Titanium-aluminum-based composite board, preparation method and application

Through the preparation method of titanium-aluminum composite sheet, combined with molding, sintering, rolling and solid solution treatment, the problems of poor thermal conductivity and low stiffness of the heat exchange core plate in aerospace equipment are solved, and lightweight, high thermal conductivity and high stiffness are achieved. Performance, suitable for the manufacture of heat exchange core plates in aerospace equipment.

CN118976900AActive Publication Date: 2024-11-19HUNAN JINTIAN ALUMINUM HI TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411047568.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing heat exchange core plates have poor thermal conductivity and low stiffness, making it difficult to meet the needs of aerospace equipment for lightweight, high thermal conductivity and high stiffness.

Method used

By using the preparation method of titanium-aluminum-based composite plate, the aluminum-based powder is mixed in a specific proportion to form the aluminum-based powder, molded into the aluminum substrate, and pressed with the titanium plate after surface etching. Afterwards, sintering, molding and multi-pass rolling were carried out, and combined with solid solution and artificial aging treatment, a 0.5-1mm thick titanium-aluminum composite sheet was obtained.

Benefits of technology

It realizes the lightweight, high thermal conductivity and high stiffness performance of titanium-aluminum-based composite sheets, solves the problems of poor thermal conductivity and low stiffness of existing heat exchange core plates, and is suitable for the manufacturing of heat exchange core plates in aerospace equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004973921540000051
    Figure BDA0004973921540000051
  • Figure BDA0004973921540000061
    Figure BDA0004973921540000061
Patent Text Reader

Abstract

The invention relates to the technical field of titanium-aluminum-based material processing, in particular to a titanium-aluminum-based composite board, a preparation method and application. The titanium-aluminum-based composite board is prepared by the preparation method. The preparation method comprises the following steps: forming an aluminum substrate; the aluminum substrate and the titanium plate subjected to surface etching treatment are pressed to form a prefabricated plate, and the prefabricated plate is sintered; carrying out mould pressing shaping on the sintered prefabricated slab; and carrying out multi-pass rolling treatment on the prefabricated plate subjected to mould pressing shaping to obtain the titanium-aluminum-based composite plate with the thickness of 0.5-1 mm. The application refers to the application of the titanium-aluminum-based composite board in the aspect of manufacturing a heat exchange core board. The prepared titanium-aluminum-based composite board has the performance advantages of being light in weight, high in heat conductivity and high in rigidity, can be used for manufacturing a heat exchange core board and used in aerospace equipment, and can solve the problems that an existing heat exchanger is poor in heat conductivity and low in rigidity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium-aluminum-based material processing, and in particular to a titanium-aluminum-based composite plate, a preparation method and application thereof. Background Art

[0002] Heat exchangers are often needed in aerospace equipment to meet heat exchange requirements. The heat exchange core plate in the heat exchanger directly determines the heat exchange performance. The heat exchange core plates used in aerospace equipment often need to have the advantages of light weight, high rigidity and high thermal conductivity. However, some of the existing heat exchange core plates are made of stainless steel, which will have the problem of poor thermal conductivity. Some of the existing heat exchange core plates are also made of aluminum alloy materials. Although this can meet the requirements of lightweight, the rigidity of aluminum alloy materials is low and it is easy to deform when stamping to form heat exchange channels, resulting in a decrease in the yield rate.

[0003] In summary, it is necessary to provide a titanium-aluminum-based composite plate, a preparation method and an application to solve the problems of poor thermal conductivity and low rigidity of existing heat exchange core plates. Summary of the invention

[0004] The present invention aims to provide a titanium-aluminum-based composite plate, a preparation method and an application thereof. The specific technical scheme is as follows:

[0005] In a first aspect, the present invention provides a method for preparing a titanium-aluminum-based composite plate, comprising:

[0006] Step S1, mixing metal powder, TiO2 powder and binder according to the mass percentage of (79%-95%): (4.5%-20%): (0.5%-1%) to form aluminum-based powder, and forming an aluminum substrate by molding; the mass percentages of the metal components in the aluminum substrate are as follows: magnesium 1.0%-1.5%, copper 0.5%-1.2%, zirconium 0.2%-0.5%, yttrium 0.2%-0.5%, titanium 0.5%-1% and the balance aluminum;

[0007] Step S2, pressing the aluminum substrate and the titanium plate after surface etching to form a prefabricated plate, and sintering the prefabricated plate;

[0008] Step S3, molding and shaping the prefabricated board after sintering;

[0009] Step S4, subjecting the prefabricated plate after molding and shaping to multiple rolling processes to obtain a titanium-aluminum-based composite plate with a thickness of 0.5-1 mm; wherein, before completing the last rolling process, the prefabricated plate is also subjected to solution treatment and artificial aging treatment in sequence, and then, the prefabricated plate is flattened by the last rolling process to obtain a titanium-aluminum-based composite plate with a thickness of 0.5-1 mm.

[0010] Optionally, in step S1, the metal powder includes aluminum powder; the particle size of the aluminum powder is 20-50 microns.

[0011] Optionally, the particle size of the TiO2 powder is 0.5-2 microns.

[0012] Optionally, in step S2, the surface etching treatment includes adding nitric acid and ferric chloride to an ammonium bifluoride solution, mixing to form an etching solution, immersing the titanium plate in the etching solution, and etching the surface of the titanium plate for 30-60s at an etching temperature of 40-50°C; cleaning and drying the titanium plate after the surface etching treatment.

[0013] Optionally, the concentration of the ammonium bifluoride solution is 10-20 g / L; the concentration of the nitric acid is 20-50 g / L; the concentration of the ferric chloride is 5-10 g / L; and the titanium plate is a TC4 titanium plate with a thickness of 0.1-0.5 mm.

[0014] Optionally, in step S2, the sintering treatment adopts a sintering temperature of 500-680°C and a sintering time of 2-4h.

[0015] Optionally, in step S3, the molding pressure used in the molding is 150-200 MPa and the molding temperature is 500-580°C.

[0016] Optionally, in step S4, the rolling temperature used in the rolling treatment is 450-550°C, and the reduction amount used in each rolling treatment is 5-10mm; the solution temperature used in the solution treatment is 465-495°C, and the solution time is 2-5h; the treatment temperature used in the artificial aging treatment is 170-190°C, and the treatment time is 5-12h.

[0017] In a second aspect, the present invention provides a titanium-aluminum-based composite plate material, which is prepared by the preparation method of the titanium-aluminum-based composite plate material.

[0018] In a third aspect, the present invention provides an application of a titanium-aluminum-based composite plate material, and uses the titanium-aluminum-based composite plate material in manufacturing a heat exchange core plate.

[0019] The application of the technical solution of the present invention has at least the following beneficial effects:

[0020] (1) The present invention provides a method for preparing a titanium-aluminum-based composite plate. The prepared titanium-aluminum-based composite plate has the performance advantages of light weight, high thermal conductivity and high rigidity. It can be used to make heat exchange core plates and used in aerospace equipment. It can solve the problems of poor thermal conductivity and low rigidity of existing heat exchangers. Specifically, the mass percentages of the metal components in the aluminum substrate obtained in step S1 of the present invention are as follows: 1.0-1.5% magnesium, 0.5%-1.2% copper, 0.2%-0.5% zirconium, 0.2%-0.5% yttrium, 0.5%-1% titanium and the remainder aluminum; the aluminum substrate composed of the metal powder and TiO2 powder can improve the rigidity and strength of the titanium-aluminum-based composite plate; the present invention performs surface etching on the titanium plate in step S2 to facilitate the formation of micro-nanoscale holes on the surface of the titanium plate, which not only increases The surface area of ​​the titanium plate is increased, and multiple pressing and embedding points are provided on the titanium plate for pressing the titanium plate and the aluminum substrate, which greatly enhances the firmness of the prefabricated plate pressed together by the titanium plate and the aluminum substrate; in addition, the titanium plate and the aluminum substrate are used in combination to facilitate the ductility of the titanium alloy, the high stiffness and lightness of the aluminum-based composite material, and titanium has better corrosion resistance. In this way, the lightweight of the aluminum alloy and the high stiffness and high elastic modulus of the aluminum-based composite material can be utilized, as well as the corrosion resistance and good impact toughness of the titanium alloy. In the present invention, the prefabricated plate is subjected to sintering treatment in step S2, so as to improve the toughness of the prefabricated plate, reduce the brittleness of the prefabricated plate, and prepare for the subsequent rolling and thinning of the prefabricated plate; in addition, during the sintering treatment, aluminum reduces TiO2 to form titanium and a new reinforcing phase Al2O3, and the two enter the matrix to facilitate the subsequent solid solution strengthening and improve the rigidity of the titanium-aluminum-based composite plate; the present invention adopts the step S3 to mold and shape the prefabricated plate; the multi-pass rolling treatment in step S4 is adopted to facilitate the metallurgical bonding between the metals in the prefabricated plate, and improve the rigidity of the titanium-aluminum-based composite plate; Before completing the last rolling pass, the prefabricated plate is also subjected to solution treatment and artificial aging treatment in sequence, wherein the solution treatment is used to facilitate the diffusion of metal elements at the grain boundaries into the matrix to achieve solid solution strengthening; the artificial aging treatment is used to facilitate the precipitation of the second phase, so that a pinning effect is formed between the interior of the grains and the grain boundaries, further improving the rigidity of the titanium-aluminum-based composite plate; the present invention uses multiple rolling passes on the titanium-aluminum-based composite plate in step S4, which is also convenient for thinning to obtain a titanium-aluminum-based composite plate with a thickness of 0.5-1 mm, thereby meeting the requirements of lightweight.

[0021] (2) In step S4, the present invention uses multiple rolling processes for the titanium-aluminum-based composite plate, and controls the rolling temperature to be 450-550°C, so as to soften the prefabricated plate and improve the rolling accuracy; avoid the problems of aluminum alloy oxidation, metal component overburning, roller sticking and energy waste caused by excessively high rolling temperature; in addition, avoid the problem of the prefabricated plate being brittle and rolling cracking caused by excessively low rolling temperature. In step S4, the present invention controls the reduction amount used in each rolling process to be 5-10mm, so as to ensure the rolling accuracy and avoid the problems of rolling deformation and cracking. DETAILED DESCRIPTION

[0022] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0023] Embodiment 1:

[0024] A method for preparing a titanium-aluminum-based composite plate comprises:

[0025] Step S1, mixing metal powder, TiO2 powder and binder in a mass percentage of 79%:20%:1% to form aluminum-based powder, and forming an aluminum substrate by molding; the mass percentages of the metal components in the aluminum substrate are as follows: 1.2% magnesium, 1.0% copper, 0.5% zirconium, 0.5% yttrium, 0.6% titanium and 96.2% aluminum;

[0026] Step S2, pressing the aluminum substrate and the titanium plate after surface etching to form a prefabricated plate, the pressure used during pressing is 200 MPa; sintering the prefabricated plate;

[0027] Step S3, molding and shaping the prefabricated board after sintering;

[0028] Step S4, subjecting the prefabricated plate after molding to multiple rolling processes to obtain a 0.5 mm titanium-aluminum-based composite plate; wherein, before completing the last rolling process, the prefabricated plate is also subjected to solution treatment and artificial aging treatment in sequence, and then, the prefabricated plate is flattened by the last rolling process to obtain a 0.5-1 mm titanium-aluminum-based composite plate.

[0029] In step S1, the metal powder includes aluminum powder; the particle size of the aluminum powder is 20-50 microns; and the particle size of the TiO2 powder is 0.5-2 microns.

[0030] In step S2, the surface etching treatment includes adding nitric acid and ferric chloride to an ammonium bifluoride solution, mixing to form an etching solution, immersing the titanium plate in the etching solution, and etching the surface of the titanium plate for 30 seconds at an etching temperature of 45°C; cleaning and drying the titanium plate after the surface etching treatment.

[0031] The concentration of the ammonium bifluoride solution is 15 g / L; the concentration of the nitric acid is 30 g / L; the concentration of the ferric chloride is 8 g / L; and the titanium plate is a TC4 titanium plate with a thickness of 0.1 mm.

[0032] In step S2, the sintering temperature used in the sintering process is 600° C. and the sintering time is 2 hours.

[0033] In step S3, the molding pressure used in the molding is 160 MPa and the molding temperature is 580°C.

[0034] In step S4, the rolling temperature used in the rolling treatment is 500°C, and the reduction amount used in each rolling treatment is 8 mm; the solution temperature used in the solution treatment is 485°C, and the solution time is 5 hours; the treatment temperature used in the artificial aging treatment is 180°C, and the treatment time is 10 hours.

[0035] Embodiment 2:

[0036] Different from Example 1, the mass percentages of the metal components in the aluminum substrate are as follows: 1.0% magnesium, 0.5% copper, 0.2% zirconium, 0.2% yttrium, 0.5% titanium and 97.6% aluminum.

[0037] Embodiment 3:

[0038] Different from Example 1, the mass percentages of the metal components in the aluminum substrate are as follows: 1.5% magnesium, 1.2% copper, 0.5% zirconium, 0.5% yttrium, 1% titanium and 95.3% aluminum.

[0039] Embodiment 4:

[0040] Different from Example 1, the sintering temperature used in the sintering process is 500°C.

[0041] Embodiment 5:

[0042] Different from Example 1, the sintering temperature used in the sintering process is 680°C.

[0043] Embodiment 6:

[0044] Different from Example 1, the rolling temperature used in the rolling process is 450°C.

[0045] Embodiment 7:

[0046] Different from Example 1, the rolling temperature used in the rolling process is 550°C.

[0047] Comparative Example 1:

[0048] Different from Example 1, the sintering temperature used in the sintering process is 450°C.

[0049] Comparative Example 2:

[0050] Different from Example 1, the sintering temperature used in the sintering process is 780°C.

[0051] Comparative Example 3:

[0052] Different from Example 1, the rolling temperature used in the rolling process is 400°C.

[0053] Comparative Example 4:

[0054] Different from Example 1, the rolling temperature used in the rolling process is 600°C.

[0055] Comparative Example 5:

[0056] Different from Example 1, the surface etching treatment of the titanium plate is eliminated.

[0057] Comparative Example 6:

[0058] The difference from Example 1 is that the metal powder is replaced by ordinary pure aluminum powder.

[0059] The titanium aluminum-based composite plates prepared in Examples 1-7 and Comparative Examples 1-6 were sampled for elastic modulus test, thermal conductivity test and thermal expansion coefficient test. The test results are shown in Table 1. Among them, the test standard adopted by the elastic modulus test method is GB / T 22315-2008: Specifically, a static pull-up test is adopted to measure the deformation and stress of the material, and the elastic modulus is calculated according to Hooke's law, the relationship between stress and strain. The thermal conductivity test method adopts the American Society for Testing and Materials ASTM C518 standard, and the test equipment is a YBF-3 tester. The test standard adopted by the thermal expansion coefficient test method is GB / T 4339 as follows: Specifically, a direct measurement method is adopted, and the expansion rate is directly measured and converted into the thermal expansion coefficient, and the temperature is 25-300°C. The tensile strength test method adopts GBT228.1-2010, Metallic Material Tensile Test Part 1: Room Temperature Test Method.

[0060] Table 1 Performance data of titanium-aluminum based composite sheet

[0061]

[0062]

[0063] From the data in Table 1, we know that:

[0064] In Example 1, a moderate amount of metal components is used for the aluminum substrate to improve the elastic modulus and tensile strength of the titanium-aluminum-based composite plate; in Example 2, a lower amount of metal components is used for the aluminum substrate, so that the elastic modulus and tensile strength of the titanium-aluminum-based composite plate are slightly reduced; in Example 3, a higher amount of metal components is used for the aluminum substrate, so that the elastic modulus and tensile strength of the titanium-aluminum-based composite plate are slightly reduced. This is because the use of more metal components will result in grain boundary enrichment, which in turn reduces the elastic modulus and tensile strength of the titanium-aluminum-based composite plate.

[0065] By comparing Examples 4-5 and Comparative Examples 1-2, it is known that too low a sintering temperature results in insufficient diffusion and sintering of the alloy elements in the prefabricated plate, and too high a sintering temperature results in coarse alloy particles in the prefabricated plate, both of which reduce the elastic modulus and tensile strength of the titanium-aluminum-based composite plate.

[0066] By comparing Examples 6-7 and Comparative Examples 3-4, it is known that using too low a rolling temperature will cause the metal alloy material in the prefabricated plate to not be completely softened, and there is deformation resistance, so that the surface of the titanium-aluminum-based composite plate has defects such as peeling, which affects the performance, thereby reducing the elastic modulus and tensile strength of the titanium-aluminum-based composite plate; using too high a rolling temperature will cause the alloy structure in the prefabricated plate to soften, and the particles to grow, thereby reducing the elastic modulus and tensile strength of the titanium-aluminum-based composite plate;

[0067] By comparing Example 1 and Comparative Example 5, it is known that the titanium plate is subjected to surface etching treatment, so as to form micro-nano-scale holes on the surface of the titanium plate, which not only increases the surface area of ​​the titanium plate, but also provides multiple pressing and embedding points on the titanium plate for pressing the titanium plate and the aluminum substrate, greatly enhancing the firmness of the prefabricated plate formed by pressing between the titanium plate and the aluminum substrate, thereby improving the elastic modulus and tensile strength of the titanium-aluminum-based composite plate;

[0068] By comparing Example 1 and Comparative Example 6, it is known that the use of the specific metal component in Example 1 of the present invention can improve the rigidity and strength of the titanium-aluminum-based composite plate, that is, improve the elastic modulus and tensile strength of the titanium-aluminum-based composite plate;

[0069] As for the thermal conductivity, in Example 3, a higher amount of metal components was used for the aluminum substrate, which resulted in a decrease in the thermal conductivity. The main reason was that the metal components were lattice distorted and enriched at the grain boundaries and in the crystals, which resulted in a decrease in the thermal conductivity.

[0070] As for the thermal expansion coefficient, the same amount of TiO2 powder is used in Examples 1-7 and Comparative Examples 1-5, which can improve the stiffness and strength of the titanium-aluminum-based composite plate, so that there is no significant difference in the thermal expansion coefficient.

[0071] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a titanium-aluminum-based composite sheet, characterized in that: include: Step S1, mixing metal powder, TiO2 powder and binder according to the mass percentage of (79%-95%): (4.5%-20%): (0.5%-1%) to form aluminum-based powder, and forming an aluminum substrate by molding; the mass percentages of the metal components in the aluminum substrate are as follows: magnesium 1.0%-1.5%, copper 0.5%-1.2%, zirconium 0.2%-0.5%, yttrium 0.2%-0.5%, titanium 0.5%-1% and the balance aluminum; Step S2, pressing the aluminum substrate and the titanium plate after surface etching to form a prefabricated plate, and sintering the prefabricated plate; Step S3, molding and shaping the prefabricated board after sintering; Step S4, subjecting the prefabricated plate after molding and shaping to multiple rolling processes to obtain a titanium-aluminum-based composite plate with a thickness of 0.5-1 mm; wherein, before completing the last rolling process, the prefabricated plate is also subjected to solution treatment and artificial aging treatment in sequence, and then, the prefabricated plate is flattened by the last rolling process to obtain a titanium-aluminum-based composite plate with a thickness of 0.5-1 mm.

2. The method for preparing the titanium-aluminum-based composite sheet according to claim 1, characterized in that: In step S1, the metal powder includes aluminum powder; the particle size of the aluminum powder is 20-50 microns.

3. The method for preparing the titanium-aluminum-based composite sheet according to claim 1, characterized in that: The particle size of the TiO2 powder is 0.5-2 microns.

4. The method for preparing the titanium-aluminum-based composite sheet according to claim 1, characterized in that: In step S2, the surface etching treatment includes adding nitric acid and ferric chloride to an ammonium bifluoride solution, mixing to form an etching solution, immersing the titanium plate in the etching solution, and etching the surface of the titanium plate for 30-60 seconds at an etching temperature of 40-50°C; cleaning and drying the titanium plate after the surface etching treatment.

5. The method for preparing the aluminum-based composite plate according to claim 4, characterized in that: The concentration of the ammonium bifluoride solution is 10-20 g / L; the concentration of the nitric acid is 20-50 g / L; the concentration of the ferric chloride is 5-10 g / L; and the titanium plate is a TC4 titanium plate with a thickness of 0.1-0.5 mm.

6. The method for preparing the titanium-aluminum-based composite sheet according to claim 1, characterized in that: In step S2, the sintering process adopts a sintering temperature of 500-680°C and a sintering time of 2-4 hours.

7. The method for preparing the titanium-aluminum-based composite sheet according to claim 1, characterized in that: In step S3, the molding pressure used in the molding is 150-200 MPa and the molding temperature is 500-580°C.

8. The method for preparing the titanium-aluminum-based composite sheet according to claim 1, characterized in that: In step S4, the rolling temperature used in the rolling treatment is 450-550°C, and the reduction amount used in each rolling treatment is 5-10mm; the solution temperature used in the solution treatment is 465-495°C, and the solution time is 2-5h; the treatment temperature used in the artificial aging treatment is 170-190°C, and the treatment time is 5-12h.

9. A titanium-aluminum-based composite sheet, characterized in that: The titanium-aluminum-based composite plate is prepared by the preparation method of any one of claims 1 to 8.

10. An application of a titanium-aluminum-based composite sheet, characterized in that: The titanium-aluminum-based composite plate material as claimed in claim 9 is used to manufacture a heat exchange core plate.

Citation Information

Patent Citations

  • Preparation method of titanium-aluminum layered composite material

    CN112157268A

  • Method for processing titanium-aluminum composite metal sheet

    CN113102541A

  • Preparation method of titanium-steel composite plate based on titanium-aluminum mixed middle layer

    CN114603143A

  • Preparation method of titanium-aluminum composite thin plate

    CN116809680A

  • Display device, data driving circuit and driving method

    KR1020200126656A