High-frequency microwave printed circuit board with high heat dissipation performance and preparation method thereof
By preparing low-mediated heat-conducting microwave ceramic powder and surface-modified polytetrafluoroethylene powder, the problem of uneven dispersion of ceramic fillers in polytetrafluoroethylene matrix is solved, and the thermal conductivity of high-frequency microwave printed circuit boards is improved and Dielectric properties enhance signal transmission and mechanical strength.
Patent Information
- Application Number
- CN202411449811.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-10-17
AI Technical Summary
The material mismatch between the ceramic filler and the polytetrafluorovinyl matrix in high-frequency microwave printed circuit boards makes it difficult to disperse the ceramic filler evenly in the matrix, affecting the dielectric and thermal conductivity of the material.
By preparing low-mediated heat microwave ceramic powder, the hydrothermal reaction of magnesium acetate and aqueous ammonia solution is used to generate nanocomposite powder, and the surface modification of the polytetrafluoroethylene powder is combined with natural surface treatment agent extracted from oak bark is enhanced. The compatibility of ceramic powder and polytetrafluoroethylene forms a uniform composite material.
It improves the thermal conductivity and dielectric properties of high-frequency microwave printed circuit boards, reduces dielectric losses, enhances signal transmission performance and mechanical strength, and ensures the high-frequency stability and reliability of the material.
Smart Images

Figure CN118973157A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of printed circuit boards, and in particular to a high-frequency microwave printed circuit board with high heat dissipation performance and a preparation method thereof. Background Art
[0002] With the development of modern electronic technology, especially in the fields of communication, radar, satellite, etc., high-frequency microwave circuits are used more and more widely. High-frequency microwave printed circuit boards (PCBs) are an important part of high-frequency circuits. They require excellent dielectric properties and heat dissipation properties to ensure signal stability and circuit reliability at high frequencies. For this type of circuit board, polytetrafluoroethylene (PTFE) has become one of the ideal substrates due to its low dielectric constant, low loss factor and high chemical stability.
[0003] However, PTFE has poor thermal conductivity (about 0.25W / m·K), which can easily cause overheating in high-frequency and high-power circuits, affecting device performance and life. Therefore, it is usually necessary to add ceramic powders with high thermal conductivity to PTFE, such as aluminum oxide (A12O3), boron nitride (BN), or silicon carbide (SiC), to improve the thermal conductivity of the circuit board.
[0004] Although the addition of ceramic fillers can effectively improve the thermal conductivity of composite materials, there is a mismatch between the materials of PTFE and ceramic fillers when preparing high-frequency microwave printed circuit boards. For example, the chemical compatibility between ceramic materials and PTFE is poor. There are obvious differences in the physical and chemical structures of the two, and it is difficult to form a stable interface through physical adsorption or chemical bonding. As a result of this poor compatibility, the ceramic fillers are difficult to disperse evenly in the PTFE matrix, and even aggregation occurs, forming an unevenly dispersed composite material, which seriously affects the dielectric and thermal conductivity of the material. Summary of the invention
[0005] In order to solve the above technical defects, the present invention has developed a high-frequency microwave printed circuit board with good compatibility between composite fillers, low material dielectric constant, low dielectric loss and high heat dissipation performance and a preparation method thereof.
[0006] A method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance comprises the following steps: S1: Preparation of low dielectric microwave ceramic powder Mixing magnesium acetate and deionized water to obtain a magnesium acetate solution, then adding the magnesium acetate solution dropwise into an ammonia solution, stirring to obtain a precursor solution I, preparing a BaCl2 solution and placing it in an ice water bath, adding a titanium tetrachloride solution dropwise, stirring to obtain a precursor solution II, first heating the precursor solution I, then adding the precursor solution II and urea to heat, adding nano boron nitride midway to continue heating, filtering to obtain a precipitate, washing and drying to obtain a nano composite powder, mixing Y2(C2O4)3·10H2O, CuO and H2BO3 and ball milling to obtain a mixed powder, mixing the nano composite powder and the mixed powder, sintering and ball milling, drying and sieving to obtain a low-medium thermal microwave ceramic powder; S2: Modification of high-frequency microwave substrate materials The oak bark is dried and crushed, mixed with deionized water, and subjected to ultrasonic treatment at elevated temperature, filtered to obtain an extract, the extract is rotary evaporated to obtain a natural surface treatment agent, polytetrafluoroethylene powder is immersed in the natural surface treatment agent and heated, and washed and dried after natural cooling to obtain pretreated polytetrafluoroethylene powder, low-medium thermal microwave ceramic powder is mixed with anhydrous ethanol and subjected to ultrasonic treatment to obtain a suspension, and then stearic acid is added, and ultrasonic treatment is continued, followed by condensation reflux, and drying to obtain surface-modified low-medium thermal microwave ceramic powder; S3: Composite pressing of microwave printed circuit boards The pretreated polytetrafluoroethylene powder, silane coupling agent and deionized water are uniformly mixed to obtain a pretreated polytetrafluoroethylene dispersion emulsion; the pretreated polytetrafluoroethylene dispersion emulsion, surface modified low-medium thermal conductivity microwave ceramic powder, thermoplastic polyimide and plasticizer are mixed and stirred to obtain a mixed glue solution; ethanol is added and stirred continuously and filtered to obtain a colloidal solid; a powdered solid is obtained after drying; the powdered solid is hot pressed to obtain a composite substrate; an electrolytic copper foil is pressed on the upper and lower sides of the composite substrate and then hot pressed to obtain a high-frequency microwave thermal conductive single-layer copper-clad substrate; the high-frequency microwave thermal conductive single-layer copper-clad substrate is taken and drilled, deburred, chemically deposited copper, electroplated copper in the hole, attached a positive film dry film, exposed and developed, electroplated, etched and de-dried to obtain a high-frequency microwave thermal conductive single-layer circuit board; the high-frequency microwave thermal conductive single-layer circuit board is loaded into a hot press in the order of high-frequency microwave thermal conductive single-layer circuit board-high-frequency microwave thermal conductive single-layer copper-clad substrate-high-frequency microwave thermal conductive single-layer circuit board for hot pressing to obtain a high-frequency microwave printed circuit board with high heat dissipation performance.
[0007] Furthermore, step S1 of preparing low-dielectric microwave ceramic powder comprises the following steps: S1.1: Mix magnesium acetate and deionized water in a mass ratio of 1: (25-30) and stir for 10-15 minutes to obtain a magnesium acetate solution, take 10-12 parts by weight of an ammonia solution and place it in a container, then dropwise add 3-4 parts by weight of the magnesium acetate solution, and when the magnesium acetate solution is completely added, stir at a speed of 450-500rpm using a magnetic stirrer for 20-30 minutes to obtain a precursor solution I, mix BaCl2·2H2O and deionized water in a mass ratio of 1: (20-25) and place it in a container, then add 4-6wt% of polyvinyl pyrrolidone, stir for 15-20 minutes to obtain a BaCl2 solution, take 6-8 parts by weight of the BaCl2 solution and place it in an ice water bath, then dropwise add 2-3 parts by weight of a titanium tetrachloride solution with a mass fraction of 15-20%, and stir at a speed of 300-350rpm for 20-25 minutes to obtain a precursor solution II; S1.2: Transfer the precursor solution I prepared in step S1.1 to a hydrothermal reactor, heat it at 150-180°C for 12-16 hours, then add the precursor solution II prepared in step S1.1 and 0.5-1 parts by weight of urea, stir for 10-20 minutes, continue to heat to 200-220°C, keep warm for 8-10 hours, add 1-1.5 parts by weight of nano boron nitride, continue heating for 6-8 hours, filter to obtain a precipitate, wash it with anhydrous ethanol for 8-10 minutes, rinse it with deionized water 2-3 times, and then place it in a vacuum drying oven at 70-80°C for 6-8 hours to obtain a nano composite powder; S1.3: Y2(C2O4)3·10H2O, CuO and H2BO3 are mixed in a mass ratio of 1: (0.3-0.4): (0.3-0.4) and placed in a planetary ball mill, 10-15 times the mass of zirconia balls and 2-3 times the volume of anhydrous ethanol are added, and the mixture is ball-milled at a speed of 400-500rpm for 6-8 hours, and the zirconia balls are separated to obtain a mixed powder. The nano-composite powder and the mixed powder are evenly mixed in a mass ratio of 1: (0.1-0.2), and then placed in a muffle furnace and heated to 500-600℃ at a heating rate of 3-5℃ / min and calcined for 4-5 hours, and then heated to 1200-1250℃ and calcined for 2-3 hours. After cooling to room temperature, the mixture is ball-milled at a speed of 500-600rpm for 5-6 hours. After drying, the mixture is sieved through an 80-100 mesh sieve to obtain a low-medium thermal microwave ceramic powder.
[0008] Furthermore, step S2 of modifying the high-frequency microwave substrate raw material comprises the following steps: S2.1: Dry the oak bark at 40-60°C to control the moisture content to 5-10%, then grind it with a grinder, pass it through a 40-50 mesh sieve to obtain oak powder, mix the oak powder with deionized water at a solid-liquid ratio of 1: (20-25) and place it in an ultrasonic constant temperature water bath, adjust the temperature to 80-90°C, the ultrasonic frequency to 25-30kHz, and perform ultrasonic treatment for 30-40 minutes, then filter through a vacuum filter to remove solid impurities to obtain an extract, and perform rotary evaporation on the extract at 45-50°C to obtain a natural surface treatment agent; S2.2: Soak the polytetrafluoroethylene powder in the natural surface treatment agent obtained in step S2.1, heat it to 180-200°C, keep it warm for 20-30 minutes, then cool it naturally, filter it out after it cools to room temperature, wash it with deionized water 2-3 times, and then dry it at 75-80°C to obtain pretreated polytetrafluoroethylene powder; S2.3: Place 1-2 parts by weight of low-medium thermal conductivity microwave ceramic powder in 100-120 parts by weight of anhydrous ethanol and ultrasonically treat it for 25-30 minutes at an ultrasonic frequency of 20-30kHz to obtain a suspension, then add 2-3wt% of stearic acid, continue ultrasonic treatment at the same frequency for 10-15 minutes, condense and reflux at 60-65°C for 2-3 hours, and finally vacuum dry at 80-85°C for 4-6 hours to obtain surface-modified low-medium thermal conductivity microwave ceramic powder.
[0009] Furthermore, step S3 of composite pressing of the microwave printed circuit board comprises the following steps: S3.1: pretreated polytetrafluoroethylene powder, silane coupling agent and deionized water are uniformly mixed in a mass ratio of 1: (0.06-0.08): (2-3) to obtain a pretreated polytetrafluoroethylene dispersion emulsion, 10-12 parts by weight of the pretreated polytetrafluoroethylene dispersion emulsion, 3-4 parts by weight of surface-modified low-mediation thermal microwave ceramic powder, 0.4-0.6 parts by weight of thermoplastic polyimide and 0.06-0.08 parts by weight of plasticizer are mixed and stirred at a speed of 1000-1200 rpm for 1-1.5 hours to obtain a mixed glue solution, and then ethanol is added to the mixed glue solution, the stirring speed is adjusted to 150-200 rpm, and the stirring is continued for 10-15 minutes and then filtered to obtain a colloidal solid, and the colloidal solid is placed in a vacuum dryer at 100-110°C to obtain a powdered solid; S3.2: Spread the powdered solid in a mold, then place the mold in a hot press, press it at a pressure of 40-50 MPa at room temperature, and then heat it at 350-400°C for 1-2 hours to obtain a composite substrate, and press a sheet of electrolytic copper foil on the upper and lower sides of the composite substrate, and then press it at a temperature of 380-400°C and a pressure of 10-15 MPa for 20-25 minutes, and naturally cool it to below 60°C to obtain a high-frequency microwave thermal conductive single-layer copper-clad substrate; S3.3: Take a high-frequency microwave thermal conductive single-layer copper-clad substrate, use a PCB CNC drilling machine to complete the drilling process of through holes and blind holes, then remove the edge burrs of the hole mouth, first chemically deposit copper in the hole, and then electroplate copper in the hole on the chemically deposited copper layer. After drying, paste positive film, expose and develop, electroplate the circuit, etch the circuit and de-dry the film on the copper surface in sequence to obtain a high-frequency microwave thermal conductive single-layer circuit board, and load them into a hot press in the order of high-frequency microwave thermal conductive single-layer circuit board-high-frequency microwave thermal conductive single-layer copper-clad substrate-high-frequency microwave thermal conductive single-layer circuit board, press at 320-350℃ and a pressure of 3-5MPa for 15-25 minutes to obtain a high-frequency microwave printed circuit board with high heat dissipation performance.
[0010] Furthermore, the concentration of the aqueous ammonia solution in step S1.1 is 25-30%.
[0011] Furthermore, in step S1.3, the particle size of the zirconium oxide balls is 0.1-1 mm.
[0012] Furthermore, the volume of the extract after rotary evaporation in step S2.1 is 1 / 5-1 / 4 of the original volume.
[0013] Furthermore, the silane coupling agent in step S3.1 is vinyl triethoxy silane, and the plasticizer is perfluoroalkoxy.
[0014] Furthermore, the thickness of the electrolytic copper foil in step S3.2 is 20-25 μm.
[0015] A high-frequency microwave printed circuit board with high heat dissipation performance is prepared by the above-mentioned preparation method of a high-frequency microwave printed circuit board with high heat dissipation performance.
[0016] The beneficial effects are as follows: 1. The present invention prepares a magnesium acetate solution and drips it into an ammonia solution and stirs it evenly to obtain a precursor solution I, then drips titanium tetrachloride into a BaCl2 solution under an ice water bath and stirs it evenly to obtain a precursor solution II, then allows the precursor solution I to undergo a hydrothermal reaction first, adds the precursor solution II and urea when the reaction is halfway through, continues to heat the two precursor solutions to undergo a hydrothermal reaction simultaneously, then adds nano boron nitride in the middle to obtain a nano composite powder, during the hydrothermal process, the precursor solution I first generates flaky nano magnesium oxide, then the precursor solution II and urea are added at this time, and the Ba in the precursor solution II is heated to a temperature of 100 °C. 2+ and Ti 4+They are combined in an alkaline hydrothermal environment to generate highly dispersed cubic phase barium titanate powder, at which time flaky nano-magnesium oxide continues to be generated, and nano-boron nitride is added. The three are coated and combined with each other, and due to the stability of urea in the alkaline environment, a nano-composite powder with high thermal conductivity, low dielectric constant and high mechanical strength with a three-phase composite structure is generated. The low dielectric thermal conductivity microwave ceramic powder obtained by sintering is doped in polytetrafluoroethylene, so that the high-frequency microwave thermal conductive single-layer copper-clad substrate also has high thermal conductivity, low dielectric constant and high mechanical strength, thereby improving the signal transmission performance of the circuit board.
[0017] 2. The present invention prepares a natural surface treatment agent from oak bark, and immerses polytetrafluoroethylene powder in the natural surface treatment agent and heats it for surface treatment. The polyphenol compounds in the natural surface treatment agent form a coating rich in polar groups on the surface of the polytetrafluoroethylene powder. At the same time, the low-medium thermal microwave ceramic powder and stearic acid are subjected to condensation reflux treatment to form a hydrophobic organic film on the surface of the ceramic powder. This film can improve the compatibility of the ceramic powder and polytetrafluoroethylene, promote the uniform dispersion of the two in the composite material, and avoid phase separation. In summary, the present invention greatly improves the compatibility of the ceramic powder and polytetrafluoroethylene. The compatibility between the prepared pretreated polytetrafluoroethylene powder and the surface-modified low-dielectric thermal conductivity microwave ceramic powder is enhanced, so that the surface-modified low-dielectric thermal conductivity microwave ceramic powder is evenly distributed in the subsequent powdered solid. After the high-frequency microwave thermal conductive single-layer copper-clad substrate is prepared, it can not only form a uniform heat conduction path and improve the heat dissipation performance, but also reduce the polarization between interfaces, thereby reducing the dielectric loss of the material. At the same time, good compatibility can also reduce the overall dielectric constant of the high-frequency microwave thermal conductive single-layer copper-clad substrate, thereby improving the operating frequency of the circuit and the signal transmission efficiency.
[0018] 3. The present invention obtains a mixed powder by ball-milling Y2(C2O4)3·10H2O, CuO and H2BO3, and then sintering the mixed powder with the nano-composite powder. The sintering temperature is reduced while the dielectric properties of the low-conductivity thermal microwave ceramic powder are maintained. The low-conductivity thermal microwave ceramic powder can be made denser during the sintering process, and the dielectric loss of the material can be reduced, thereby improving the dielectric properties of the prepared circuit board. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention is a flowchart of a method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance adopted in an embodiment of the present invention. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Embodiment 1: A method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance, such as Figure 1 As shown, the following steps are included: S1: Preparation of low dielectric microwave ceramic powder S1.1: Mix magnesium acetate and deionized water in a mass ratio of 1:25 and stir for 10 minutes to obtain a magnesium acetate solution, take 10 parts by weight of a 25% ammonia solution and place it in a container, then dropwise add 3 parts by weight of the magnesium acetate solution, and when the magnesium acetate solution is completely added, stir at a speed of 450 rpm for 20 minutes using a magnetic stirrer to obtain a precursor solution I, mix BaCl2·2H2O and deionized water in a mass ratio of 1:20 and place it in a container, then add 4wt% of polyvinyl pyrrolidone and stir for 15 minutes to obtain a BaCl2 solution, take 6 parts by weight of the BaCl2 solution and place it in an ice water bath, then dropwise add 2 parts by weight of a 15% titanium tetrachloride solution, and stir at a speed of 300 rpm for 20 minutes to obtain a precursor solution II; S1.2: The precursor solution I prepared in step S1.1 is transferred to a hydrothermal reactor, heated at 150°C for 12 hours, and then the precursor solution II prepared in step S1.1 and 0.5 parts by weight of urea are added, stirred for 10 minutes, and then the temperature is continuously raised to 200°C. After keeping the temperature for 8 hours, 1 part by weight of nano-boron nitride is added, and then the temperature is continuously heated for 6 hours. The precipitate is filtered to be washed with anhydrous ethanol for 8 minutes, and then rinsed with deionized water twice, and then placed in a vacuum drying oven to dry at 70°C for 6 hours to obtain a nano-composite powder; S1.3: Y2(C2O4)3·10H2O, CuO and H2BO3 are mixed in a mass ratio of 1:0.3:0.3 and placed in a planetary ball mill. 10 times the mass of zirconia balls with a particle size of 0.1 mm and 2 times the volume of anhydrous ethanol are added. The mixture is ball-milled at a speed of 400 rpm for 6 hours. The zirconia balls are separated to obtain a mixed powder. The nano-composite powder and the mixed powder are evenly mixed in a mass ratio of 1:0.1. The mixture is then placed in a muffle furnace and heated to 500°C at a heating rate of 3°C / min and calcined for 4 hours. The mixture is then heated to 1250°C and calcined for 2 hours. After cooling to room temperature, the mixture is ball-milled at a speed of 500 rpm for 5 hours. After drying, the mixture is sieved through an 80-mesh sieve to obtain a low-medium thermal conductivity microwave ceramic powder.
[0022] S2: Modification of high-frequency microwave substrate materials S2.1: Dry the oak bark at 40°C to control the moisture content to 5%, then crush it with a pulverizer, pass it through a 40-mesh sieve to obtain oak powder, mix the oak powder with deionized water at a solid-liquid ratio of 1:20 and place it in an ultrasonic constant temperature water bath, adjust the temperature to 80°C, the ultrasonic frequency to 25kHz, and ultrasonicate for 30 minutes, then filter through a vacuum filter to remove solid impurities to obtain an extract, perform rotary evaporation on the extract at 45°C, and concentrate it to 1 / 5 of the original volume to obtain a natural surface treatment agent; S2.2: Soak the polytetrafluoroethylene powder in the natural surface treatment agent obtained in step S2.1, heat it to 180°C, keep it warm for 20 minutes and then cool it naturally, filter it out after it cools to room temperature, wash it twice with deionized water, and then dry it at 75°C to obtain pretreated polytetrafluoroethylene powder; S2.3: Place 1 weight part of low-medium thermal conductivity microwave ceramic powder in 100 weight parts of anhydrous ethanol and ultrasonically treat it for 25 minutes at an ultrasonic frequency of 20 kHz to obtain a suspension, then add 2 wt% of stearic acid, continue ultrasonic treatment at the same frequency for 10 minutes, condense and reflux at 60°C for 2 hours, and finally vacuum dry at 80°C for 4 hours to obtain surface-modified low-medium thermal conductivity microwave ceramic powder.
[0023] S3: Composite pressing of microwave printed circuit boards S3.1: Pretreated polytetrafluoroethylene powder, vinyl triethoxysilane and deionized water are uniformly mixed in a mass ratio of 1:0.06:2 to obtain a pretreated polytetrafluoroethylene dispersion emulsion, 10 parts by weight of the pretreated polytetrafluoroethylene dispersion emulsion, 3 parts by weight of surface-modified low-mediation thermal microwave ceramic powder, 0.4 parts by weight of thermoplastic polyimide and 0.06 parts by weight of perfluoroalkoxy are mixed and stirred at a speed of 1000 rpm for 1 hour to obtain a mixed glue solution, and then ethanol is added to the mixed glue solution, the stirring speed is adjusted to 150 rpm, and the stirring is continued for 10 minutes and then filtered to obtain a colloidal solid, and the colloidal solid is placed in a vacuum dryer at 100°C to obtain a powdered solid; S3.2: Spread the powdered solid in a mold, then place the mold in a hot press, press and form it at a pressure of 40 MPa at room temperature, and then heat it at 350°C for 2 hours to obtain a composite substrate, and press a 20 μm thick electrolytic copper foil on the upper and lower sides of the composite substrate, and then press it at a temperature of 380°C and a pressure of 15 MPa for 20 minutes, and naturally cool it to below 60°C to obtain a high-frequency microwave thermal conductive single-layer copper-clad substrate; S3.3: Take a high-frequency microwave thermal conductive single-layer copper-clad substrate, use a PCB CNC drilling machine to complete the drilling process of through holes and blind holes, then remove the edge burrs of the hole mouth, first chemically deposit copper in the hole, and then electroplate copper in the hole on the chemically deposited copper layer. After drying, the copper surface is sequentially subjected to positive film pasting, exposure and development, circuit electroplating, circuit etching and dry film de-drying to obtain a high-frequency microwave thermal conductive single-layer circuit board, and the high-frequency microwave thermal conductive single-layer circuit board is loaded into a hot press in the order of high-frequency microwave thermal conductive single-layer circuit board-high-frequency microwave thermal conductive single-layer copper-clad substrate-high-frequency microwave thermal conductive single-layer circuit board, and pressed at 320°C and a pressure of 3MPa for 25 minutes to obtain a high-frequency microwave printed circuit board with high heat dissipation performance.
[0024] Embodiment 2: A method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance, such as Figure 1 As shown, the following steps are included: S1: Preparation of low dielectric microwave ceramic powder S1.1: Mix magnesium acetate and deionized water in a mass ratio of 1:30 and stir for 10 minutes to obtain a magnesium acetate solution, take 12 parts by weight of a 30% ammonia solution and place it in a container, then dropwise add 4 parts by weight of the magnesium acetate solution, and when the magnesium acetate solution is completely added, stir at a speed of 450 rpm for 20 minutes using a magnetic stirrer to obtain a precursor solution I, mix BaCl2·2H2O and deionized water in a mass ratio of 1:25 and place it in a container, then add 4wt% of polyvinyl pyrrolidone and stir for 15 minutes to obtain a BaCl2 solution, take 8 parts by weight of the BaCl2 solution and place it in an ice water bath, then dropwise add 3 parts by weight of a 20% titanium tetrachloride solution, and stir at a speed of 300 rpm for 20 minutes to obtain a precursor solution II; S1.2: The precursor solution I prepared in step S1.1 is transferred to a hydrothermal reactor, heated at 150°C for 12 hours, and then the precursor solution II prepared in step S1.1 and 0.5 parts by weight of urea are added, stirred for 10 minutes, and then the temperature is continuously raised to 200°C. After keeping the temperature for 8 hours, 1.5 parts by weight of nano-boron nitride is added, and then the temperature is continuously heated for 6 hours. The precipitate is filtered to be washed with anhydrous ethanol for 8 minutes, and then rinsed with deionized water twice, and then dried in a vacuum drying oven at 70°C for 6 hours to obtain a nano-composite powder; S1.3: Y2(C2O4)3·10H2O, CuO and H2BO3 are mixed in a mass ratio of 1:0.4:0.4 and placed in a planetary ball mill. Ten times the mass of zirconia balls with a particle size of 0.1 mm and 2 times the volume of anhydrous ethanol are added. The mixture is ball-milled at a speed of 400 rpm for 6 hours. The zirconia balls are separated to obtain a mixed powder. The nano-composite powder and the mixed powder are evenly mixed in a mass ratio of 1:0.2. The mixture is then placed in a muffle furnace and heated to 500°C at a heating rate of 3°C / min and calcined for 4 hours. The mixture is then heated to 1250°C and calcined for 2 hours. After cooling to room temperature, the mixture is ball-milled at a speed of 500 rpm for 5 hours. After drying, the mixture is sieved through an 80-mesh sieve to obtain a low-medium thermal conductivity microwave ceramic powder.
[0025] S2: Modification of high-frequency microwave substrate materials S2.1: Dry the oak bark at 40°C to control the moisture content to 5%, then crush it with a pulverizer, pass it through a 40-mesh sieve to obtain oak powder, mix the oak powder with deionized water at a solid-liquid ratio of 1:25 and place it in an ultrasonic constant temperature water bath, adjust the temperature to 80°C, the ultrasonic frequency to 25kHz, and ultrasonicate for 30 minutes, then filter through a vacuum filter to remove solid impurities to obtain an extract, perform rotary evaporation on the extract at 45°C, and concentrate it to 1 / 5 of the original volume to obtain a natural surface treatment agent; S2.2: Soak the polytetrafluoroethylene powder in the natural surface treatment agent obtained in step S2.1, heat it to 180°C, keep it warm for 20 minutes and then cool it naturally, filter it out after it cools to room temperature, wash it twice with deionized water, and then dry it at 75°C to obtain pretreated polytetrafluoroethylene powder; S2.3: Place 2 parts by weight of low-medium thermal conductivity microwave ceramic powder in 120 parts by weight of anhydrous ethanol and ultrasonically treat it for 25 minutes at an ultrasonic frequency of 20 kHz to obtain a suspension, then add 2 wt% of stearic acid, continue ultrasonic treatment at the same frequency for 10 minutes, condense and reflux at 60°C for 2 hours, and finally vacuum dry at 80°C for 4 hours to obtain surface-modified low-medium thermal conductivity microwave ceramic powder.
[0026] S3: Composite pressing of microwave printed circuit boards S3.1: Pretreated polytetrafluoroethylene powder, vinyl triethoxysilane and deionized water are uniformly mixed in a mass ratio of 1:0.08:3 to obtain a pretreated polytetrafluoroethylene dispersion emulsion, 12 parts by weight of the pretreated polytetrafluoroethylene dispersion emulsion, 4 parts by weight of surface-modified low-mediation thermal microwave ceramic powder, 0.6 parts by weight of thermoplastic polyimide and 0.08 parts by weight of perfluoroalkoxy are mixed and stirred at a speed of 1000 rpm for 1 hour to obtain a mixed glue solution, and then ethanol is added to the mixed glue solution, the stirring speed is adjusted to 150 rpm, and the stirring is continued for 10 minutes and then filtered to obtain a colloidal solid, and the colloidal solid is placed in a vacuum dryer at 100°C to obtain a powdered solid; S3.2: Spread the powdered solid in a mold, then place the mold in a hot press, press and form it at a pressure of 40 MPa at room temperature, and then heat it at 350°C for 2 hours to obtain a composite substrate, and press a 20 μm thick electrolytic copper foil on the upper and lower sides of the composite substrate, and then press it at a temperature of 380°C and a pressure of 15 MPa for 20 minutes, and naturally cool it to below 60°C to obtain a high-frequency microwave thermal conductive single-layer copper-clad substrate; S3.3: Take a high-frequency microwave thermal conductive single-layer copper-clad substrate, use a PCB CNC drilling machine to complete the drilling process of through holes and blind holes, then remove the edge burrs of the hole mouth, first chemically deposit copper in the hole, and then electroplate copper in the hole on the chemically deposited copper layer. After drying, the copper surface is sequentially subjected to positive film pasting, exposure and development, circuit electroplating, circuit etching and dry film de-drying to obtain a high-frequency microwave thermal conductive single-layer circuit board, and the high-frequency microwave thermal conductive single-layer circuit board is loaded into a hot press in the order of high-frequency microwave thermal conductive single-layer circuit board-high-frequency microwave thermal conductive single-layer copper-clad substrate-high-frequency microwave thermal conductive single-layer circuit board, and pressed at 320°C and a pressure of 3MPa for 25 minutes to obtain a high-frequency microwave printed circuit board with high heat dissipation performance.
[0027] Embodiment 3: A method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance, such as Figure 1 As shown, the following steps are included: S1: Preparation of low dielectric microwave ceramic powder S1.1: Mix magnesium acetate and deionized water in a mass ratio of 1:25 and stir for 15 minutes to obtain a magnesium acetate solution, take 10 parts by weight of a 30% ammonia solution and place it in a container, then dropwise add 3 parts by weight of the magnesium acetate solution, and when the magnesium acetate solution is completely added, stir at a speed of 500 rpm for 30 minutes using a magnetic stirrer to obtain a precursor solution I, mix BaCl2·2H2O and deionized water in a mass ratio of 1:20 and place it in a container, then add 6wt% of polyvinyl pyrrolidone and stir for 20 minutes to obtain a BaCl2 solution, take 6 parts by weight of the BaCl2 solution and place it in an ice water bath, then dropwise add 2 parts by weight of a 15% titanium tetrachloride solution, and stir at a speed of 350 rpm for 25 minutes to obtain a precursor solution II; S1.2: Transfer the precursor solution I prepared in step S1.1 to a hydrothermal reactor, heat at 180°C for 16 hours, then add the precursor solution II prepared in step S1.1 and 1 part by weight of urea, stir for 20 minutes, then continue to heat to 220°C, keep warm for 10 hours, add 1 part by weight of nano boron nitride, and continue heating for 8 hours, filter to obtain a precipitate, wash with anhydrous ethanol for 10 minutes, then rinse with deionized water 3 times, and then place in a vacuum drying oven and dry at 80°C for 8 hours to obtain a nano composite powder; S1.3: Y2(C2O4)3·10H2O, CuO and H2BO3 are mixed in a mass ratio of 1:0.3:0.3 and placed in a planetary ball mill. 15 times the mass of zirconia balls with a particle size of 1 mm and 3 times the volume of anhydrous ethanol are added. The mixture is ball-milled at a speed of 500 rpm for 8 hours. The zirconia balls are separated to obtain a mixed powder. The nano-composite powder and the mixed powder are evenly mixed in a mass ratio of 1:0.1. The mixture is then placed in a muffle furnace and heated to 600°C at a heating rate of 5°C / min and calcined for 4 hours. The mixture is then heated to 1200°C and calcined for 3 hours. After cooling to room temperature, the mixture is ball-milled at a speed of 600 rpm for 6 hours. After drying, the mixture is sieved through a 100-mesh sieve to obtain a low-medium thermal conductivity microwave ceramic powder.
[0028] S2: Modification of high-frequency microwave substrate materials S2.1: Dry the oak bark at 60°C to control the moisture content to 10%, then crush it with a pulverizer, pass it through a 550-mesh sieve to obtain oak powder, mix the oak powder with deionized water at a solid-liquid ratio of 1:25 and place it in an ultrasonic constant temperature water bath, adjust the temperature to 90°C, the ultrasonic frequency to 30kHz, and ultrasonicate for 40 minutes, then filter through a vacuum filter to remove solid impurities to obtain an extract, and perform rotary evaporation on the extract at 50°C to concentrate it to 1 / 4 of the original volume to obtain a natural surface treatment agent; S2.2: Soak the polytetrafluoroethylene powder in the natural surface treatment agent obtained in step S2.1, heat it to 200°C, keep it warm for 30 minutes and then cool it naturally, filter it out after it drops to room temperature, wash it with deionized water for 3 times, and then dry it at 80°C to obtain pretreated polytetrafluoroethylene powder; S2.3: Place 1 weight part of low-medium thermal conductivity microwave ceramic powder in 100 weight parts of anhydrous ethanol and ultrasonically treat it for 30 minutes at an ultrasonic frequency of 30 kHz to obtain a suspension, then add 3 wt% of stearic acid, continue ultrasonic treatment at the same frequency for 15 minutes, condense and reflux at 65°C for 3 hours, and finally vacuum dry at 85°C for 6 hours to obtain surface-modified low-medium thermal conductivity microwave ceramic powder.
[0029] S3: Composite pressing of microwave printed circuit boards S3.1: Pretreated polytetrafluoroethylene powder, vinyl triethoxysilane and deionized water are uniformly mixed in a mass ratio of 1:0.06:2 to obtain a pretreated polytetrafluoroethylene dispersion emulsion, 10 parts by weight of the pretreated polytetrafluoroethylene dispersion emulsion, 3 parts by weight of surface-modified low-mediation thermal microwave ceramic powder, 0.4 parts by weight of thermoplastic polyimide and 0.06 parts by weight of perfluoroalkoxy are mixed and stirred at a speed of 1200 rpm for 1.5 hours to obtain a mixed glue solution, and then ethanol is added to the mixed glue solution, the stirring speed is adjusted to 200 rpm, and the stirring is continued for 15 minutes and then filtered to obtain a colloidal solid, and the colloidal solid is placed at 110°C and vacuum dried to obtain a powdered solid; S3.2: Spread the powdered solid in a mold, then place the mold in a hot press, press it at a pressure of 50 MPa at room temperature, and then heat it at 400°C for 1 hour to obtain a composite substrate, and press a 25 μm thick electrolytic copper foil on the upper and lower sides of the composite substrate, and then press it at a temperature of 400°C and a pressure of 10 MPa for 25 minutes, and naturally cool it to below 60°C to obtain a high-frequency microwave thermal conductive single-layer copper-clad substrate; S3.3: Take a high-frequency microwave thermal conductive single-layer copper-clad substrate, use a PCB CNC drilling machine to complete the drilling process of through holes and blind holes, then remove the edge burrs of the hole mouth, first chemically deposit copper in the hole, and then electroplate copper in the hole on the chemically deposited copper layer. After drying, the copper surface is sequentially subjected to positive film pasting, exposure and development, circuit electroplating, circuit etching and dry film de-drying to obtain a high-frequency microwave thermal conductive single-layer circuit board. The high-frequency microwave thermal conductive single-layer circuit board-high-frequency microwave thermal conductive single-layer copper-clad substrate-high-frequency microwave thermal conductive single-layer circuit board are loaded into a hot press in the order of high-frequency microwave thermal conductive single-layer circuit board-high-frequency microwave thermal conductive single-layer circuit board, and pressed at 350°C and a pressure of 5MPa for 15 minutes to obtain a high-frequency microwave printed circuit board with high heat dissipation performance.
[0030] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 removes step S1, and replaces the subsequent low-medium thermal conductivity microwave ceramic powder with a ceramic powder of the BaO-ZnO-TiO2 system. The remaining steps are the same as those in Example 1 to obtain a high-frequency microwave thermal conductive single-layer circuit board, which is recorded as Comparative Example 1.
[0031] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 removes step S2.1 and step S2.2, replaces the subsequent pre-treated polytetrafluoroethylene powder with polytetrafluoroethylene powder, and the remaining steps are the same as Example 1 to obtain a high-frequency microwave thermal conductive single-layer circuit board, which is recorded as Comparative Example 2.
[0032] Comparative Example 3: The difference between Comparative Example 3 and Example 1 is that Comparative Example 3 removes step S2.3, and replaces the subsequent surface-modified low-medium thermal conductivity microwave ceramic powder with low-medium thermal conductivity microwave ceramic powder. The remaining steps are the same as Example 1, and a high-frequency microwave thermal conductive single-layer circuit board is obtained, which is recorded as Comparative Example 3.
[0033] Comparative Example 4: The difference between Comparative Example 4 and Example 1 is that, in Comparative Example 4, Y2(C2O4)3·10H2O, CuO and H2BO3 are not added in step S1.3, and the remaining steps are the same as those in Example 1 to prepare a high-frequency microwave thermal conductive single-layer circuit board, which is recorded as Comparative Example 4.
[0034] Experiment 1: Take the high-frequency microwave thermal conductive single-layer circuit boards prepared in Examples 1-3 and Comparative Examples 1-4, and use a KEYSIGHT-N5224B vector network analyzer to test their dielectric constants and dielectric losses. The test frequency is 10 GHz, and the data are recorded and tabulated, as shown in Table 1.
[0035] Table 1: Dielectric constant and dielectric loss of high-frequency microwave thermal conductive single-layer circuit board Dielectric constant / 10GHz Dielectric loss / 10GHz Example 1 2.81 0.0035 Example 2 2.78 0.0029 Example 3 2.68 0.0028 Comparative Example 1 4.73 0.0083 Comparative Example 2 3.31 0.0062 Comparative Example 3 3.35 0.0064 Comparative Example 4 4.13 0.0071 Experiment 2: Take the high-frequency microwave thermal conductive single-layer circuit boards prepared in Examples 1-3 and Comparative Examples 1-3, take three of each, and use a thermal constant analyzer to measure their thermal conductivity by the non-steady-state heat flow method. Under a 25°C environment, clamp the probes on both sides of the wafer samples, set the test time and power to 20s and 20mW respectively, record the data and make a table, as shown in Table 2.
[0036] Table 2: Thermal conductivity of high-frequency microwave thermal conductive single-layer circuit board Thermal conductivity / (W / m·k) The first Second copy The third Example 1 16.2 16.4 16.1 Example 2 16.5 16.7 16.8 Example 3 17.1 17.3 17.2 Comparative Example 1 2.5 2.7 2.6 Comparative Example 2 14.3 14.6 14.5 Comparative Example 3 14.7 14.5 14.8 Experiment 3: Take the composite substrates prepared in Examples 1-3 and the composite substrate prepared in Comparative Example 1, take three portions respectively and use a universal testing machine to test the tensile strength, record the data and make a table, as shown in Table 3.
[0037] Table 3: Tensile strength of composite substrates <![CDATA[Tensile strength (N / cm 2 ).]]> The first Second copy The third Example 1 151.4 151.6 151.7 Example 2 153.3 153.1 153.5 Example 3 154.2 153.9 154.3 Comparative Example 1 90.3 90.4 90.6 It can be seen from Table 1 that the dielectric constant of the high-frequency microwave thermal conductive single-layer circuit board prepared in the embodiment is lower than that of comparative examples 1-4, and the dielectric loss is lower than that of comparative examples 1-4. It can be proved that the dielectric properties of the circuit board can be improved by preparing low dielectric thermal conductivity microwave ceramic powder and adding it to the preparation process of the high-frequency microwave thermal conductive single-layer copper-clad substrate. At the same time, it can be proved that modifying the polytetrafluoroethylene powder and the low dielectric thermal conductivity microwave ceramic powder can reduce the dielectric loss of the circuit board and improve the dielectric properties, thereby improving the operating frequency and signal transmission efficiency of the circuit. It can also be proved that Y2(C2O4)3·10H2O, CuO and H2BO3 are mixed and ball-milled to obtain a mixed powder, and then sintered with the nano-composite powder to obtain a low dielectric thermal conductivity microwave ceramic powder. Adding it to the preparation process of the high-frequency microwave thermal conductive single-layer circuit board can improve its dielectric properties.
[0038] It can be seen from Table 2 that the thermal conductivity of the high-frequency microwave thermal conductive single-layer circuit board prepared in the embodiment is greater than that of comparative examples 1-3, which can prove that the thermal conductivity of the circuit board can be improved by preparing low-medium thermal conductivity microwave ceramic powder and adding it into the preparation process of the high-frequency microwave thermal conductive single-layer copper-clad substrate, thereby improving its heat dissipation capacity. At the same time, it can be proved that the polytetrafluoroethylene powder and the low-medium thermal conductivity microwave ceramic powder can be modified to be uniformly dispersed in the circuit board to form a heat conduction path, thereby improving its heat dissipation capacity.
[0039] It can be seen from Table 3 that the tensile strength of the composite substrate prepared in Example 1 is greater than that of the composite substrate prepared in Comparative Example 1, which can prove that the mechanical properties of the circuit board can be improved by preparing low-medium thermal conductivity microwave ceramic powder and adding it to the preparation process of a high-frequency microwave thermal conductive single-layer copper-clad substrate.
[0040] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance, characterized in that: The following steps are involved: S1: Preparation of low dielectric microwave ceramic powder Mixing magnesium acetate and deionized water to obtain a magnesium acetate solution, then adding the magnesium acetate solution dropwise into an ammonia solution, stirring to obtain a precursor solution I, preparing a BaCl2 solution and placing it in an ice water bath, adding a titanium tetrachloride solution dropwise, stirring to obtain a precursor solution II, first heating the precursor solution I, then adding the precursor solution II and urea to heat, adding nano boron nitride midway to continue heating, filtering to obtain a precipitate, washing and drying to obtain a nano composite powder, mixing Y2(C2O4)3·10H2O, CuO and H2BO3 and ball milling to obtain a mixed powder, mixing the nano composite powder and the mixed powder, sintering and ball milling, drying and sieving to obtain a low-medium thermal microwave ceramic powder; S2: Modification of high-frequency microwave substrate materials The oak bark is dried and crushed, mixed with deionized water, and subjected to ultrasonic treatment at elevated temperature, filtered to obtain an extract, the extract is rotary evaporated to obtain a natural surface treatment agent, polytetrafluoroethylene powder is immersed in the natural surface treatment agent and heated, and washed and dried after natural cooling to obtain pretreated polytetrafluoroethylene powder, low-medium thermal microwave ceramic powder is mixed with anhydrous ethanol and subjected to ultrasonic treatment to obtain a suspension, and then stearic acid is added, and ultrasonic treatment is continued, followed by condensation reflux, and drying to obtain surface-modified low-medium thermal microwave ceramic powder; S3: Composite pressing of microwave printed circuit boards The pretreated polytetrafluoroethylene powder, silane coupling agent and deionized water are uniformly mixed to obtain a pretreated polytetrafluoroethylene dispersion emulsion; the pretreated polytetrafluoroethylene dispersion emulsion, surface modified low-medium thermal conductivity microwave ceramic powder, thermoplastic polyimide and plasticizer are mixed and stirred to obtain a mixed glue solution; ethanol is added and stirred continuously and filtered to obtain a colloidal solid; a powdered solid is obtained after drying; the powdered solid is hot pressed to obtain a composite substrate; an electrolytic copper foil is pressed on the upper and lower sides of the composite substrate and then hot pressed to obtain a high-frequency microwave thermal conductive single-layer copper-clad substrate; the high-frequency microwave thermal conductive single-layer copper-clad substrate is taken and drilled, deburred, chemically deposited copper, electroplated copper in the hole, attached a positive film dry film, exposed and developed, electroplated, etched and de-dried to obtain a high-frequency microwave thermal conductive single-layer circuit board; the high-frequency microwave thermal conductive single-layer circuit board is loaded into a hot press in the order of high-frequency microwave thermal conductive single-layer circuit board-high-frequency microwave thermal conductive single-layer copper-clad substrate-high-frequency microwave thermal conductive single-layer circuit board for hot pressing to obtain a high-frequency microwave printed circuit board with high heat dissipation performance.
2. The method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance according to claim 1, characterized in that: Step S1: Preparation of low dielectric microwave ceramic powder, comprising the following steps: S1.1: Mix magnesium acetate and deionized water in a mass ratio of 1: (25-30) and stir for 10-15 minutes to obtain a magnesium acetate solution, take 10-12 parts by weight of an ammonia solution and place it in a container, then dropwise add 3-4 parts by weight of the magnesium acetate solution, and when the magnesium acetate solution is completely added, stir at a speed of 450-500rpm using a magnetic stirrer for 20-30 minutes to obtain a precursor solution I, mix BaCl2·2H2O and deionized water in a mass ratio of 1: (20-25) and place it in a container, then add 4-6wt% of polyvinyl pyrrolidone, stir for 15-20 minutes to obtain a BaCl2 solution, take 6-8 parts by weight of the BaCl2 solution and place it in an ice water bath, then dropwise add 2-3 parts by weight of a titanium tetrachloride solution with a mass fraction of 15-20%, and stir at a speed of 300-350rpm for 20-25 minutes to obtain a precursor solution II; S1.2: Transfer the precursor solution I prepared in step S1.1 to a hydrothermal reactor, heat it at 150-180°C for 12-16 hours, then add the precursor solution II prepared in step S1.1 and 0.5-1 parts by weight of urea, stir for 10-20 minutes, continue to heat to 200-220°C, keep warm for 8-10 hours, add 1-1.5 parts by weight of nano boron nitride, continue heating for 6-8 hours, filter to obtain a precipitate, wash it with anhydrous ethanol for 8-10 minutes, rinse it with deionized water 2-3 times, and then place it in a vacuum drying oven at 70-80°C for 6-8 hours to obtain a nano composite powder; S1.3: Y2(C2O4)3·10H2O, CuO and H2BO3 are mixed in a mass ratio of 1: (0.3-0.4): (0.3-0.4) and placed in a planetary ball mill, 10-15 times the mass of zirconia balls and 2-3 times the volume of anhydrous ethanol are added, and the mixture is ball-milled at a speed of 400-500rpm for 6-8 hours, and the zirconia balls are separated to obtain a mixed powder. The nano-composite powder and the mixed powder are evenly mixed in a mass ratio of 1: (0.1-0.2), and then placed in a muffle furnace and heated to 500-600℃ at a heating rate of 3-5℃ / min and calcined for 4-5 hours, and then heated to 1200-1250℃ and calcined for 2-3 hours. After cooling to room temperature, the mixture is ball-milled at a speed of 500-600rpm for 5-6 hours. After drying, the mixture is sieved through an 80-100 mesh sieve to obtain a low-medium thermal microwave ceramic powder.
3. The method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance according to claim 2, characterized in that: Step S2: modification of high-frequency microwave substrate raw materials, including the following steps: S2.1: Dry the oak bark at 40-60°C to control the moisture content to 5-10%, then grind it with a grinder, pass it through a 40-50 mesh sieve to obtain oak powder, mix the oak powder with deionized water at a solid-liquid ratio of 1: (20-25) and place it in an ultrasonic constant temperature water bath, adjust the temperature to 80-90°C, the ultrasonic frequency to 25-30kHz, and perform ultrasonic treatment for 30-40 minutes, then filter through a vacuum filter to remove solid impurities to obtain an extract, and perform rotary evaporation on the extract at 45-50°C to obtain a natural surface treatment agent; S2.2: Soak the polytetrafluoroethylene powder in the natural surface treatment agent obtained in step S2.1, heat it to 180-200°C, keep it warm for 20-30 minutes, then cool it naturally, filter it out after it cools to room temperature, wash it with deionized water 2-3 times, and then dry it at 75-80°C to obtain pretreated polytetrafluoroethylene powder; S2.3: Place 1-2 parts by weight of low-medium thermal conductivity microwave ceramic powder in 100-120 parts by weight of anhydrous ethanol and ultrasonically treat it for 25-30 minutes at an ultrasonic frequency of 20-30kHz to obtain a suspension, then add 2-3wt% of stearic acid, continue ultrasonic treatment at the same frequency for 10-15 minutes, condense and reflux at 60-65°C for 2-3 hours, and finally vacuum dry at 80-85°C for 4-6 hours to obtain surface-modified low-medium thermal conductivity microwave ceramic powder.
4. The method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance according to claim 3, characterized in that: Step S3: Composite pressing of microwave printed circuit boards. The following steps are involved: S3.1: pretreated polytetrafluoroethylene powder, silane coupling agent and deionized water are uniformly mixed in a mass ratio of 1: (0.06-0.08): (2-3) to obtain a pretreated polytetrafluoroethylene dispersion emulsion, 10-12 parts by weight of the pretreated polytetrafluoroethylene dispersion emulsion, 3-4 parts by weight of surface-modified low-mediation thermal microwave ceramic powder, 0.4-0.6 parts by weight of thermoplastic polyimide and 0.06-0.08 parts by weight of plasticizer are mixed and stirred at a speed of 1000-1200 rpm for 1-1.5 hours to obtain a mixed glue solution, and then ethanol is added to the mixed glue solution, the stirring speed is adjusted to 150-200 rpm, and the stirring is continued for 10-15 minutes and then filtered to obtain a colloidal solid, and the colloidal solid is placed in a vacuum dryer at 100-110°C to obtain a powdered solid; S3.2: Spread the powdered solid in a mold, then place the mold in a hot press, press it at a pressure of 40-50 MPa at room temperature, and then heat it at 350-400°C for 1-2 hours to obtain a composite substrate, and press a sheet of electrolytic copper foil on the upper and lower sides of the composite substrate, and then press it at a temperature of 380-400°C and a pressure of 10-15 MPa for 20-25 minutes, and naturally cool it to below 60°C to obtain a high-frequency microwave thermal conductive single-layer copper-clad substrate; S3.3: Take a high-frequency microwave thermal conductive single-layer copper-clad substrate, use a PCB CNC drilling machine to complete the drilling process of through holes and blind holes, then remove the edge burrs of the hole mouth, first chemically deposit copper in the hole, and then electroplate copper in the hole on the chemically deposited copper layer. After drying, paste positive film, expose and develop, electroplate the circuit, etch the circuit and de-dry the film on the copper surface in sequence to obtain a high-frequency microwave thermal conductive single-layer circuit board, and load them into a hot press in the order of high-frequency microwave thermal conductive single-layer circuit board-high-frequency microwave thermal conductive single-layer copper-clad substrate-high-frequency microwave thermal conductive single-layer circuit board, press at 320-350℃ and a pressure of 3-5MPa for 15-25 minutes to obtain a high-frequency microwave printed circuit board with high heat dissipation performance.
5. The method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance according to claim 2, characterized in that: The concentration of the aqueous ammonia solution in step S1.1 is 25-30%.
6. The method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance according to claim 2, characterized in that: The particle size of the zirconium oxide balls in step S1.3 is 0.1-1 mm.
7. The method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance according to claim 3, characterized in that: The volume of the extract in step S2.1 after rotary evaporation is 1 / 5-1 / 4 of the original volume.
8. The method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance according to claim 4, characterized in that: The silane coupling agent in step S3.1 is vinyl triethoxy silane, and the plasticizer is perfluoroalkoxy.
9. The method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance according to claim 4, characterized in that: The thickness of the electrolytic copper foil in step S3.2 is 20-25 μm.
10. A high-frequency microwave printed circuit board with high heat dissipation performance, characterized in that: It is prepared by the method for preparing a high-frequency microwave printed circuit board with high heat dissipation performance according to any one of claims 1 to 9.
Citation Information
Patent Citations
High-efficiency and high-frequency microwave composite multilayer board manufacturing method
CN107567209A
Microwave dielectric ceramics and polytetrafluoroethylene-ceramic composite substrate, and preparation methods thereof
CN107746272A
Preparation method of low-loss ultrathin PTFE microwave dielectric substrate
CN117429141A
Ceramic filler, method of preparing the ceramic filler and applications as resonator and laminate thereof
US20150274926A1
Cited By
Multi-layer composite circuit board preparation method and multi-layer composite circuit board
CN119653647A
Multilayer composite circuit board preparation method and multilayer composite circuit board
CN119653647B