TPU (thermoplastic polyurethane) film for solar back panel and preparation method of TPU film

By using polyurethane, polyvinyl fluoride and other materials to prepare TPU films, combined with modified hollow glass microbeads, the problem of insufficient interface bonding power of fluorine-containing materials is solved, the anti-aging and corrosion resistance of the solar backplane film is improved, and the use is extended Lifespan and reduce production costs.

CN118978804AInactive Publication Date: 2024-11-19东莞市华盛新材料有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411279603.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The interface bonding force between fluorine-containing materials and other layers is weak, resulting in the solar backplane film being prone to layering and peeling problems in harsh environments. The existing modification methods and equipment are expensive and complex, making it difficult to adapt to large areas or complex shapes. .

Method used

The TPU film is prepared using polyurethane, polyvinyl fluoride, silicone resin, oleic acid amide, ethylene-vinyl acetate copolymer, titanium dioxide and hollow glass microbeads. By improving the surface energy and intermolecular interaction force, the interface binding force is enhanced , and improve the anti-aging performance and corrosion resistance by modifying hollow glass microbeads.

Benefits of technology

It significantly improves the interface bonding force between the TPU film and other layers, reduces layering and peeling, extends service life, and reduces production costs and operation burden, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005041213260000061
    Figure BDA0005041213260000061
  • Figure BDA0005041213260000091
    Figure BDA0005041213260000091
Patent Text Reader

Abstract

The invention relates to the technical field of solar backboard film processing, in particular to a TPU film for a solar backboard and a preparation method of the TPU film. The TPU film is prepared from the following raw materials in percentage by weight: 40%-50% of polyurethane, 10%-15% of polyvinyl fluoride, 4%-8% of organic silicon resin, 2%-4% of oleamide, 5%-10% of an ethylene-vinyl acetate copolymer, 2%-4% of a compatilizer, 0.5%-1% of an antioxidant, 6%-8% of titanium dioxide and the balance of hollow glass beads. The interface bonding force between the TPU film and other layers is effectively improved, the layering and stripping phenomena in the long-term use process are reduced, and meanwhile the TPU film has good strength, weather resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar backplane film processing, and more specifically, to a TPU film for solar backplane and a preparation method thereof. Background Art

[0002] The solar backplane film is located on the back of the solar panel, and plays the role of protecting the components, isolating water vapor and oxygen, and preventing internal oxidation of the components. Its structure mainly includes a substrate layer, a coating layer, an adhesive layer, a functional layer, and a protective film layer. Among them, the functional layer is set to meet the use needs of the solar backplane film. When it is in the outermost layer, it is in contact with the external environment, so it needs good weather resistance and can resist the influence of harsh environmental factors such as ultraviolet rays, humidity and heat, and extend the service life of the solar backplane film. In order to improve the weather resistance of the functional layer, the weather-resistant layer usually uses fluorine-containing materials, such as polyvinylidene fluoride, polyvinyl fluoride, etc. The reason is that the CF bond energy inside the fluorine-containing material is high, and it has extremely strong anti-aging performance and corrosion resistance stability.

[0003] However, due to the low surface energy characteristics of fluorine-containing materials, the interfacial bonding force between them and other layers is weak, making it difficult to form a good bonding interface. After long-term use, the backplane film will have quality problems such as delamination and peeling, especially in Yunnan, Guizhou, Tibet, Qinghai and Xinjiang. In order to improve the interfacial bonding force between the fluorine-containing weather-resistant layer and other materials, the prior art uses low-temperature plasma treatment, chemical etching and other methods to modify the surface of the fluorine-containing material to increase its surface energy, thereby improving the bonding strength with the adhesive. Among them, low-temperature plasma treatment equipment is usually expensive and requires regular maintenance to ensure its stability and efficiency, increasing production costs and operating burdens. At the same time, when low-temperature plasma treatment is performed on fluorine-containing materials with large areas or complex shapes, there is a problem of uneven treatment. Chemical etching requires precise control of parameters such as the concentration, temperature, and treatment time of the etching solution to ensure the consistency of the treatment effect. The treatment process is complex and difficult to operate. At the same time, the surface quality of the fluorine-containing material may change, such as the surface becoming darker, blacker, or the roughness increases, which will affect the appearance and performance of the product. Summary of the invention

[0004] In order to solve the problem of weak interface bonding between fluorine-containing materials and other materials, the present application provides a TPU film for a solar backplane and a preparation method thereof.

[0005] In a first aspect, the present application provides a TPU film for a solar backsheet, using the following technical solution: A TPU film for a solar backsheet is prepared from the following raw materials in the following weight percentages: Polyurethane 40-50% Polyvinyl fluoride 10-15% Silicone resin 4-8% Oleic acid amide 2-4% Ethylene-vinyl acetate copolymer 5-10% Compatibilizer 2-4% Antioxidants 0.5-1% Titanium dioxide 6-8% The rest is hollow glass beads.

[0006] By adopting the above technical solution, the prepared TPU film for solar backsheet has high surface performance, effectively improves the interface bonding strength between the TPU film and other layers, and reduces the delamination and peeling phenomena during long-term use.

[0007] In this application, a large amount of polyurethane is added because polyurethane has good adhesion and elasticity, which can promote the interface bonding between the weather-resistant layer and other layers. At the same time, the addition of silicone resin and oleic acid amide significantly enhances the interface bonding between the TPU film and other layers by improving the surface energy and enhancing the intermolecular interaction force, and also improves the TPU film's UV resistance, moisture and heat resistance, and corrosion resistance, so that TPU can adapt to more complex environments and extend its service life.

[0008] In this application, polyvinyl fluoride improves the anti-aging performance and corrosion resistance stability of TPU film, and can effectively resist the influence of harsh environmental factors such as ultraviolet rays, humidity and heat, thereby extending the service life of solar backplane film. However, in order to reduce the influence of low surface energy characteristics of fluorine-containing materials in this application, the amount of fluorine-containing materials is reduced, which will lead to a decrease in the anti-aging performance and corrosion resistance stability of TPU film. Titanium dioxide and hollow micro glass beads are added in this application to further improve the anti-aging performance and corrosion resistance stability of TPU film. Titanium dioxide effectively reduces the direct exposure of ultraviolet rays to the substrate through ultraviolet reflection and scattering capabilities, and reduces the rate of photochemical reactions caused by ultraviolet rays. Hollow glass micro beads have excellent acid resistance, alkali resistance and corrosion resistance, and can maintain stable performance in various chemical environments, which can improve the corrosion resistance of TPU film. In a molten state, ethylene-vinyl acetate copolymer penetrates into the tiny pores of adjacent materials to form a stronger physical and chemical bond, making the TPU film structure more stable.

[0009] In addition, the formula in the present application is easy to process and shape, suitable for large-scale production, and has relatively low cost, which reduces production costs and operating burdens.

[0010] Preferably, the number average molecular weight of the polyurethane is 30,000-100,000.

[0011] By adopting the above technical solution, the number average molecular weight of polyurethane is optimized, and the length of the polyurethane molecular chain is moderate, which can better form physical and chemical bonds with other materials and reduce the possibility of stratification and peeling. At the same time, within this range, the processing performance of the TPU film is greatly improved. Too low a molecular weight will cause the material to be too fluid and it will be difficult to control the shape of the TPU; while too high a molecular weight will make the material too hard, increase the difficulty of processing, and affect the quality of the TPU film.

[0012] Preferably, the silicone resin is obtained by mixing vinyl polydimethylsiloxane and polyaryl silicone resin in a weight ratio of (3-5):1.

[0013] By adopting the above technical solution, the weather resistance and corrosion resistance of the TPU film are improved. Vinyl polydimethylsiloxane has good flexibility, high and low temperature resistance and chemical stability, and is not easy to age or deteriorate; polyaryl silicone resin has excellent weather resistance and corrosion resistance, and improves the ability to resist external environmental erosion. The combination of the two can enhance the strength and toughness of the TPU film, and improve the weather resistance and corrosion resistance of the TPU film. At the same time, the mixed use of vinyl polydimethylsiloxane and polyaryl silicone resin can also help improve the interface bonding between the silicone resin layer and other material layers, help reduce the risk of delamination and peeling, and improve the overall stability and durability of the solar backplane TPU film.

[0014] Preferably, the hollow glass microspheres are modified hollow glass microspheres, which are prepared by the following method: 1) placing the hollow glass microspheres in a sodium hydroxide solution, soaking, filtering, rinsing, and drying to obtain hydroxylated hollow glass microspheres; 2) Mixing the hydroxylated hollow glass microspheres and fatty alcohol, heating to 60-80° C., and stirring for 2-3 hours to obtain a primary product; 3) Mixing and stirring the primary product with a silane coupling agent to obtain modified hollow glass microspheres.

[0015] Preferably, the raw materials used to prepare the modified hollow glass microspheres are as follows: Hollow glass beads 20-30 parts 20-30 parts of sodium hydroxide solution 15-20 parts fatty alcohol Silane coupling agent 4-6 parts.

[0016] By adopting the above technical scheme, the stability and compatibility of hollow glass microbeads in TPU film can be improved through hydroxylation, reaction with fatty alcohol and treatment with silane coupling agent, thereby improving the corrosion resistance and mechanical properties of TPU film.

[0017] Hollow glass microspheres have poor miscibility with polyurethane, silicone resin, polyvinyl fluoride and ethylene-vinyl acetate copolymer, resulting in poor uniformity of dispersion in the polyurethane system, affecting the corrosion resistance of the TPU film. Step 1) The hollow glass microspheres are placed in a sodium hydroxide solution and soaked, so that their surface is partially dissolved to form hydroxyl functional groups, which is conducive to subsequent reactions. In 2), the hydroxylated hollow glass microspheres and fatty alcohols are reacted so that the fatty alcohol molecules can be adsorbed on the surface of the hollow glass microspheres, which helps to reduce the agglomeration phenomenon between the microspheres and make the microspheres more evenly distributed in the composite material. In step 3), the interface bonding force between the hollow glass microspheres and polyurethane, silicone resin, polyvinyl fluoride, and ethylene-vinyl acetate copolymer is enhanced, thereby improving the mechanical properties and corrosion resistance of the TPU film.

[0018] Preferably, the mass fraction of the sodium hydroxide solution is 30-50%.

[0019] By adopting the above technical solution, the mass fraction of the sodium hydroxide solution is optimized, which is beneficial to promoting the hydroxylation of the surface of the hollow glass microspheres and is beneficial to subsequent treatment.

[0020] Preferably, the compatibilizer is obtained by mixing maleic anhydride grafted polyethylene resin and ethylene vinyl acetate copolymer grafted maleic anhydride copolymer in a weight ratio of (4-6):3.

[0021] By adopting the above technical scheme, the type and amount of compatibilizer are optimized, the compatibility of polyurethane, silicone resin, polyvinyl fluoride and ethylene-vinyl acetate copolymer is improved, and the components in the TPU film are mixed more evenly, thereby improving the comprehensive properties of the TPU film such as weather resistance, corrosion resistance, and strength. At the same time, the viscosity and internal stress of the blending system during the processing can be reduced, the fluidity and plasticity of the material can be improved, and processing is facilitated.

[0022] Preferably, the ethylene content of the ethylene-vinyl acetate copolymer is 20-40%, and the number average molecular weight is 5000-50000.

[0023] By adopting the above technical solution, the ethylene content and number average molecular weight in the ethylene-vinyl acetate copolymer are optimized, and good mechanical properties such as tensile strength and tear strength are obtained, which is beneficial to improving the mechanical properties of the TPU film. At the same time, within this range, the melt fluidity and processing performance of the ethylene-vinyl acetate copolymer A are good, which is beneficial for the ethylene-vinyl acetate copolymer to be fully mixed and dispersed with other raw materials during the preparation process of the TPU film to form a uniform composite structure, thereby improving the comprehensive performance of the TPU film.

[0024] Preferably, the average particle size of the titanium dioxide is 50-100 nm, and the average particle size of the hollow glass microspheres is 100-200 nm.

[0025] By adopting the above technical scheme, the average particle size of titanium dioxide and hollow glass microspheres is optimized, and the uniform mixing of titanium dioxide and hollow glass microspheres in the TPU film system is promoted, which is beneficial to improving the UV resistance and corrosion resistance of the TPU film, while effectively enhancing the mechanical properties of the TPU film, such as tensile strength, tear strength and hardness, thereby improving the overall performance of the solar backplane film.

[0026] In a second aspect, the present application provides a method for preparing a TPU film for a solar backplane, using the following technical solution: A method for preparing a TPU film for a solar backplane, comprising the following preparation steps: S1, mixing polyurethane, silicone resin, oleic acid amide, ethylene-vinyl acetate copolymer, polyvinyl fluoride, a compatibilizer, an antioxidant, titanium dioxide and hollow glass microspheres to obtain a mixture; S2. The mixture is melted and plasticized, and the well-plasticized melt enters a casting die through a distributor to be extruded to form a TPU film for a solar back panel.

[0027] By adopting the above technical solution, a uniform, dense and smooth TPU film for solar backplane is formed. At the same time, the preparation process is simple, and the operation of each step is highly controllable, which is conducive to realizing automated production and quality control. In addition, the preparation method has low requirements on equipment, which reduces production costs.

[0028] In summary, this application has the following beneficial effects: 1. In the present application, the TPU film for solar backsheet is prepared by mixing polyurethane, polyvinyl fluoride, silicone resin, oleic acid amide, ethylene-vinyl acetate copolymer, compatibilizer, antioxidant, titanium dioxide and hollow glass microspheres to achieve high surface performance, effectively improve the interfacial bonding force between the TPU film and other layers, reduce the delamination and peeling phenomenon during long-term use, and also have good strength, weather resistance and corrosion resistance.

[0029] 2. In the present application, hollow glass microspheres, sodium hydroxide solution, fatty alcohol and silane coupling agent are used to prepare modified hollow glass microspheres, thereby improving the dispersion uniformity and stability of the hollow glass microspheres in the polyurethane, silicone resin, polyvinyl fluoride and ethylene-vinyl acetate copolymer system, thereby improving the corrosion resistance of the TPU film used for the solar back panel and the bonding strength with other layers. DETAILED DESCRIPTION Example

[0030] The thermoplastic polyurethane used in the embodiments is commercially available as polyether polyurethane, with a brand of BASF.

[0031] Vinyl polydimethylsiloxane was purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd. with a CAS number of 53529-60-5.

[0032] The polyaryl silicone resin used in the examples is methylphenyl silicone resin, purchased from Shenzhen Jipeng Silicon Fluoride Materials Co., Ltd., with CAS number 9654315-2012.

[0033] Maleic anhydride grafted polyethylene resin was purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd. with a brand name of ZJ-900E.

[0034] Ethylene vinyl acetate copolymer grafted maleic anhydride copolymer was purchased from Guangzhou Jinkai Chemical Co., Ltd. The brand is DuPont and the model is C250.

[0035] Example 1 A TPU film for a solar back sheet is prepared by the following method: S1, 400 g of polyurethane, 80 g of silicone resin (vinyl polydimethylsiloxane), 40 g of oleamide, 100 g of ethylene-vinyl acetate copolymer, 150 g of polyvinyl fluoride, 40 g of compatibilizer (maleic anhydride grafted polyethylene resin), 10 g of antioxidant (BASF antioxidant 1135), 80 g of titanium dioxide and 100 g of hollow glass microspheres were mixed to obtain a mixture; S2, melting and plasticizing the mixture, and the well-plasticized melt enters a casting die through a distributor to be extruded to form a TPU film for a solar back panel.

[0036] Polyether polyurethane, number average molecular weight is 30,000.

[0037] The ethylene content of the ethylene-vinyl acetate copolymer is 20% and the number average molecular weight is 5000.

[0038] The average particle size of titanium dioxide is 50-70 nm, and the average particle size of the hollow glass microspheres is 100-140 nm.

[0039] The difference between Example 2-3 and Example 1 is that the types, amounts and parameters of the raw materials for preparing the TPU film for the solar backsheet are different. The specific differences are shown in Table 1: Table 1 Types, amounts and parameters of TPU film raw materials for preparing solar backsheets in Examples 1-3 Example 4 A TPU film for a solar back panel. The difference between this embodiment and embodiment 1 is that the silicone resin is obtained by mixing vinyl polydimethylsiloxane and polyaryl silicone resin (methylphenyl silicone resin) in a weight ratio of 3:1.

[0040] Example 5 A TPU film for a solar back panel, the difference between this embodiment and embodiment 1 is that the silicone resin is obtained by mixing vinyl polydimethylsiloxane and polyaryl silicone resin (methylphenyl silicone resin) in a weight ratio of 5:1.

[0041] Example 6 A TPU film for a solar back sheet, the difference between this embodiment and embodiment 1 is that the hollow glass microspheres are modified hollow glass microspheres, which are prepared by the following method: 1) placing 400 g of hollow glass microspheres in 400 g of sodium hydroxide solution, soaking, filtering, rinsing, and drying to obtain hydroxylated hollow glass microspheres; 2) Mix the hydroxylated hollow glass microspheres and 300 g of fatty alcohol, raise the temperature to 60° C., and stir for 2 h to obtain a primary product; 3) The primary product was mixed with 80 g of a silane coupling agent (acetyltrimethoxysilane) to obtain modified hollow glass microspheres.

[0042] Example 7 A TPU film for a solar back sheet, the difference between this embodiment and embodiment 4 is that the hollow glass microspheres are modified hollow glass microspheres, which are prepared by the following method: 1) placing 600 g of hollow glass microspheres in 600 g of sodium hydroxide solution, soaking, filtering, rinsing, and drying to obtain hydroxylated hollow glass microspheres; 2) Mixing hydroxylated hollow glass microspheres and 400 g of fatty alcohol, heating to 80° C., and stirring for 3 h to obtain a primary product; 3) The primary product was mixed with 120 g of a silane coupling agent (3-aminopropyltrimethoxysilane) to obtain modified hollow glass microspheres.

[0043] Example 8 A TPU film for a solar back panel. The difference between this embodiment and embodiment 1 is that the compatibilizer is obtained by mixing maleic anhydride grafted polyethylene resin and ethylene vinyl acetate copolymer grafted maleic anhydride copolymer in a weight ratio of 4:3.

[0044] Example 9 A TPU film for a solar back panel. The difference between this embodiment and embodiment 4 is that the compatibilizer is obtained by mixing maleic anhydride grafted polyethylene resin and ethylene vinyl acetate copolymer grafted maleic anhydride copolymer in a weight ratio of 6:3.

[0045] Example 10 A TPU film for a solar back sheet. The difference between this embodiment and embodiment 1 is that the ethylene content in the ethylene-vinyl acetate copolymer is 20%, and the number average molecular weight is 5000.

[0046] Embodiment 11 A TPU film for a solar back sheet. The difference between this embodiment and embodiment 4 is that the ethylene content in the ethylene-vinyl acetate copolymer is 40%, and the number average molecular weight is 50,000.

[0047] Example 12 A TPU film for a solar back panel. The difference between this embodiment and embodiment 1 is that the average particle size of the titanium dioxide is 50-70 nm, and the average particle size of the hollow glass microspheres is 50-70 nm.

[0048] Example 13 A TPU film for a solar backsheet, this embodiment is different from Embodiment 1 in that the organosilicon resin is a polyaryl organosilicon resin.

[0049] Comparative Example Comparative Example 1 A TPU film for a solar back sheet. The difference between this comparative example and Example 1 is that polyester resin is used instead of silicone resin of equal mass.

[0050] The polyester resin was purchased from Shanghai Kaiyin Chemical Co., Ltd. The brand is Korean SK and the model is SKYGREEN.

[0051] Comparative Example 2 A TPU film for a solar back sheet. The difference between this comparative example and Example 1 is that stearyl glyceryl is used instead of oleic acid amide of the same mass.

[0052] Comparative Example 3 A TPU film for a solar back sheet. The difference between this comparative example and Example 1 is that polyethylene is used instead of ethylene-vinyl acetate copolymer of equal mass.

[0053] The molecular weight of polyethylene is 5000.

[0054] Comparative Example 4 A TPU film for a solar back panel. The difference between this comparative example and Example 1 is that titanium dioxide is replaced with an equal amount of polyvinyl fluoride.

[0055] Comparative Example 5 A TPU film for a solar back sheet. The difference between this comparative example and Example 1 is that the hollow glass microspheres are replaced with an equal amount of polyvinyl fluoride.

[0056] Detection method / test method Tensile strength and elongation at break: The TPU films for solar backsheets prepared in Examples 1-13 and Comparative Examples 1-5 were tested according to GB / T1040-2006.

[0057] A PET film (purchased from Dongguan Wenxuan New Materials Co., Ltd., brand is Yihua Dongli, with a transmittance of 93.4%) was selected as the substrate, and a layer of adhesive (purchased from Shanghai Yujie Chemical Technology Co., Ltd., model is YJ-812) was coated on its surface, and then the TPU films used for solar back panels in Examples 1-13 and Comparative Examples 1-5 were respectively adhered to the surface of the adhesive and cured to obtain samples.

[0058] 180° initial peel force: Each sample was measured according to GB 2792-1998.

[0059] Ultraviolet accelerated aging test: The test samples were placed in an ultraviolet lamp aging test box (model: UVZN-320), and the ultraviolet accelerated aging test (PCT) was performed on the test samples according to the method described in ISO4892.3 "Plastics Laboratory Light Source Exposure Methods Part 3 Fluorescent Ultraviolet Lamps". The test conditions are as follows: light source, UVA is 340; radiation energy, 0.83W / (m2nm); test temperature, 70℃; each light exposure is 4 hours, and the light is turned off for 1 hour, and the cycle test is 50 hours. After the experiment, observe whether there are delamination, bubbling, etc. If not, continue to test the peel strength.

[0060] Wet heat aging treatment test: add the sample to a constant temperature and humidity test box, and conduct the test for 1500 hours at 85℃ and 85% humidity. After the experiment, observe whether there are delamination, bubbling, etc. If not, continue to test the peel strength.

[0061] Corrosion resistance test: Place the sample in an acetic acid aqueous solution with a pH of 3. After 30 days of testing, observe whether there are delamination, bubbling, etc. If not, continue to test the peeling force. The experimental data is shown in Table 2: Table 2 Experimental data of Examples 1-13 and Comparative Examples 1-5 By comparing Example 1 with Comparative Examples 1-3, the tensile strength, elongation at break and peeling force of Comparative Examples 1-3 are all lower than those of Example 1; in the ultraviolet accelerated aging test, bubbles appeared in Comparative Example 1, and the rate of change of the peeling force of Comparative Examples 1-2 was greater than that of Example 1; in the wet heat aging treatment test, bubbles appeared in Comparative Example 3, and the rate of change of the peeling force of Comparative Examples 1-2 was greater than that of Example 1; in the corrosion resistance test, delamination appeared in Comparative Example 2, and the rate of change of the peeling force of Comparative Examples 1 and 2 was greater than that of Example 1; Compared with Example 1 and Comparative Examples 4-5, the tensile strength and elongation at break of Comparative Examples 4-5 are improved, but the peeling force of Comparative Examples 4-5 is greatly reduced; delamination occurs in Comparative Example 4 in the ultraviolet accelerated aging test; delamination occurs in Comparative Example 5 in the wet heat aging treatment test; delamination occurs in Comparative Example 5 in the corrosion resistance test; From the experimental data of Example 1 and Comparative Examples 1-5, the TPU film for solar backsheet prepared by the formula of the present application has good strength, peeling strength, UV resistance, moisture and heat resistance, and corrosion resistance, and can be used for a long time in complex environments.

[0062] Comparing Example 1 with Examples 4-5 and 13, the tensile strength, elongation at break and peel force of Example 4-5 are all higher than those of Example 1, and the tensile strength, elongation at break and peel force of Example 13 are all lower than those of Example 1; after the ultraviolet accelerated aging test, the wet heat aging treatment test and the corrosion resistance test, the change rate of tensile strength, change rate of elongation at break and change rate of peel force of Examples 4-5 are all lower than those of Example 1, and the change rate of tensile strength, change rate of elongation at break and change rate of peel force of Example 13 are all higher than those of Example 1, indicating that the optimization of the type and proportion of silicone resin in the present application is beneficial to improving the tensile strength, elongation at break, peel force, weather resistance and corrosion resistance of the TPU film.

[0063] By comparing Example 1 with Example 6, and Example 4 with Example 7, the tensile strength, elongation at break and peel force of Examples 1 and 7 are all improved; after the ultraviolet accelerated aging test, the wet heat aging treatment test and the corrosion resistance test, the change rate of the tensile strength, the change rate of the elongation at break and the change rate of the peel force of Examples 1 and 7 are all reduced, indicating that the modified hollow glass microspheres prepared in the present application are beneficial to improving the tensile strength, elongation at break, peel force, weather resistance and corrosion resistance of the TPU film.

[0064] Compared with Example 1 and Example 8, and Example 4 and Example 9, the tensile strength, elongation at break and peel force of Examples 1 and 9 are improved; after the ultraviolet accelerated aging test, the wet heat aging treatment test and the corrosion resistance test, the change rate of the tensile strength, the change rate of the elongation at break and the change rate of the peel force of Examples 1 and 9 are reduced, indicating that by optimizing the type and amount of the compatibilizer, it is beneficial to improve the tensile strength, elongation at break, peel force, weather resistance and corrosion resistance of the TPU film.

[0065] Compared with Example 1 and Example 10, and Example 4 and Example 11, the tensile strength, elongation at break and peel force of Examples 1 and 11 are improved; after the ultraviolet accelerated aging test, the wet heat aging treatment test and the corrosion resistance test, the change rate of the tensile strength, the change rate of the elongation at break and the change rate of the peel force of Examples 1 and 11 are reduced, indicating that by optimizing the type and amount of the compatibilizer, it is beneficial to improve the tensile strength, elongation at break, peel force, weather resistance and corrosion resistance of the TPU film.

[0066] Compared with Example 1 and Example 12, the tensile strength, elongation at break and peel force of Example 12 are all reduced; after the ultraviolet accelerated aging test, the wet heat aging treatment test and the corrosion resistance test, the change rate of the tensile strength, the change rate of the elongation at break and the change rate of the peel force of Example 12 are all increased, indicating that optimizing the particle size of titanium dioxide and medium glass beads is beneficial to improving the tensile strength, elongation at break, peel force, weather resistance and corrosion resistance of the TPU film.

[0067] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A TPU film for solar backsheet, It is characterized in that Prepared from the following raw materials in weight percentage: Polyurethane 40-50% Polyvinyl fluoride 10-15% Silicone resin 4-8% Oleic acid amide 2-4% Ethylene-vinyl acetate copolymer 5-10% Compatibilizer 2-4% Antioxidant 0.5-1% Titanium dioxide 6-8% The rest is hollow glass beads.

2. A TPU film for a solar back sheet according to claim 1, Features: The number average molecular weight of the polyurethane is 30,000-100,000.

3. A TPU film for a solar back sheet according to claim 1, Features: The silicone resin is obtained by mixing vinyl polydimethylsiloxane and polyaryl silicone resin in a weight ratio of (3-5):

1.

4. The TPU film for solar backsheet according to claim 1, Features: The hollow glass microspheres are modified hollow glass microspheres, which are prepared by the following method: 1) placing the hollow glass microspheres in a sodium hydroxide solution, soaking, filtering, leaching, and drying to obtain hydroxylated hollow glass microspheres; 2) Mix the hydroxylated hollow glass microspheres and fatty alcohol, raise the temperature to 60-80°C, and stir for 2-3 hours to obtain a primary product; 3) Mixing and stirring the primary product with a silane coupling agent to obtain modified hollow glass microspheres.

5. A TPU film for a solar back sheet according to claim 4, It is characterized in that The raw materials used to prepare the modified hollow glass microspheres are as follows: Hollow glass beads 20-30 parts 20-30 parts of sodium hydroxide solution 15-20 parts fatty alcohol Silane coupling agent 4-6 parts.

6. A TPU film for a solar back sheet according to claim 4, Features: The mass fraction of the sodium hydroxide solution is 30-50%.

7. The TPU film for solar backsheet according to claim 1, Features: The compatibilizer is obtained by mixing maleic anhydride grafted polyethylene resin and ethylene vinyl acetate copolymer grafted maleic anhydride copolymer in a weight ratio of (4-6):

3.

8. The TPU film for solar backsheet according to claim 1, Features: The ethylene content of the ethylene-vinyl acetate copolymer is 20-40%, and the number average molecular weight is 5000-50000.

9. The TPU film for solar backsheet according to claim 1, Features: The average particle size of the titanium dioxide is 50-100 nm, and the average particle size of the hollow glass microspheres is 100-200 nm.

10. A method for preparing a TPU film for a solar backplane according to any one of claims 1 to 9, It is characterized in that The method comprises the following preparation steps: S1, mixing polyurethane, silicone resin, oleic acid amide, ethylene-vinyl acetate copolymer, polyvinyl fluoride, a compatibilizer, an antioxidant, titanium dioxide and hollow glass microspheres to obtain a mixture; S2. The mixture is melted and plasticized, and the well-plasticized melt enters a casting die through a distributor to be extruded to form a TPU film for a solar back panel.

Citation Information

Patent Citations

  • Tri-layer PET (polyethylene glycol terephthalate) film and solar battery backboard constituted by same

    CN104518041A

  • Copper powder-hollow glass microsphere blending modified conductive phenolic resin and preparation method thereof

    CN107177162A

  • AU2003200290A1