formed on the surface of the first dry film 102, promote the formation of the groove 110, and at the same time will not penetrate the first dry film 102 in the thickness direction, avoiding damage to the current collector 101.
[0059] In some embodiments, the spacing between any two adjacent laser scanning paths is 1 mm to 2 mm. For example, the spacing may be 1 mm, 1.2 mm, 1.4 mm, 1.5 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2 mm, or any value within the range formed by any two of the above values. Such a setting promotes the formation of spaced grooves 110 on the surface of the first dry film 102, and the density of the grooves 110 can be controlled. By forming grooves 110 of suitable density, on the one hand, the loss of active materials can be controlled, and on the other hand, it is beneficial to increase the surface area of the dry electrode 100, thereby improving the wettability of the electrolyte.
[0060] The scheme of the present application will be explained below in conjunction with the embodiments. Those skilled in the art will understand that the following examples are only used to explain the present application and cannot be construed as limiting the present application. Unless otherwise stated, the reagents, software and instruments not specifically stated in the following embodiments are all conventional commercial products or open source.
[0061] Embodiment 1:
[0062] S1: Provide a dry positive electrode sheet, including, by mass percentage, 95% lithium iron phosphate active material, 2% binder, and 3% conductive agent; the binder material is powdered polytetrafluoroethylene, and the conductive agent is conductive carbon black. The mixed powder is processed in a jet mill for 15 minutes, and after calendering and compounding with the current collector, the thickness is 350μm.
[0063] S2: On the dry film on one of the surfaces of the dry electrode obtained in S1, a high-power MOPA fiber laser is used for laser scanning to etch a groove with an inverted triangle cross-section; including using a multiple scanning method, setting the etching spot diameter to d1, d2, d3, gradually reducing the laser spot diameter, removing material layer by layer, and forming an inverted triangle groove. The overlap rate of each scan is set between 50% and 70% to ensure the uniformity of etching and the accuracy of the groove shape. The laser setting parameters and the obtained groove results are shown in Table 1.
[0064] S3: The dry-process electrode with inverted triangular grooves obtained in S2 is prepared into a cylindrical battery cell by winding.
[0065] Embodiment 2:
[0066] The difference from Example 1 is that in S1, a dry-process positive electrode sheet is provided, including, by mass percentage, LiNi 0.8 Co 0.1 Mn 0.1 02 active material 94%, binder 2.5%, conductive agent 3.5%; the binder material is powdered polytetrafluoroethylene, and the conductive agent is conductive carbon black. The mixed powder is processed in a jet mill for 18 minutes, and the thickness after calendering and compounding is 400μm; in S2, the laser setting parameters and the obtained groove results are shown in Table 1.
[0067] Embodiment 3:
[0068] The difference from Example 1 is that in S1, a dry-process negative electrode sheet is provided, including, by mass percentage, 97% natural graphite active material, 2% binder, and 1% conductive agent; the binder material is powdered polytetrafluoroethylene, and the conductive agent is conductive carbon black. The mixed powder is processed in a jet mill for 16 minutes, and the thickness after calendering and compounding is 300 μm; in S2, the laser setting parameters and the obtained groove results refer to 1.
[0069] Embodiment 4:
[0070] The difference from Example 1 is that in S1, a dry-process negative electrode sheet is provided, including, by mass percentage, 96.5% of hard carbon active material, 2% of binder, and 1.5% of conductive agent; the binder material is powdered polytetrafluoroethylene, and the conductive agent is conductive carbon black. The mixed powder is treated in a jet mill for 20 minutes, and the thickness after calendering and compounding is 350 μm; in S2, the laser setting parameters and the obtained groove results are shown in Table 1.
[0071] Comparative Example 1:
[0072] The difference from Example 1 is that S2 is not performed, and the dry-process positive electrode sheet obtained in S1 is wound into a cylindrical battery cell through S3.
[0073] Comparative Example 2:
[0074] The difference from Example 2 is that S2 is not performed, and the dry-process positive electrode sheet obtained in S1 is wound into a cylindrical battery cell through S3.
[0075] Comparative Example 3:
[0076] The difference from Example 3 is that S2 is not performed, and the dry-process positive electrode sheet obtained in S1 is wound into a cylindrical battery cell through S3.
[0077] Comparative Example 4:
[0078] The difference from Example 4 is that S2 is not performed, and the dry-process positive electrode sheet obtained in S1 is wound into a cylindrical battery cell through S3.
[0079] Comparative Example 5:
[0080] The difference from Example 1 is that in S2, the laser setting parameters are different, so that the shape of the cross section of the groove along the thickness direction is different.
[0081] Please refer to Table 1 for the laser setting parameters and groove structures used in each embodiment and comparative example.
[0082] Table 1. Laser setting parameters and groove results of Examples 1-4 and Comparative Example 5 of the present application
[0083]
[0084] The present application conducted an electrolyte wettability test on the cylindrical cells obtained in Examples 1-4 and Comparative Examples 1-5, and the test method included:
[0085] Step 1: Take the cylindrical battery cells obtained in Examples 1-4 and Comparative Examples 1-5 as electrode materials, ensure that the surface of the electrode materials is clean and free of contaminants, and use electrolyte as the test liquid.
[0086] Step 2: Set up the contact angle meter and ensure that the light source and camera system are working properly.
[0087] Step 3: Use a microsyringe to drop 1 mL of electrolyte on the surface of the electrode material and start timing. The contact angle can be clearly measured. The contact angle gradually decreases through the camera system of the measuring instrument until the electrolyte is completely absorbed by the electrode. The timing ends. This period of time is the electrolyte infiltration time of the electrode. Perform the above steps 5 times to obtain the average value of the electrolyte infiltration time.
[0088] The present application also conducted a charge and discharge rate performance test on the cylindrical cells obtained in Examples 1-4 and Comparative Examples 1-5. The charge and discharge rate performance test method was a constant current charge and discharge test. The specific steps are as follows:
[0089] Step 1: Ensure that the test equipment Arbin model BT-5HC has been calibrated and is in normal working condition, and the test environment maintains a constant temperature of 25℃ and humidity of 30%.
[0090] Step 2: Check that there is no obvious mechanical damage on the appearance of the 3Ah soft-pack battery with a rated capacity. First, charge the battery with a constant current of 15A at a set rate of 5C. When the battery voltage reaches the set cut-off voltage (4.2V), end the charging and let the battery rest for 10 minutes. Then, discharge the battery with a constant current of 15A at a rate of 5C. When the battery voltage reaches the set cut-off voltage (3V), end the discharging and let the battery rest for 10 minutes to stabilize the internal chemical reaction of the battery. Charge the battery with a constant current of 3A at a set rate of 1C. When the battery voltage reaches the set cut-off voltage (4.2V), end the charging and let the battery rest for 10 minutes to stabilize the internal chemical reaction of the battery. Then, discharge the battery with a constant current of 3A at a rate of 1C. When the battery voltage reaches the set cut-off voltage (3V), end the discharging and let the battery rest for 10 minutes. The above test steps are repeated 5 times.
[0091] Step 3: The rate charge and discharge capacity results are calculated by the test equipment based on current and time. The 5C charge capacity is X, the 5C discharge capacity is Y, the 1C charge capacity is M, and the 1C discharge capacity is N. The unit is Ah, the 5C / 1C charge rate performance is X / M, and the 5C / 1C discharge rate performance is Y / N.
[0092] The present application also conducted an initial internal resistance test on the cylindrical cells obtained in Examples 1-4 and Comparative Examples 1-5, using an electrochemical impedance spectroscopy (EIS) initial internal resistance test method. The specific test steps are as follows:
[0093] Step 1: Ensure that the EIS test instrument is working properly, correctly connect the positive and negative poles of the battery, connect the battery to the EIS test instrument, ensure that the connection is good, set the test parameters on the test instrument, the frequency range is 1Hz to 10kHz, and the voltage amplitude is 3-4.2V; start the EIS test, the equipment will automatically apply an AC signal within the set frequency range and measure the impedance of the battery.
[0094] Step 2: After the test is completed, a Nyquist plot of a complex impedance data set is obtained (a plot of the real impedance Z' and the imaginary impedance Z"). The impedance spectrum is analyzed by fitting with the ZSimpWin software. The electrolyte resistance α in the high-frequency region, the interface resistance β in the medium-frequency region, and the diffusion impedance γ in the low-frequency region, the initial internal resistance of the battery cell is α+β+γ, in mΩ.
[0095] Please refer to Table 2 for the above test results.
[0096] Table 2. Electrolyte wettability, charge and discharge rate performance and initial internal resistance test results of Examples 1-4 and Comparative Examples 1-5
[0097] Saturated absorption time min 5C / 1C charge and discharge rate performance Initial internal resistance mΩ Example 1 37 97% / 96% 6.1 Example 2 43 98% / 96% 5.3 Example 3 35 94% / 96% 3.2 Example 4 41 97% / 95% 4.8 Comparative Example 1 53 94% / 92% 9.3 Comparative Example 2 57 92% / 90% 10.2 Comparative Example 3 48 91% / 90% 5.1 Comparative Example 4 58 94% / 91% 7.7 Comparative Example 5 48 91% / 90% 9.7
[0098] Compared with Comparative Examples 1-4, the dry-process electrodes of Examples 1-4 are all provided with inverted triangle grooves, and the saturated liquid absorption time of Examples 1-4 is all shorter and the charge and discharge rate is all higher, indicating that the inverted triangle grooves on the surface of the dry-process membrane of the dry-process electrode can increase the surface area of the electrode, and the increase in surface area can further improve the electrolyte wettability of the electrode, thereby reducing the time required for saturated liquid absorption, thereby reducing the electrolyte standing time of the dry-process electrode during the aging process, which helps to improve the rate performance of the battery. At the same time, compared with Comparative Examples 1-4, the initial internal resistance of the cylindrical battery cells formed by winding in Examples 1-4 is all lower, indicating that the inverted triangle grooves on the surface of the dry-process membrane of the dry-process electrode can reduce the local stress generated when the electrode is wound, thereby reducing the internal resistance and helping to improve the capacity release.
[0099] In the comparative example 5 of the present application, the laser parameters are changed to etch the surface of the dry film with a fixed laser spot diameter. Figure 3 , a groove with a rectangular cross-sectional shape along the thickness direction is obtained. In comparison, the dry-process electrode of Example 1 is provided with an inverted triangular groove. Example 1 has a significantly shorter saturated liquid absorption time, significantly higher rate performance and significantly lower initial internal resistance, which shows that the inverted triangular groove is more conducive to improving the electrolyte wettability of the electrode and has a better effect in alleviating local stress during winding.
[0100] The above implementation modes are only used to illustrate the technical solutions of the present application and are not intended to limit the present application. Although the present application has been described in detail with reference to the above preferred implementation modes, a person skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application.
Claims
1. A dry electrode, comprising a current collector, a first dry membrane and a second dry membrane, wherein the current collector is arranged between the first dry membrane and the second dry membrane, characterized in that: A plurality of grooves are provided on the surface of the first dry membrane sheet facing away from the current collector. When viewed along the width direction of the dry electrode sheet, the groove is triangular and one of the vertices of the groove is arranged toward the current collector. The groove does not penetrate the first dry membrane sheet along the thickness direction of the dry electrode sheet. The plurality of grooves are arranged at intervals along the length direction of the first dry membrane sheet.
2. The dry electrode according to claim 1, characterized in that: Along the length direction, the maximum width of the groove is 55 μm to 80 μm; and the depth of the groove is 20 μm to 50 μm.
3. The dry electrode according to claim 1, characterized in that: The groove does not penetrate the first dry film along the width direction of the dry electrode, and along the width direction, the distance between the edge of the groove and the edge of the first dry film is 1 mm to 3 mm.
4. A secondary battery, comprising an electrode assembly, wherein the electrode assembly is a wound structure and comprises a dry electrode sheet, wherein the dry electrode sheet comprises a current collector, a first dry membrane sheet and a second dry membrane sheet, wherein the current collector is disposed between the first dry membrane sheet and the second dry membrane sheet, wherein: The first dry film is arranged toward the winding center axis of the electrode assembly, and a plurality of gaps are provided on the surface of the first dry film facing away from the current collector, the gaps do not penetrate the first dry film along the thickness direction of the dry electrode sheet, and the plurality of gaps are arranged at intervals along the length direction of the first dry film.
5. The secondary battery according to claim 4, characterized in that: The slit includes a first end and a second end that are arranged opposite to each other, the first end is closer to the winding center axis than the second end, and the spacing between the second ends of two adjacent slits is 1 mm to 2 mm.
6. A method for preparing a dry electrode, characterized in that: include: Providing a current collector, and arranging a first dry film and a second dry film on two surfaces of the current collector respectively; Using a laser to etch a plurality of grooves on the surface of the first dry film away from the current collector to obtain the dry electrode; Among them, when observed along the width direction of the dry electrode, the groove is triangular and one of the vertices of the groove is set toward the current collector, the groove does not penetrate the first dry membrane along the thickness direction of the dry electrode, and the multiple grooves are arranged at intervals along the length direction of the first dry membrane.
7. The preparation method according to claim 6, characterized in that: The etching comprises: Set the spot diameter of the laser to d1, and perform etching once along the laser scanning path; Setting the spot diameter of the laser to d2, and performing secondary etching along the laser scanning path; Setting the spot diameter of the laser to d3, and performing etching three times along the laser scanning path; Among them, d1>d2>d3.
8. The preparation method according to claim 7, characterized in that: The spot diameter d1 of the laser is 50 μm to 60 μm, and d3 is 20 μm to 35 μm.
9. The preparation method according to claim 7, characterized in that: The power of the laser is 10W to 70W, or the pulse frequency of the laser is 50 kHz to 60 kHz.
10. The preparation method according to claim 7, characterized in that: The distance between any two adjacent laser scanning paths is 1 mm to 2 mm.
Citation Information
Cited By
Battery pole piece suitable for large cylindrical battery and large cylindrical battery
CN121812466A