Preparation of S-rich porous zinc-based MOF flexible film and lithium battery performance regulation and control
By preparing S-rich porous zinc-based MOF flexible films, the problems of low specific capacity, poor rate performance, and stability of lithium-ion batteries have been solved, realizing a lithium-ion battery separator material with high conductivity and high safety, and improving the electrochemical stability and safety of the battery.
Patent Information
- Application Number
- CN202411056455.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-02
AI Technical Summary
Existing lithium-ion batteries suffer from low specific capacity, unsatisfactory rate performance, and poor stability, especially when using solid electrolytes.
A method for preparing S-rich porous zinc-based MOF flexible films was adopted. A metal-organic framework material with a channel structure containing negative electrons was synthesized by hydrothermal method and blended with lithium salt and polymer to form a composite polymer film for use as a separator material in lithium-ion batteries.
It improves the electrochemical stability and rate performance of lithium-ion batteries, reduces the risk of internal short circuits, enhances safety performance, and exhibits good cycle stability and high ionic conductivity at different current densities.
Smart Images

Figure CN118970365A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field related to lithium-ion solid-state batteries, and specifically relates to a method for preparing a S-rich porous zinc-based MOF flexible film, and also relates to performance regulation of lithium-ion batteries based on the S-rich porous zinc-based MOF flexible film. Background Art
[0002] Lithium-ion batteries are widely regarded as the most efficient, environmentally friendly and clean energy storage devices and have achieved great success in commercialization. With the widespread application of lithium-ion batteries in the field of electric vehicles, safety issues have become increasingly prominent, especially the fire risk caused by flammable organic liquid electrolytes. Compared with lithium-ion batteries using flammable liquid organic electrolytes, solid-state lithium metal batteries using solid electrolytes are considered to be a promising strategy, but solid electrolytes currently face problems including low ionic conductivity, large interface resistance and poor contact with electrodes, which limit the energy density, cycle stability and safety of the battery.
[0003] Solid polymer electrolytes have low ionic conductivity and poor stability. Although inorganic electrolytes have high conductivity, they have large interfacial resistance with electrodes and cannot withstand large strains or pose safety risks. The development of new composite electrolyte diaphragm materials is expected to solve the above problems. An effective way is to add functional materials to polymer-based diaphragms. MOF is a functional material with a periodic porous structure. It has the characteristics of high specific surface area, adjustable chemical properties and uniform morphology. Using MOF's low ion transport resistance and uniform pores as a diaphragm modification material for lithium batteries and as a polymer-based ion conduction material has become a very promising method. However, from the current technology, there are still problems such as low conductivity and poor stability of polymer electrolytes.
[0004] For example, in the paper "Metal organic framework modified poly (vinylidenefluoride-co-hexanopropylen) separator membranes to improve lithium-ion battery capacity filling" published in "Chemical Engineering Journal" in April 2022, the authors selected three MOFs with similar surface areas and topological structures to modify the PVDF-HFP membrane, using the porosity of MOF to improve battery performance, and conducted a series of characterization and electrochemical performance tests to explore the effects of different MOFs on membrane performance. Due to the differences in MOF particle size and pore structure, there are still problems such as low battery specific capacity, poor stability and low rate performance. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a S-rich porous zinc-based MOF flexible film, in order to solve the problems of low battery specific capacity, unsatisfactory rate performance and poor stability existing in the prior art.
[0006] To achieve the above object, the technical solution adopted by the present invention is a method for preparing a S-rich porous zinc-based MOF flexible film, comprising the following steps:
[0007] Step 1: Weigh 5-methyl-1H tetrazole and dissolve it in N,N-dimethylacetamide to obtain solution A; weigh 2,5-thiophene dicarboxylic acid and dissolve it in methanol to obtain solution B; after ultrasonicating solution A and solution B for 10-15 minutes, slowly pour solution A into solution B, and then stir to obtain solution C; the molar ratio of 5-methyl-1H tetrazole to 2,5-thiophene dicarboxylic acid is 4:1;
[0008] Step 2: weigh the template agent pyrazine, add it to solution C and stir to obtain solution D, wherein the molar ratio of pyrazine to 2,5-thiophenedicarboxylic acid is 3:2;
[0009] Step 3: Add a few drops of tetramethylammonium hydroxide to solution D to adjust the pH, and stir to obtain a mixed solution E;
[0010] Step 4: Add zinc salt to the mixed solution E, the molar ratio of 2,5-thiophenedicarboxylic acid to zinc salt is 1:2, and ultrasonicate for 10-15 minutes; react in an oven, cool to room temperature, wash with N,N-dimethylacetamide several times, and dry to obtain light yellow crystals F, which are ground to obtain precursor G;
[0011] Step 5: Precursor G is used as a filler and mixed with lithium salt and polymer in N-methyl-2-pyrrolidone, with a mass ratio of G: polymer: salt being 1:8:1. Stir at room temperature for 40-50 hours to obtain a milky white viscous liquid H.
[0012] Step 6: The viscous liquid H is formed into a film on a glass plate, and a S-rich porous zinc-based MOF flexible film is obtained after vacuum drying.
[0013] Furthermore, in the above step 4, the temperature of the oven is set at 100-140° C., and the reaction time is 48-72 hours.
[0014] Furthermore, in the above step 4, the zinc salt is zinc nitrate hexahydrate, zinc acetate or zinc chloride.
[0015] Furthermore, in the above step 5, the polymer is any one of polyethylene oxide (PEO), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polyacrylonitrile (PAN).
[0016] Furthermore, in the above step 6, the vacuum drying temperature is 40-70° C., and the drying time is 10-20 hours.
[0017] Furthermore, in the above step 6, the viscous liquid H is first vacuum filtered for 15-40 minutes to remove bubbles before film formation.
[0018] Furthermore, in the above step 6, the film is formed by scraping the viscous liquid H onto the glass plate using a 1000 micron scraper.
[0019] Furthermore, in the above step 6, the film is formed by pouring the viscous liquid H onto the glass plate and rotating it to make it naturally level.
[0020] Furthermore, the S-rich porous zinc-based MOF flexible film prepared by the above preparation method.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention successfully synthesizes a new metal-organic framework material with a large pore structure centered on zinc metal by precise control through the addition of a template agent and a pH regulator. This crystal forms a pore structure with negative electrons through tetrazole and carboxylic acid ligands. Because the sulfur atoms in the pores are lithium-philic groups, the precursor, the S-rich porous zinc-based metal-organic framework material, is incorporated into the polymer base material as an electrolyte filler to form an ultra-thin polymer flexible film that can be used as an excellent ion conductor.
[0023] (2) The present invention introduces longer carboxylic acid ligands, which increases the porosity and window size of the crystalline material, and together constructs a uniform and fast ion transmission path. The sulfur in the pores will adsorb metal cations and promote the conduction of metal cations, allowing more lithium ions to be solvated with less restriction, providing a fast channel for the transmission of lithium ions, thereby preventing the formation of lithium dendrites that pierce the diaphragm during the cycle of the lithium-ion battery, effectively enhancing the electrochemical stability of the lithium battery, demonstrating excellent cycle stability, and also showing good rate performance at different current densities.
[0024] (3) In the preparation process of the present invention, the S-rich porous zinc-based metal organic framework material is dispersed in a polymer substrate to prepare a flexible film. This effective combination method not only retains the porous crystalline structure, but also promotes the movement of the chain segments and the contact at the interface. Therefore, the stable interface provided by the MOF / polymer composite separator helps to prevent adverse reactions between the electrolyte and the electrode, thereby improving the electrochemical stability of the battery. The assembled lithium iron phosphate (LFP) battery exhibits low electrochemical impedance characteristics. The specific capacity of the battery at a current of 0.1C is 140mAhg -1, the capacity retention rate is close to 100%, which reduces the risk of internal short circuit in the battery and also has higher safety performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the preparation process of a S-rich porous zinc-based MOF flexible film according to the present invention;
[0026] Figure 2 The electrochemical impedance spectroscopy (EIS) of a lithium-ion battery assembled from the S-rich porous zinc-based MOF flexible film prepared in Example 1 of the present invention;
[0027] Figure 3 This is the Nyquist plot at different temperatures of the S-rich porous zinc-based MOF flexible film assembled with a stainless steel symmetric battery test prepared in Example 1 of the present invention;
[0028] Figure 4 It is an Arrhenius curve obtained by testing the ionic conductivity of a stainless steel symmetric battery assembled with a S-rich porous zinc-based MOF flexible film prepared in Example 1 of the present invention at different temperatures;
[0029] Figure 5 This is a relationship diagram between the efficiency and specific capacity of the S-rich porous zinc-based MOF flexible film assembled lithium-ion battery prepared in Example 1 of the present invention at a rated capacity of 0.1C after 100 cycles;
[0030] Figure 6 This is a rate performance diagram of a lithium-ion battery assembled with a S-rich porous zinc-based MOF flexible film prepared in Example 1 of the present invention at different currents. DETAILED DESCRIPTION
[0031] The present invention will be further described below in conjunction with specific embodiments and drawings.
[0032] The preparation idea of the present invention is shown in Figure 1 Tetrazolyl, carboxyl and zinc ions were coordinated by a hydrothermal method, with pyrazine as a template and tetramethylammonium hydroxide as a pH regulator, to obtain a new S-rich porous zinc-based metal-organic framework material with special pores containing negative electrons. It was further blended with lithium salts and polymers to obtain a metal-organic framework composite polymer viscous liquid, which was then scraped onto a glass plate and allowed to stand to obtain a S-rich porous zinc-based MOF flexible film.
[0033] Example 1, see Figure 1 , a method for preparing a S-rich porous zinc-based MOF flexible film, comprising the following steps:
[0034] Step 1: Weigh 5-methyl-1H tetrazole (1.2 mmol, 0.1 g) and dissolve it in 3 mL of N, N-dimethylacetamide to obtain solution A; weigh 2,5-thiophenedicarboxylic acid (0.29 mmol, 0.0499 g) and dissolve it in 3 mL of methanol to obtain solution B; after ultrasonicating solution A and solution B for 15 minutes, slowly pour solution A into solution B, and then stir them to obtain solution C;
[0035] Step 2: Weigh 0.035 g of pyrazine, add it to solution C and stir to obtain solution D;
[0036] Step 3: Add 1 drop of tetramethylammonium hydroxide to solution D to adjust the pH, and stir to obtain a mixed solution E.
[0037] Step 4: Add zinc nitrate hexahydrate (0.54 mmol, 0.16 g) to the mixed solution E, sonicate for 15 minutes, transfer to a vial, react in an oven at 120°C for 48 hours, and then cool naturally. Wash three times with N,N-dimethylacetamide, and dry to obtain light yellow crystals F, which are ground for 30 minutes to obtain precursor G;
[0038] Step 5: Take 0.125 g of precursor G as a filler, mix it with 1 g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and 0.125 g of lithium bis(trifluoromethylsulfonyl)imide in 7 mL of N-methyl-2-pyrrolidone, and stir at room temperature for 48 hours to obtain a milky white viscous liquid H.
[0039] Step 6: First, vacuum filter the milky white viscous liquid H for 30 minutes to remove bubbles, then use a 1000-micron scraper to scrape the viscous liquid H on a glass plate to form a thin film, and then dry it under vacuum conditions to finally obtain a solidified S-rich porous zinc-based MOF flexible film.
[0040] Embodiment 2, a method for preparing a S-rich porous zinc-based MOF flexible film, comprising the following steps:
[0041] Step 1: Weigh 5-methyl-1H tetrazole (1.2 mmol, 0.1 g) and dissolve it in 4 mL of N, N-dimethylacetamide to obtain solution A; weigh 2,5-thiophenedicarboxylic acid (0.29 mmol, 0.0499 g) and dissolve it in 4 mL of methanol to obtain solution B; after ultrasonicating solution A and solution B for 10 minutes, slowly pour solution A into solution B, and then stir them to obtain solution C;
[0042] Step 2: Weigh 0.035 g of pyrazine, add it to solution C and stir to obtain solution D;
[0043] Step 3: Add 2 drops of tetramethylammonium hydroxide to solution D to adjust the pH, and stir to obtain a mixed solution E.
[0044] Step 4: Add zinc nitrate hexahydrate (0.54 mmol, 0.16 g) to the mixed solution E, sonicate for 15 minutes, transfer to a small vial, react in an oven at 120°C for 50 hours, and then cool naturally. Wash twice with N,N-dimethylacetamide, and dry to obtain light yellow crystals F, which are ground for 30 minutes to obtain precursor G;
[0045] Step 5: 0.125 g of precursor G was used as a filler, mixed with 1 g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and 0.125 g of lithium bis(trifluoromethylsulfonyl)imide in 7 mL of N-methyl-2-pyrrolidone, and stirred at room temperature for 40 hours to obtain a milky white viscous liquid H.
[0046] Step 6: Pour the milky white viscous liquid H onto a glass plate and rotate it to make it naturally level to form a thin film. After drying under vacuum conditions, a solidified S-rich porous zinc-based MOF flexible film material is finally obtained.
[0047] Embodiment 3, a method for preparing a S-rich porous zinc-based MOF flexible film, comprising the following steps:
[0048] Step 1: Weigh 5-methyl-1H tetrazole (1.2 mmol, 0.1 g) and dissolve it in 5 mL of N, N-dimethylacetamide to obtain solution A; weigh 2,5-thiophenedicarboxylic acid (0.29 mmol, 0.0499 g) and dissolve it in 5 mL of methanol to obtain solution B; after ultrasonicating solution A and solution B for 15 minutes, slowly pour solution A into solution B, and then stir them to obtain solution C;
[0049] Step 2: Weigh 0.035 g of pyrazine, add it to solution C and stir to obtain solution D;
[0050] Step 3: Add 1 drop of tetramethylammonium hydroxide to solution D to adjust the pH, and stir to obtain a mixed solution E.
[0051] Step 4: Add zinc nitrate hexahydrate (0.54 mmol, 0.16 g) to the mixed solution E, sonicate for 10 minutes, transfer to a small bottle, react in an oven at 110°C for 55 hours, and then cool naturally. Wash with N,N-dimethylacetamide four times, dry, and obtain light yellow crystals F, which are ground for 40 minutes to obtain precursor G;
[0052] Step 5: 0.125 g of precursor G was used as a filler, mixed with 1 g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and 0.125 g of lithium bis(trifluoromethylsulfonyl)imide in 7 mL of N-methyl-2-pyrrolidone, and stirred at room temperature for 50 hours to obtain a milky white viscous liquid H.
[0053] Step 6: Apply the viscous liquid H on a glass plate to form a thin film, and then dry it under vacuum conditions to finally obtain a solidified S-rich porous zinc-based MOF flexible thin film material.
[0054] Example 4, a method for preparing a S-rich porous zinc-based MOF flexible film, comprising the following steps:
[0055] Step 1: Weigh 5-methyl-1H tetrazole (1.2 mmol, 0.1 g) and dissolve it in 6 mL of N, N-dimethylacetamide to obtain solution A; weigh 2,5-thiophenedicarboxylic acid (0.29 mmol, 0.0499 g) and dissolve it in 6 mL of methanol to obtain solution B; after ultrasonicating solution A and solution B for 13 minutes, slowly pour solution A into solution B, and then stir them to obtain solution C;
[0056] Step 2: Weigh 0.035 g of pyrazine, add it to solution C and stir to obtain solution D;
[0057] Step 3: Add 2 drops of tetramethylammonium hydroxide to solution D to adjust the pH, and stir to obtain a mixed solution E.
[0058] Step 4: Add zinc nitrate hexahydrate (0.54 mmol, 0.16 g) to the mixed solution E, sonicate for 10 minutes, transfer to a vial, react in an oven at 130°C for 48 hours, and then cool naturally. Wash three times with N,N-dimethylacetamide, and dry to obtain light yellow crystals F, which are ground for 30 minutes to obtain precursor G;
[0059] Step 5: 0.125 g of precursor G was used as a filler, mixed with 1 g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and 0.125 g of lithium bis(trifluoromethylsulfonyl)imide in 6 mL of N-methyl-2-pyrrolidone, and stirred at room temperature for 72 hours to obtain a milky white viscous liquid H.
[0060] Step 6: Apply the viscous liquid H on a glass plate to form a thin film, and then dry it under vacuum conditions to finally obtain a solidified S-rich porous zinc-based MOF flexible thin film material.
[0061] The S-rich porous zinc-based MOF flexible film obtained in Examples 1-4 was cut into circular sheets with a diameter of 19 mm, and these circular sheets were used as diaphragms I. The diaphragm I was respectively assembled with lithium iron phosphate positive electrode material and lithium metal negative electrode in a glove box with a water oxygen value of less than 0.01 ppm and filled with argon gas, and the shrapnel and gasket were assembled into lithium ion batteries, and the rate performance (0.1C, 0.2C, 0.5C, 1C, 2C), ionic conductivity, and cycle performance (operating voltage of 2.5V-4V) were tested at different currents.
[0062] Take embodiment 1 as the best embodiment, as Figure 2 As shown, the lithium-ion battery of the S-rich porous zinc-based MOF flexible film prepared by the present invention is subjected to electrochemical impedance spectroscopy (EIS) before cycling under an electrochemical workstation, and the frequency is 0.01-100000 Hz. From the smaller semicircle in the figure, it can be seen that the charge transfer resistance before cycling is smaller, indicating that the S-rich porous zinc-based MOF flexible film promotes faster charge transfer.
[0063] like Figure 3 As shown in the figure, in the ionic conductivity test, the electrochemical impedance was tested in the temperature range of 25 to 85 °C by the AC impedance method. It can be seen from the figure that the conductivity of the S-rich porous zinc-based MOF flexible film gradually increases with the increase of temperature, and the lithium ion conductivity is 4.88×10 -4 S cm -1 , 1.21×10 at 85℃ -3 S cm -1 , illustrating that the S-rich porous Zn-based MOF flexible film has high ionic conductivity.
[0064] like Figure 4 As shown, it can be seen that the conductivity shows a good linear relationship with the change of temperature. The activation energy of ion transition conduction in the S-rich porous zinc-based MOF flexible film is calculated to be 0.136 eV by the Arrhenius formula, which shows that the S-rich porous zinc-based MOF flexible film is conducive to the desolvation and ion transport of lithium ions.
[0065] like Figure 5 As shown in the figure, after 100 cycles at a current density of 0.1C, the S-rich porous zinc-based MOF flexible film has a specific capacity of 140 mAh g –1 , the capacity retention rate is close to 100%.
[0066] like Figure 6 As shown in the figure, the S-rich porous zinc-based MOF flexible film is cycled 10 times at different current densities of 0.1C, 0.2C, 0.5C, 1C, and 2C. The corresponding charge and discharge specific capacities at different current densities are 148, 145, 139, 130, and 112 mAh g –1 , and the efficiency is close to 100%. This shows that the composite flexible film can maintain a high energy output and absorption rate at a high rate without losing too much energy due to the high rate.
[0067] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a S-rich porous zinc-based MOF flexible film, characterized in that: The following steps are involved: Step 1: Weigh 5-methyl-1H tetrazole and dissolve it in N,N-dimethylacetamide to obtain solution A; weigh 2,5-thiophene dicarboxylic acid and dissolve it in methanol to obtain solution B; after ultrasonicating solution A and solution B for 10-15 minutes, slowly pour solution A into solution B, and then stir to obtain solution C; the molar ratio of 5-methyl-1H tetrazole to 2,5-thiophene dicarboxylic acid is 4:1; Step 2: weigh the template agent pyrazine, add it to solution C and stir to obtain solution D, wherein the molar ratio of pyrazine to 2,5-thiophenedicarboxylic acid is 3:2; Step 3: Add a few drops of tetramethylammonium hydroxide to solution D to adjust the pH, and stir to obtain a mixed solution E; Step 4: Add zinc salt to the mixed solution E, the molar ratio of 2,5-thiophenedicarboxylic acid to zinc salt is 1:2, and ultrasonicate for 10-15 minutes; react in an oven, cool to room temperature, wash with N,N-dimethylacetamide several times, and dry to obtain light yellow crystals F, which are ground to obtain precursor G; Step 5: Precursor G is used as a filler and mixed with lithium salt and polymer in N-methyl-2-pyrrolidone, with a mass ratio of G: polymer: salt being 1:8:1, and stirred at room temperature for 40-50 hours to obtain a milky white viscous liquid H; Step 6: Form a film of the viscous liquid H on a glass plate, and obtain a S-rich porous zinc-based MOF flexible film after vacuum drying.
2. The method for preparing a S-rich porous zinc-based MOF flexible film according to claim 1, characterized in that: In step 4, the temperature of the oven is set at 100-140° C., and the reaction time is 48-72 hours.
3. The method for preparing a S-rich porous zinc-based MOF flexible film according to claim 2, characterized in that: In step 4, the zinc salt is zinc nitrate hexahydrate, zinc acetate or zinc chloride.
4. The method for preparing a S-rich porous zinc-based MOF flexible film according to claim 3, characterized in that: In the step 5, the polymer is any one of polyethylene oxide (PEO), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polyacrylonitrile (PAN).
5. The method for preparing a S-rich porous zinc-based MOF flexible film according to claim 4, characterized in that: In step 6, the vacuum drying temperature is 40-70° C., and the drying time is 10-20 hours.
6. The method for preparing a S-rich porous zinc-based MOF flexible film according to claim 5, characterized in that: In the step 6, the viscous liquid H is first vacuum filtered for 15-40 minutes to remove bubbles, and then the membrane is formed.
7. The method for preparing a S-rich porous zinc-based MOF flexible film according to claim 6, characterized in that: In step 6, the film is formed by coating the viscous liquid H on a glass plate using a 1000 micron scraper.
8. The method for preparing a S-rich porous zinc-based MOF flexible film according to claim 6, characterized in that: In step 6, the film is formed by pouring the viscous liquid H onto the glass plate and rotating it to make it naturally level.
9. The S-rich porous zinc-based MOF flexible film obtained according to the preparation method of claim 1.
Citation Information
Patent Citations
Method for predicting performance of metal organic framework material for catalyzing carbon dioxide
CN113689918A
Super-macroporous metal organic framework lithium sodium ion conductor film and preparation method thereof
CN117924756A
Composition comprising insulin-like growth factor 2 inhibitor for preventing or treating of chronic pulmonary disease
KR1020200088559A
Conductivity enhancement of mofs via development of mofpolymer composite material