Preparation method of water-based environment-friendly UV (ultraviolet) curing bio-based resin for nail polish gel
By introducing the ring-opening reaction and cross-linking network of epoxy soybean oil into polyurethane, the problems of slow curing speed and poor mechanical properties of UV curing polyurethane are solved, and its application performance in fields such as nail polish glue is improved.
Patent Information
- Application Number
- CN202411083335.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The curing speed of existing UV curing polyurethane is slow and has poor mechanical properties, which affects its application in fields such as nail polish.
By conducting ring-opening reaction of epoxy soybean oil with maleate monoester polyetheramine, hydrophilic carboxyl and polyether bonds, polymerization and chain extension reaction with diol and isophorone diisocyanate, forming cross-section Connect the network to improve the hydrophilicity and mechanical properties of polyurethane.
It significantly improves the hydrophilicity and dispersion of polyurethane, shortens the curing time, improves the tensile strength and hardness of the cured substance, improves storage stability, and expands its application prospects in the fields of nail polish glue and coatings.
Smart Images

Figure BDA0004985167540000022 
Figure BDA0004985167540000031 
Figure BDA0004985167540000042
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane, and in particular to a method for preparing a water-based environmentally friendly UV-curable bio-based resin for nail polish. Background Art
[0002] In recent years, with the rapid development of the nail industry, the demand for nail polish has also increased. Nail polish is mainly composed of base resin, photoinitiator, pigment, dye, solvent, etc. Among them, polyurethane has the advantages of high elasticity, good wear resistance, and excellent curing performance. It is widely used in nail polish, coatings, inks and other fields. UV-curable water-based resin has a fast curing speed, convenient construction, and is green and environmentally friendly. It is widely used. Usually, 2,2-dihydroxymethylpropionic acid, 1,2-dihydroxy-3-propanesulfonic acid, etc. are used as water-based chain extenders, and hydroxyethyl acrylate is used as a capping agent. Polymerizable alkenyl functional groups can be introduced at the end of the polyurethane to obtain UV-curable water-based polyurethane resin. However, this UV-curable polyurethane only contains alkenyl groups at the end, and has the disadvantages of low alkenyl conversion rate and slow photocuring speed. In addition, the current UV-curable polyurethane has problems such as poor mechanical properties.
[0003] Epoxidized soybean oil is a bio-based compound that is non-toxic, environmentally friendly, cheap and readily available. It contains multiple epoxy groups, which can generate hydroxyl groups through the epoxy ring-opening reaction, thus being used as a chain extender and having good practical applications in polymer materials such as polyurethane. However, epoxy soybean oil is highly hydrophobic, and adding it to polyurethane will affect the dehydration performance, resulting in poor dispersion of the resin in aqueous media and poor storage stability. It is usually necessary to add additional water-based chain extenders to obtain water-based polyurethane with good dispersion, which can expand the application of polyurethane in nail polish. Practical applications in coatings and other fields Summary of the invention
[0004] The invention solves the problems of slow curing speed and poor mechanical properties of UV-cured polyurethane, and enables polyurethane resin to have better practical applications in the fields of nail polish and the like.
[0005] The technical solution of the present invention is a method for preparing a water-based environmentally friendly UV-curable bio-based resin, characterized in that the preparation method comprises the following steps:
[0006] S1, add epoxidized soybean oil and maleic acid monoester polyetheramine into a reaction bottle, stir to react, and remove low-boiling substances by reduced pressure distillation to obtain maleic acid monoester modified epoxidized soybean oil;
[0007] The structural formula of the maleic acid monoester polyether amine is n=2, 3 or 4.
[0008] S2. In a nitrogen atmosphere, add vacuum-dehydrated diol and isophorone diisocyanate into a reaction bottle to carry out a polymerization reaction, then add acetone, maleic acid monoester-modified epoxy soybean oil, and dibutyltin dilaurate to carry out a chain extension reaction, then add distilled water and triethylamine, stir to neutralize, remove acetone by vacuum distillation, place the solution in a high shear disperser, add a defoamer, a thickener, a dispersant, and a color paste, and shear and disperse to obtain a water-based environmentally friendly UV-curable bio-based resin.
[0009] Among them, the molar ratio of epoxy soybean oil and maleic acid monoester polyetheramine in S1 is 1:(5.6-6.3).
[0010] The reaction in S1 is carried out at 55-70°C for 6-12h.
[0011] Among them, the molar ratio of diol, isophorone diisocyanate, and maleic acid monoester modified epoxy soybean oil in S2 is 1:(2.4-2.8):(0.05-0.015).
[0012] Wherein, the diol includes at least one of polyethylene glycol and polytetramethylene glycol.
[0013] The polymerization reaction in S2 is carried out at 70-80°C for 2-2.5 hours; and the chain extension reaction is carried out at 50-55°C for 30-60 minutes.
[0014] Wherein, the preparation method of maleic acid monoester polyether amine is:
[0015] (1) Add pyridine, Boc-based polyetheramine, and maleic anhydride in a molar ratio of (10-15):1:(1-1.1) to a reaction flask, stir and react at room temperature for 10-18 hours, concentrate the solution, add distilled water and ethyl acetate, concentrate the organic phase after extraction, and dry to obtain maleic acid monoester Boc-based polyetheramine. The reaction formula is:
[0016]
[0017] (2) Add dichloromethane, trifluoroacetic acid in a molar ratio of (40-60):1, and maleic acid monoester boc-based polyetheramine to a reaction flask, stir and react at room temperature for 3-5 hours, concentrate the solution, add saturated sodium bicarbonate solution and ethyl acetate, extract, concentrate the organic phase, and dry to obtain maleic acid monoester polyetheramine.
[0018] The reaction formula is:
[0019]
[0020] Among them, water-based environmentally friendly UV-curable bio-based resin is used in nail polish.
[0021] The technical effect of the present invention is as follows: the present invention utilizes the amino group of maleic acid monoester polyether amine to carry out a ring-opening reaction with the epoxy group of epoxy soybean oil, thereby introducing hydrophilic carboxyl group, polyether bond and imino group into the molecular chain of epoxy soybean oil, and the obtained maleic acid monoester modified epoxy soybean oil has good hydrophilicity. It is further used as a chain extender to carry out polymerization and chain extension reaction with diol and isophorone diisocyanate, thereby introducing carboxyl group and more ether bond hydrophilic groups into polyurethane, significantly improving the hydrophilicity of polyurethane and its nail polish glue product, and improving the dispersibility of polyurethane and nail polish glue products in water and the storage stability of resin.
[0022] The maleic acid monoester modified epoxy soybean oil prepared by the present invention contains a large number of alkenyl groups, which are grafted to the polyurethane molecular chain as a chain extender, thereby introducing a large number of alkenyl groups into the side chain of the polyurethane, accelerating the reaction rate of ultraviolet light curing, improving the conversion rate of alkenyl double bonds, and reducing the curing time.
[0023] When the amino group of the maleic acid monoester polyether amine of the present invention undergoes a ring-opening reaction with the epoxy group of the epoxy soybean oil, the epoxy ring is opened to generate a hydroxyl group, so that the maleic acid monoester modified epoxy soybean oil contains a plurality of hydroxyl groups, and undergoes a cross-linking reaction with the diol and isophorone diisocyanate to form a cross-linking network, and the side chain contains a large number of alkenyl groups, which further undergo a light-emitting cross-linking reaction to form a high-strength and stable double chemical network cross-linking structure, thereby improving the mechanical properties of the resin and the nail polish glue cured product, such as tensile strength and hardness. The polyurethane has a broad application prospect in the fields of nail polish glue, coatings, etc. DETAILED DESCRIPTION
[0024] Example 1
[0025] (1) Add 50 mmol pyridine and 5 mmol 2-[2-(2-T-BOC-aminoethoxy)ethoxy]ethanol (structural formula: CAS No. 139115-92-7), 5.5 mmol maleic anhydride, stirred at room temperature for 12 hours, concentrated the solution, added distilled water and ethyl acetate, extracted, concentrated the organic phase, and dried to obtain maleic acid monoester BOC polyetheramine. The structural formula is:
[0026] (2) Add 25 mL of dichloromethane, 200 mmol of trifluoroacetic acid, and 5 mmol of maleic acid monoester boc-based polyetheramine to the reaction flask, stir and react for 5 h at room temperature, concentrate the solution, add saturated sodium bicarbonate solution and ethyl acetate, concentrate the organic phase after extraction, and dry to obtain maleic acid monoester polyetheramine. The structural formula is:
[0027] (3) Add 2 mmol of epoxidized soybean oil and 12.6 mmol of maleic acid monoester polyetheramine to a reaction flask, raise the temperature to 55° C., stir and react for 12 h, and remove low-boiling substances by vacuum distillation to obtain maleic acid monoester-modified epoxidized soybean oil.
[0028] (4) In a nitrogen atmosphere, 100 mmol of vacuum-dehydrated polyethylene glycol 2000 and 240 mmol of isophorone diisocyanate were added to the reaction bottle, the temperature was raised to 70°C, and the polymerization reaction was carried out for 2.5 hours. Then, 50 mL of acetone, 5 mmol of maleic acid monoester-modified epoxy soybean oil, and 0.4 mmol of dibutyltin dilaurate were added, the temperature was lowered to 55°C, and the chain extension reaction was carried out for 30 minutes. Then, 400 mL of distilled water and triethylamine were added, and the pH of the solution was neutralized to 7 by stirring. The acetone was removed by vacuum distillation, and the solution was placed in a high shear disperser. 0.7 g of defoamer DAPRO DF1760, 8 g of thickener RM2020, 7 g of dispersant RKZ9014, and 35 g of red color paste UR236 were added, and shear dispersion was performed to obtain a water-based environmentally friendly UV-curable bio-based resin.
[0029] Example 2
[0030] (1) Add 75 mmol pyridine and 5 mmol 2-(2-(2-(2-hydroxyethoxy)-ethoxy)ethoxy)ethyl carbamate tert-butyl ester (structural formula: CAS No. 106984-09-2), 5 mmol maleic anhydride, stirred at room temperature for 12 hours, concentrated the solution, added distilled water and ethyl acetate, extracted, concentrated the organic phase, and dried to obtain maleic acid monoester BOC polyetheramine. The structural formula is:
[0031]
[0032] (2) Add 35 mL of dichloromethane, 250 mmol of trifluoroacetic acid, and 5 mmol of maleic acid monoester boc-based polyetheramine to a reaction flask, stir and react at room temperature for 5 hours, concentrate the solution, add saturated sodium bicarbonate solution and ethyl acetate, concentrate the organic phase after extraction, and dry to obtain maleic acid monoester polyetheramine. The structural formula is:
[0033] (3) Add 2 mmol of epoxidized soybean oil and 11.2 mmol of maleic acid monoester polyetheramine to a reaction flask, raise the temperature to 55° C., stir and react for 12 h, and remove low-boiling substances by vacuum distillation to obtain maleic acid monoester-modified epoxidized soybean oil.
[0034] (4) In a nitrogen atmosphere, 100 mmol of vacuum-dehydrated polyethylene glycol 2000 and 250 mmol of isophorone diisocyanate were added to the reaction bottle, the temperature was raised to 70°C, and the polymerization reaction was carried out for 2.5 hours. Then, 60 mL of acetone, 8 mmol of maleic acid monoester-modified epoxy soybean oil, and 0.5 mmol of dibutyltin dilaurate were added, the temperature was lowered to 50°C, and the chain extension reaction was carried out for 60 minutes. Then, 500 mL of distilled water and triethylamine were added, and the pH of the solution was neutralized to 7 by stirring. The acetone was removed by vacuum distillation, and the solution was placed in a high shear disperser. 0.7 g of defoamer DAPRO DF1760, 6.8 g of thickener RM2020, 7 g of dispersant RKZ9014, and 35 g of red color paste UR236 were added, and shear dispersion was performed to obtain a water-based environmentally friendly UV-curable bio-based resin.
[0035] Example 3
[0036] (1) Add 60 mmol pyridine and 5 mmol pentaethylene glycol-tert-butyloxycarbonyl (structural formula: CAS No. 1404111-67-6), 5.5 mmol maleic anhydride, stirred at room temperature for 10 hours, concentrated the solution, added distilled water and ethyl acetate, extracted, concentrated the organic phase, and dried to obtain maleic acid monoester BOC polyetheramine. The structural formula is:
[0037] (2) Add 30 mL of dichloromethane, 220 mmol of trifluoroacetic acid, and 5 mmol of maleic acid monoester boc-based polyetheramine to the reaction flask, stir and react for 3 h at room temperature, concentrate the solution, add saturated sodium bicarbonate solution and ethyl acetate, concentrate the organic phase after extraction, and dry to obtain maleic acid monoester polyetheramine. The structural formula is:
[0038] (3) Add 2 mmol of epoxidized soybean oil and 12.6 mmol of maleic acid monoester polyetheramine to a reaction flask, raise the temperature to 60° C., stir and react for 6 h, and remove low-boiling substances by vacuum distillation to obtain maleic acid monoester-modified epoxidized soybean oil.
[0039] (4) In a nitrogen atmosphere, 100 mmol of vacuum-dehydrated polytetramethylene glycol 2000 and 265 mmol of isophorone diisocyanate were added to a reaction bottle, the temperature was raised to 80°C, and a polymerization reaction was carried out for 2 h. Then, 80 mL of acetone, 12 mmol of maleic acid monoester-modified epoxy soybean oil, and 0.6 mmol of dibutyltin dilaurate were added, the temperature was lowered to 50°C, and a chain extension reaction was carried out for 60 min. Then, 500 mL of distilled water and triethylamine were added, and the pH of the solution was neutralized to 7 by stirring. The acetone was removed by vacuum distillation, and the solution was placed in a high shear disperser. 1.5 g of defoamer DAPRO DF1760, 5.5 g of thickener RM2020, 5.6 g of dispersant RKZ9014, and 23 g of red color paste UR236 were added, and shear dispersion was performed to obtain a water-based environmentally friendly UV-curable bio-based resin.
[0040] Example 4
[0041] (1) Add 50 mmol pyridine and 5 mmol pentaethylene glycol-tert-butyloxycarbonyl (structural formula: CAS No. 1404111-67-6), 5 mmol maleic anhydride, stirred at room temperature for 18 hours, concentrated the solution, added distilled water and ethyl acetate, extracted, concentrated the organic phase, and dried to obtain maleic acid monoester BOC polyetheramine. The structural formula is:
[0042] (2) Add 25 mL of dichloromethane, 200 mmol of trifluoroacetic acid, and 5 mmol of maleic acid monoester boc-based polyetheramine to the reaction flask, stir and react at room temperature for 4 h, concentrate the solution, add saturated sodium bicarbonate solution and ethyl acetate, concentrate the organic phase after extraction, and dry to obtain maleic acid monoester polyetheramine. The structural formula is
[0043] (3) Add 2 mmol of epoxidized soybean oil and 11.5 mmol of maleic acid monoester polyetheramine to a reaction flask, raise the temperature to 70° C., stir and react for 6 h, and remove low-boiling substances by vacuum distillation to obtain maleic acid monoester-modified epoxidized soybean oil.
[0044] (4) In a nitrogen atmosphere, 100 mmol of vacuum-dehydrated polytetramethylene glycol 2000 and 280 mmol of isophorone diisocyanate were added to a reaction bottle, the temperature was raised to 75°C, and a polymerization reaction was carried out for 2 h. Then, 80 mL of acetone, 15 mmol of maleic acid monoester-modified epoxy soybean oil, and 0.6 mmol of dibutyltin dilaurate were added, the temperature was lowered to 55°C, and a chain extension reaction was carried out for 30 min. Then, 500 mL of distilled water and triethylamine were added, and the pH of the solution was neutralized to 7 by stirring. The acetone was removed by vacuum distillation, and the solution was placed in a high shear disperser. 1.3 g of defoamer DAPRO DF1760, 4.5 g of thickener RM2020, 4 g of dispersant RKZ9014, and 15 g of red color paste UR236 were added, and shear dispersion was performed to obtain a water-based environmentally friendly UV-curable bio-based resin.
[0045] Comparative Example 1
[0046] In a nitrogen atmosphere, 100 mmol of vacuum-dehydrated polyethylene glycol 2000 and 240 mmol of isophorone diisocyanate were added to the reaction bottle, the temperature was raised to 70°C, and the polymerization reaction was carried out for 2.5 hours. Then 50 mL of acetone, 5 mmol of 2,2-dihydroxymethylpropionic acid, and 0.4 mmol of dibutyltin dilaurate were added, the temperature was lowered to 55°C, and the chain extension reaction was carried out for 30 minutes. Then 400 mL of distilled water and triethylamine were added, and the pH of the solution was neutralized to 7 by stirring. Finally, 18 mmol of hydroxyethyl acrylate was added, the end-capping reaction was carried out for 3 hours, and the acetone was removed by vacuum distillation. The solution was placed in a high shear disperser, 0.7 g of defoamer DAPRO DF1760, 8 g of thickener RM2020, 7 g of dispersant RKZ9014, and 35 g of red color paste UR236 were added, and shear dispersion was performed to obtain a water-based environmentally friendly UV-curable resin.
[0047] Comparative Example 2
[0048] Epoxidized soybean oil acrylate was prepared according to the method of the literature "Synthesis and Performance Study of Photocurable Waterborne Polyurethane Based on Epoxidized Soybean Oil". 30g of epoxy soybean oil, 0.562g of triphenylphosphine, and 0.112g of inhibitor p-hydroxyanisole were added to the reaction bottle, the temperature was raised to 90°C, 7.494g of acrylic acid was added dropwise, and the temperature was raised to 120°C until the acid value of the reaction system dropped to 5mgKOH / g to obtain epoxy soybean oil acrylate.
[0049] In a nitrogen atmosphere, 100 mmol of vacuum-dehydrated polyethylene glycol 2000 and 240 mmol of isophorone diisocyanate were added to the reaction bottle, the temperature was raised to 70°C, and the polymerization reaction was carried out for 2.5 hours. Then 50 mL of acetone, 5 mmol of epoxy soybean oil acrylate, and 0.4 mmol of dibutyltin dilaurate were added, the temperature was lowered to 55°C, and the chain extension reaction was carried out for 30 minutes. 400 mL of distilled water and triethylamine were added, and the pH of the solution was neutralized to 7 by stirring. The acetone was removed by vacuum distillation, and the solution was placed in a high shear disperser. 0.7 g of defoamer DAPRO DF1760, 8 g of thickener RM2020, 7 g of dispersant RKZ9014, and 35 g of red color paste UR236 were added, and shear dispersion was performed to obtain a water-based environmentally friendly UV-curable bio-based resin.
[0050] The storage stability of UV-curable waterborne bio-based resin was tested according to GB / T 6753.3-1986. The test results are shown in Table 1.
[0051] Table 1 UV curing waterborne bio-based resin performance test
[0052]
[0053]
[0054] As can be seen from Table 1, the storage stability of the UV-curable water-based bio-based resins of Examples 1 to 4 reaches 8-10 months, which is attributed to the use of the amino group of the maleic acid monoester polyether amine and the epoxy group of the epoxy soybean oil to carry out a ring-opening reaction, thereby introducing the hydrophilic carboxyl group, polyether bond and imino group into the molecular chain of the epoxy soybean oil. The obtained maleic acid monoester modified epoxy soybean oil has good hydrophilicity. It is further used as a chain extender to carry out polymerization and chain extension reaction with diols and isophorone diisocyanate, thereby introducing carboxyl groups and more ether bond hydrophilic groups into the polyurethane, significantly improving the hydrophilicity of the polyurethane, and improving the dispersibility of the polyurethane in water and the storage stability of the resin.
[0055] Compared with Example 1, Comparative Example 1 uses conventional 2,2-dimethylolpropionic acid as a chain extender, and the obtained water-based environmentally friendly UV curable resin also has good hydrophilicity, good dispersibility of polyurethane in water, and good storage stability of the resin.
[0056] In Comparative Example 2, conventional epoxy soybean oil acrylate is used as a chain extender, which does not contain hydrophilic carboxyl groups and ether bonds. Epoxidized soybean oil is highly hydrophobic and when grafted to the polyurethane molecular chain, it reduces its hydrophilicity, resulting in poor dispersibility of the polyurethane in water and poor storage stability of the resin.
[0057] Double bond conversion test. The specific method is as follows: Taking Example 1 as an example, in a nitrogen atmosphere, 100 mmol of vacuum dehydrated polyethylene glycol 2000 and 240 mmol of isophorone diisocyanate are added to a reaction bottle, the temperature is raised to 70°C, and a polymerization reaction is carried out for 2.5 hours, then 50 mL of acetone, 5 mmol of maleic acid monoester-modified epoxy soybean oil, and 0.4 mmol of dibutyltin dilaurate are added, the temperature is lowered to 55°C, and a chain extension reaction is carried out for 30 minutes, and then 400 mL of distilled water and triethylamine are added, and the solution is stirred and neutralized to pH 7, acetone is removed by vacuum distillation, and 10.6 g of photoinitiator 1173 is added to obtain a polyurethane resin (without adding defoaming agent, color paste and other additives).
[0058] The polyurethane resin was dropped into 2 clean NaCl salt tablets, dried, and then cured in a 30W UV curing machine for 0-60s at a lighting distance of 15cm. The cured resin was analyzed by infrared spectroscopy to determine the conversion rate of olefinic double bonds.
[0059] Double bond conversion rate = (A0-A t ) / A0×100%; A0 is the infrared spectrum of the resin at 1635cm when it is not irradiated with ultraviolet light. -1 The peak area integration at .
[0060] A t The infrared spectrum of the cured resin at 1635 cm after UV irradiation for t -1 The test results are shown in Table 2.
[0061] Table 2 Polyurethane resin double bond conversion test
[0062]
[0063] As shown in Table 1, the double bond conversion rate of the polyurethane resins of Examples 1 to 4 has reached 78.7-82.0% when the irradiation time is 40s. The higher the double bond conversion rate, the better the curing effect and the faster the curing speed. This is attributed to the fact that the maleic acid monoester modified epoxy soybean oil contains a large number of alkenyl groups, which are grafted to the polyurethane molecular chain as a chain extender, thereby introducing a large number of alkenyl groups into the side chains of the polyurethane, accelerating the reaction rate of ultraviolet light curing, thereby reducing the curing time.
[0064] In Comparative Example 1, no maleic acid monoester-modified epoxy soybean oil was added, and hydroxyethyl acrylate was used as a capping agent. The polyurethane only contained alkenyl groups at the terminal positions, and the main chain of the molecule did not contain alkenyl groups. The reaction rate of UV curing was slow, the double bond conversion rate was low in a short time, and the curing time was long.
[0065] In comparative example 2, conventional epoxy soybean oil acrylate is used as a chain extender, which is grafted onto the polyurethane molecular chain. A large number of olefin groups can also be introduced into the side chain of the polyurethane, which is beneficial to accelerate the reaction rate of UV curing and reduce the curing time.
[0066] Add 0.96g of photoinitiator 1173 to 50mL of water-based environmentally friendly UV curable bio-based resin, stir and mix, pour the solution on the tinplate surface, and cure it in a UV curing machine with a power of 30W for 40s, with a lighting distance of 15cm. Get a cured product. The tensile properties are tested according to the GB / T 528-2009 method. The pencil hardness is tested according to GB / T 6736-2006. The test results are shown in Table 3.
[0067] Table 3 Performance test of cured resin
[0068]
[0069] As shown in Table 3, the tensile strength of the cured resin reaches 26.1-39.0 MPa, and the pencil hardness reaches 4-6H, showing excellent mechanical properties. This is attributed to the ring-opening reaction between the amino group of the maleic acid monoester polyether amine and the epoxy group of the epoxy soybean oil, which generates hydroxyl groups through epoxy ring opening. As a result, the maleic acid monoester modified epoxy soybean oil contains multiple hydroxyl groups, which react with diols and isophorone diisocyanate to form a cross-linked network. At the same time, the side chain contains a large number of alkenyl groups, which further undergoes cross-linking reactions to form a high-strength and stable double chemical network cross-linking structure, thereby improving the tensile strength, hardness and other mechanical properties of the cured resin.
[0070] In Comparative Example 2, acrylic acid is reacted with epoxidized soybean oil. The obtained epoxidized soybean oil acrylate also contains multiple hydroxyl groups, and undergoes cross-linking reaction with diols and isophorone diisocyanate to form a cross-linked network. At the same time, the side chain contains a large number of olefin groups, and further luminescent cross-linking reaction can form a high-strength and stable double chemical network cross-linking structure, without improving the mechanical properties of the resin cured product such as tensile strength and hardness.
Claims
1. A method for preparing a water-based environmentally friendly UV-curable bio-based resin, characterized in that: The preparation method comprises the following steps: S1. Add epoxidized soybean oil and maleic acid monoester polyether amine to a reaction flask, stir to react, and remove low-boiling substances by vacuum distillation to obtain maleic acid monoester-modified epoxidized soybean oil; the structural formula of the maleic acid monoester polyether amine is n = 2, 3 or 4; S2. In a nitrogen atmosphere, add vacuum-dehydrated diol and isophorone diisocyanate into a reaction bottle to carry out a polymerization reaction, then add acetone, maleic acid monoester-modified epoxy soybean oil, and dibutyltin dilaurate to carry out a chain extension reaction, then add distilled water and triethylamine, stir to neutralize, remove acetone by vacuum distillation, place the solution in a high shear disperser, add a defoamer, a thickener, a dispersant, and a color paste, and shear and disperse to obtain a water-based environmentally friendly UV-curable bio-based resin.
2. The method for preparing the water-based environmentally friendly UV-curable bio-based resin according to claim 1, characterized in that: The molar ratio of the epoxidized soybean oil to the maleic acid monoester polyetheramine in S1 is 1:(5.6-6.3).
3. The method for preparing the water-based environmentally friendly UV-curable bio-based resin according to claim 1, characterized in that: The reaction in S1 is carried out at 55-70° C. for 6-12 h.
4. The method for preparing the water-based environmentally friendly UV-curable bio-based resin according to claim 1, characterized in that: The molar ratio of diol, isophorone diisocyanate and maleic acid monoester modified epoxy soybean oil in S2 is 1:(2.4-2.8):(0.05-0.015).
5. The method for preparing the water-based environmentally friendly UV-curable bio-based resin according to claim 4, characterized in that: The diol includes at least one of polyethylene glycol and polytetramethylene glycol.
6. The method for preparing the water-based environmentally friendly UV-curable bio-based resin according to claim 1, characterized in that: The polymerization reaction in S2 is carried out at 70-80° C. for 2-2.5 hours; and the chain extension reaction is carried out at 50-55° C. for 30-60 minutes.
7. The method for preparing the water-based environmentally friendly UV-curable bio-based resin according to claim 1, characterized in that: The preparation method of the maleic acid monoester polyether amine is: (1) Add pyridine, Boc-based polyetheramine and maleic anhydride to a reaction flask, stir and react at room temperature for 10-18 hours, concentrate the solution, concentrate the organic phase after extraction, and dry to obtain maleic acid monoester Boc-based polyetheramine; The structural formula of the Boc-based polyetheramine is n = 2, 3 or 4; (2) Add dichloromethane, trifluoroacetic acid, and maleic acid monoester boc-based polyetheramine to a reaction flask, stir and react at room temperature for 3-5 hours, concentrate the solution, concentrate the organic phase after extraction, and dry to obtain maleic acid monoester polyetheramine.
8. The method for preparing the water-based environmentally friendly UV-curable bio-based resin according to claim 7, characterized in that: The molar ratio of pyridine, Boc-based polyetheramine and maleic anhydride is (10-15):1:(1-1.1).
9. The method for preparing the water-based environmentally friendly UV-curable bio-based resin according to claim 7, characterized in that: The molar ratio of trifluoroacetic acid to maleic acid monoester boc-based polyetheramine is (40-60):
1.
10. Use of the water-based environmentally friendly UV-curable bio-based resin obtained by the preparation method according to any one of claims 1 to 9 in nail polish.
Citation Information
Cited By
Polyurethane resin for nail polish gel and preparation process of polyurethane resin
CN120098228A
A polyurethane resin for nail polish and a preparation process thereof
CN120098228B