High-purity high-aluminum steel and preparation method thereof

By optimizing the deoxygenation, slag-making process and vacuum treatment of high-aluminum steel, the problem of poor cleanliness of metal aluminum oxidation and steel water during smelting is solved, and the preparation of high-purity high-aluminum steel is realized, and the harvest of aluminum elements is improved. rate and productivity.

CN118979191AActive Publication Date: 2024-11-19INST OF RES OF IRON & STEEL JIANGSU PROVINCE +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411477148.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-22
Publication Date
2024-11-19
Estimated Expiration
2044-10-22

AI Technical Summary

Technical Problem

In the field of high-purity high-aluminum steel, the prior art is difficult to effectively control the operability of the smelting process and product performance stability, resulting in serious metal aluminum oxidation, poor cleanliness of molten steel, low production efficiency and high cost.

Method used

By optimizing the design of high-aluminum steel deoxygenation and slag-making processes, LF refining slag system and RH vacuum treatment systems, the oxidation of metal aluminum during smelting process and strengthening the removal of alumina inclusions in the steel water, KR molten pretreatment, Converter smelting, LF refining, RH vacuum treatment and continuous casting process flow, control the vacuum chamber pressure, gas flow and stirring method, and ensure the yield of aluminum elements and the cleanliness of molten steel.

Benefits of technology

The preparation of high-purity high-aluminum steel is achieved, which improves the yield rate of aluminum elements and the cleanliness of molten steel, reduces the production cost and uncertainty of the smelting process, and improves the stability and production efficiency of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_9
    Figure SMS_9
  • Figure SMS_10
    Figure SMS_10
  • Figure SMS_11
    Figure SMS_11
Patent Text Reader

Abstract

The invention relates to high-purity high-aluminum steel and a preparation method thereof, and belongs to the technical field of steelmaking. In chemical components of the high-purity high-aluminum steel, the mass ratio of Al is 0.60%-0.90%, and the mass ratio of S is smaller than or equal to 0.005%. According to the preparation method, production is carried out according to the technological process of KR molten iron pretreatment, converter smelting, converter tapping, LF furnace refining, RH furnace refining and continuous casting, oxidation of metal aluminum in the smelting process is reduced through the measures of optimization design of the high-aluminum steel deoxidation alloying and slagging process, the LF refining slag system, the RH vacuum treatment system and the like, removal of aluminum oxide inclusions in molten steel is enhanced, and the production efficiency is improved. And a high-purity high-aluminum steel product is obtained. And calculating the total amount of the dissolved aluminum to the total addition amount of the metal aluminum according to the content of the metal aluminum in the continuous casting billet, wherein the yield of the obtained metal aluminum element is 85% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to high-purity high-aluminum steel and a preparation method thereof, belonging to the technical field of steelmaking. Background Art

[0002] 10CrMoAl is a seawater corrosion-resistant steel plate, mainly used to manufacture pipelines and structural parts for conveying water, oil, gas, etc., and is widely used in coastal oil fields, power plants, petrochemical natural gas and other fields. Because it serves in the marine environment, the seawater contains a large amount of salt and chlorine and other substances, which are extremely corrosive to it. The aluminum in the material can be oxidized to form a dense aluminum oxide film to prevent material corrosion; the chromium ions and molybdenum ions in the material can automatically fill the gaps formed by pitting corrosion of the steel, forming a dense protective layer to prevent pitting corrosion from developing in depth, further playing a corrosion-resistant role and extending the service life.

[0003] In recent years, with the rapid development of science and technology, people have gradually deepened their development and utilization of the ocean, and the use of seawater corrosion-resistant steel plates has also increased significantly. Since the Al content in corrosion-resistant steel is much higher than that in conventional steel grades, the Al content control stability is poor during the smelting process, resulting in low production efficiency, high cost, and the cleanliness of molten steel cannot be guaranteed.

[0004] The patent application with publication number CN116590619A provides a production method for 10CrMoAl, a seawater corrosion-resistant steel. The key production steps include: converter smelting, LF refining, VD vacuum treatment, continuous casting, rolling, and heat treatment. VD vacuum degassing treatment, vacuuming to below 0.5 torr, vacuum holding time 15 minutes, can control a low gas content. However, the slag-metal reaction during the VD vacuum treatment process is violent, the slag rolls are serious, the metal aluminum yield is poorly stable, and it is difficult to stably control the Al2O3 inclusions in the steel. The cleanliness of the molten steel is poor, and the submerged nozzle in the continuous casting and pouring process has the risk of nodules, which affects the number of continuous casting furnaces and production efficiency.

[0005] The patent application with publication number CN115961118A provides a high-aluminum steel and its preparation method and products, adopting LF refining + continuous casting production process, mainly designed with two-step aluminum addition operation: the first step is to add aluminum to the converter steel for deoxidation and desulfurization; the second step is to add aluminum 3-5 times during the LF refining process, and stir at 500-800NL / min with bottom blowing. The technical problems of large amount of metal aluminum addition and low efficiency in the production process of high-aluminum steel are solved, and high-aluminum molten steel with stable composition is obtained. However, the LF refining process adds aluminum blocks many times and stirs with large bottom blowing, which leads to long refining time and serious oxidation loss of metal aluminum, affecting the cleanliness of molten steel, increasing production costs and reducing production efficiency.

[0006] The patent application with publication number CN116024485A provides a preparation method of high aluminum steel and high aluminum steel, and the production steps include: converter smelting, LF refining, RH vacuum, and continuous casting. The converter is blown for decarburization and dephosphorization, and the molten steel is transported to LF refining after blowing; lime and pre-melted slag are used for slag desulfurization during LF furnace refining; metallic aluminum is added, and lime is added during the melting process of metallic aluminum to reduce the oxidation of molten steel; then the alloyed molten steel is transported to RH vacuum treatment, degassed at the minimum vacuum pressure of 69Pa, and the gas flow rate is increased to accelerate the circulation of molten steel. High aluminum molten steel with P≤0.025%, S≤0.015%, and N≤0.01% is obtained. However, the refining process takes a long time and the amount of metallic aluminum oxidation is large, which is not conducive to the cleanliness of the molten steel; the RH process adopts a large lifting gas flow rate and a low vacuum chamber pressure process, the molten steel stirring intensity is high, the metallic aluminum is easy to gasify, and the decarburization effect of the vacuum furnace net circulation process is not ideal, resulting in poor control of impurity elements such as P, S, and N in the product.

[0007] The patent application with publication number CN116042958A provides a high-efficiency refining preparation method of high-aluminum steel and high-aluminum steel. 0.4-0.6t of aluminum is first added during the converter steelmaking process, and then low-silicon steel hot refined slag, lime and low-silicon pre-melted refined slag are added to the LF refining station to make slag, and then the remaining 9.4-9.6t of aluminum is added for deoxidation and alloying to improve the slag system composition of the ladle slag, which can reduce the secondary oxidation problem of aluminum in the refining process. However, metallic aluminum is also mainly added during the refining process, and the power-on time is long. It relies on bottom blowing stirring and power-on to stir and melt metallic aluminum into molten steel. The metallic aluminum reacts violently with slag and air, resulting in large consumption of metallic aluminum and deterioration of the cleanliness of the molten steel. The molten steel with high aluminum content is then transported to RH deep vacuum treatment. Al is easily gasified under high vacuum conditions, and the difficulty of stable control of Al content in the steelmaking process increases.

[0008] It can be seen that in the field of high-purity high-aluminum steel, there is still an urgent need to propose a method for preparing high-purity high-aluminum steel with high control process operability, stable product performance and stable process. Summary of the invention

[0009] In order to solve the above-mentioned problems, the present invention discloses a high-purity high-aluminum steel and a preparation method thereof. By optimizing the design of the high-aluminum steel deoxidation alloying and slag making process, LF refining slag system, RH vacuum treatment system and other measures, the oxidation of metallic aluminum in the smelting process is reduced, and the removal of alumina inclusions in molten steel is strengthened to obtain a high-purity high-aluminum steel product.

[0010] The specific technical solution is as follows: A method for preparing high-purity high-aluminum steel, which is produced according to the process flow of KR hot metal pretreatment → converter smelting → converter steel tapping → LF furnace refining → RH furnace refining → continuous casting, and the total amount of dissolved aluminum is calculated based on the metal aluminum content in the continuous casting billet to calculate the total amount of metal aluminum added, so that the recovery rate of the metal aluminum element is above 85%, which specifically includes: Step 1: KR hot metal pretreatment, before desulfurization, the chemical composition of hot metal includes by mass percentage: C: 3.8%-4.5%, Si: 0.2%-0.7%, P≤0.12%, S≤0.03%, and the rest is Fe and other inevitable impurities; temperature 1350-1430℃; after desulfurization, the S content of hot metal is ≤0.0030%, and the slag removal rate is ≥95%; Step 2: Converter smelting, using the molten iron and clean scrap steel from step 1, the converter terminal molten steel temperature is 1630-1670°C, the oxygen mass content is 0.045%-0.065%, the S mass content is ≤0.005%, and the slide plate is used to block the slag during the steel tapping process; Step 3: When the converter taps steel, when 30% of the steel is tapped, aluminum ingots, silicon alloys, manganese alloys, and ferrochrome alloys are added to the ladle in sequence for deoxidation and alloying, and the bottom blowing flow rate is 200-300NL / min; when 65%-75% of the steel is tapped, all the alloys are added, and then lime and calcium aluminate are added to synthesize slag to control the slag CaO / Al2O3 ratio of 1.7-2.2. When the tapping is completed, the bottom blowing flow rate is 300-500NL / min, and after stirring for 3-5 minutes, it is transported to the LF for furnace treatment; Step 4: LF furnace refining, the ladle is opened with small and medium bottom blowing argon throughout the whole process, lime, calcium aluminate synthetic slag and alkali metal carbonate are added in the refining process to make slag, the basicity of the final slag is controlled above 20, CaO: 50%-60%, Al2O3: 30%-40%, SiO2≤2%, Na2O: 5%-10%, T.Fe+MnO≤1% in the slag, the refining process is powered on to increase the temperature, and metal aluminum, silicon alloy, manganese alloy, chromium iron alloy are added, and after the composition and temperature of the molten steel are all adjusted to meet the standards, it is transported to the RH for treatment; Step 5: RH furnace refining, the RH furnace vacuum chamber pressure is controlled at 5-50mbar, and the riser gas flow rate of the RH vacuum chamber is 80-120Nm 3 / h, keep for more than 12min, then break the air for calcium treatment, the feeding amount of pure calcium wire is 120-180m / furnace, soft stirring, calming treatment, and then transported to continuous casting; Step 6: Continuous casting, using slab continuous casting machine for casting, protecting the casting throughout the whole process, controlling the superheat of the molten steel in the tundish to 25-35°C, the crystallizer liquid level fluctuation to ±2mm, the crystallizer electromagnetic stirring frequency to 5-10Hz, and the current to 400-600A.

[0011] Furthermore, the clean scrap steel added in the converter smelting in step 2 accounts for 10%-15%, and the components of the clean scrap steel used in the converter include: P mass content ≤0.015%, S mass content ≤0.010%, and the rest are C, Si, Al, Mn, Fe elements, and other inevitable impurity elements, and is equipped with 2.5-3.5 kg / t of ferromolybdenum.

[0012] Furthermore, in step 3, the mass M of the aluminum ingot added to the converter during steel tapping satisfies the following relationship with the converter endpoint: , When the S mass content at the converter end point is greater than or equal to 0.01%: , When the S mass content at the converter end point is less than 0.01%: , Where: w [O] represents the oxygen content of steel tapped from the converter, in ppm; M1 represents the weight of molten steel, in t; w [Al] represents the target Al content, unit: %; Indicates Al yield, unit: %; Δ w [Al] represents the aluminum loss from slag, air, etc., in units of %; λ represents the Al loss coefficient, which is related to the converter end temperature and the end S content; T represents the converter end temperature, in units of K; w [S] represents the S content at the converter end point, in %.

[0013] Furthermore, in step 3, when 30% of the steel is tapped from the converter, aluminum ingots, 70%-85% of the manganese alloy, 70%-85% of the silicon alloy and all of the ferrochrome alloy are added.

[0014] Furthermore, the chemical composition of the aluminum ingot in step 3 includes, by mass percentage: Al≥98%, P≤0.010%, and the rest is Fe and other inevitable impurity components; The chemical composition of manganese alloy includes, by mass percentage: Mn ≥ 98%, P ≤ 0.010%, and the rest is Fe and other inevitable impurity components; The chemical composition of silicon alloy includes by mass percentage: Si: 75%-80%, P≤0.015%, and the rest is Fe and other inevitable impurity components; The chemical composition of ferrochrome alloy includes, by mass percentage: Cr: 55%-65%, P≤0.015%, C: 0.1%-0.5%, and the rest is Fe and other inevitable impurities; The addition amount of calcium aluminate synthetic slag is 7-9kg / t, and the chemical composition by mass percentage includes: CaO: 45%-55%, Al2O3: 30%-40%, SiO2≤5%, and other inevitable components.

[0015] Furthermore, in the step 4, the CaO mass content in the lime added in the LF furnace refining process is ≥95%, and the rest are inevitable impurity components; the amount of calcium aluminate synthetic slag added is 0.5-1kg / t, and the components include by mass percentage: CaO: 45%-55%, Al2O3: 30%-40%, SiO2≤5%, and other inevitable components; the alkali metal carbonate components include by mass percentage: Na2CO3: 60%-70%, CaO: 20%-30%, and other inevitable components.

[0016] Furthermore, after the RH calcium treatment in step 5 is completed, the soft stirring time is ≥10 min, and the sedation time is ≥5 min.

[0017] Furthermore, in step 6, the continuous casting is protected throughout the entire casting process, the argon flow rate of the long water inlet of the large ladle is 150-200NL / min, the argon flow rate of the upper water inlet of the medium ladle is 3-8NL / min, and the argon flow rate of the stopper rod is 5-10NL / min; the tonnage of the continuous casting tundish is ≥45t; the tonnage of the tundish during normal casting is ≥60t; the tonnage of the tundish when continuously casting and changing the large ladle is ≥45t; the insertion depth of the immersion water inlet is 120-180mm, and the continuous casting pulling speed is controlled at 1.2-1.5m / min.

[0018] A high-purity high-aluminum steel is prepared by the above-mentioned preparation method of high-purity high-aluminum steel, and the chemical composition of the high-purity high-aluminum steel includes, by mass percentage: C: 0.06%-0.15%, Si: 0.20%-0.50%, Mn: 0.45%-0.85%, Cr: 0.8%-1.3%, Mo: 0.15%-0.25%, Al: 0.60%-0.90%, S≤0.005%, P≤0.015%, Ni≤0.02%, Cu≤0.015%, TO≤0.0010%, N≤0.0025%, H≤0.0002%, and the rest are Fe and other inevitable impurity components.

[0019] The working principle of the present invention is: In order to reduce the fluctuation of the metal aluminum yield during the high-aluminum steel smelting process and thereby obtain high-aluminum steel products with stable chemical composition and high purity, the smelting process is strictly controlled.

[0020] Firstly, KR is used for deep desulfurization of molten iron, and clean scrap steel is used for converter smelting to obtain low-sulfur molten steel, reducing desulfurization in the LF refining process, that is, avoiding large bottom blowing and stirring, which can reduce the oxidation of metallic aluminum and improve the cleanliness of molten steel.

[0021] Secondly, the slag-blocking operation of the BOF is used to strictly control the slag under the BOF during steel tapping, reduce the oxidizability of the top slag of the ladle, and reduce the oxidation of the aluminum ingots added to the ladle by the slag, thereby affecting the Al element recovery rate and deteriorating the cleanliness of the molten steel. The amount of aluminum ingot added during the BOF steel tapping process is accurately controlled according to the endpoint conditions to improve the Al element recovery rate, so that the generated Al2O3 inclusions can be floated and removed in time. After the alloying is completed, lime and calcium aluminate synthetic slag are added immediately for slag making. The molten steel mixing and stirring during the steel tapping process can be used to quickly make white slag, deoxidize and desulfurize, and adsorb inclusions to improve the cleanliness of the molten steel.

[0022] Thirdly, the LF refining process uses lime and calcium aluminate synthetic slag and alkali metal carbonate low melting point, high basicity calcium aluminate slag system to improve slag fluidity, which is conducive to the adsorption of inclusions and improves the cleanliness of molten steel. In addition, the addition of CO2 gas generated by the decomposition of Na2CO3 is conducive to the foaming of the refined slag, thereby better isolating the air to prevent secondary oxidation of the molten steel and improve the recovery rate of aluminum elements.

[0023] Finally, the minimum vacuum chamber pressure of the RH vacuum treatment process is controlled at 5-50mbar, and the gas flow rate of the riser is reduced, so that the molten steel is circulated for more than 12 minutes, which can ensure that the inclusions in the steel are well removed and reduce the erosion of the RH refractory by the molten steel; it can also avoid the gasification loss of aluminum elements in the steel under high vacuum and improve the recovery rate of aluminum elements. Combined with soft stirring, calming treatment, continuous casting and full protection pouring and other measures, high-purity high-aluminum steel molten steel is obtained.

[0024] The beneficial effects of the present invention are: (1) Use KR to carry out deep desulfurization of molten iron, and combine it with low-sulfur scrap steel for converter smelting to obtain low-sulfur molten steel, reduce the desulfurization in the LF refining process, that is, avoid large bottom blowing and stirring, reduce the oxidation of metallic aluminum, and improve the cleanliness of molten steel.

[0025] (2) High aluminum steel is aluminum deoxidized steel. The LF refining process uses high basicity calcium aluminate refining slag for deoxidation, desulfurization and inclusion adsorption. However, the high basicity slag has a high CaO content, and the refining slag has high viscosity and poor fluidity, which affects the deoxidation, desulfurization and inclusion adsorption effects, and further affects the cleanliness of molten steel. The present invention uses lime, calcium aluminate synthetic slag and alkali metal carbonate to make foam slag, and reduces the melting point of the refining slag, which is not only beneficial to improving the cleanliness of molten steel, but also beneficial to improving the recovery rate of aluminum element.

[0026] (3) The RH high vacuum treatment process does not use extremely low vacuum pressure to treat molten steel. The minimum vacuum pressure is controlled at 5-50 mbar to reduce the gasification loss of aluminum in the molten steel and increase the recovery rate of aluminum. It is combined with soft stirring, calming treatment and other measures to ensure the cleanliness of the molten steel. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0028] The present invention provides a high-purity high-aluminum steel and a preparation method thereof. By optimizing the design of high-aluminum steel deoxidation alloying and slag making processes, LF refining slag system, RH vacuum treatment system and other measures, the oxidation of metal aluminum in the smelting process is reduced, and the removal of aluminum oxide inclusions in molten steel is strengthened, so as to obtain a high-purity high-aluminum steel product.

[0029] Firstly, KR is used for deep desulfurization of molten iron, combined with low-sulfur scrap steel for converter smelting to obtain low-sulfur molten steel, reducing desulfurization in the LF refining process, that is, avoiding large bottom blowing and stirring, which can reduce the oxidation of metallic aluminum and improve the cleanliness of molten steel.

[0030] Secondly, during the steel-making process of the converter, alloys such as metallic aluminum, ferrosilicon, and metallic manganese are added to the molten steel, and the alloys are quickly dissolved into the molten steel by mixed flushing. In the later stage of steel-making, a large amount of lime, synthetic slag, etc. are added to make slag to protect the molten steel from being oxidized by the air, that is, to reduce the oxidation of alloy elements and increase the recovery rate of alloy elements such as metallic aluminum.

[0031] Secondly, the LF refining process produces ultra-high basicity, low-oxidizing calcium aluminate slag, and at the same time adds an appropriate amount of calcium carbonate for slag treatment, which improves the fluidity of the slag, reduces the oxidation of aluminum in the molten steel by the slag, and increases the metallic aluminum recovery rate and the cleanliness of the molten steel.

[0032] Finally, the molten steel is circulated under the conditions of high RH pressure and low lifting gas flow to strengthen the removal of inclusions and reduce the gasification of metallic aluminum. Combined with calcium treatment, soft stirring, calming, continuous casting protection pouring and other measures, the cleanliness of the molten steel is comprehensively improved, the secondary oxidation of metallic aluminum is reduced, and high-quality high-aluminum steel is obtained.

[0033] The specific process is: Step 1: KR molten iron pretreatment, before desulfurization, molten iron C: 3.8%-4.5%, Si: 0.2%-0.7%, P≤0.12%, S≤0.03%, temperature 1350-1430℃; after desulfurization, molten iron S content ≤0.0030%, slag removal rate ≥95%.

[0034] Step 2: Converter smelting, converter scrap ratio 10%-15%, converter scrap steel composition includes: P≤0.015%, S≤0.010%, the rest are conventional C, Si, Al, Mn, Fe elements, and other unavoidable impurity elements, and ferromolybdenum 2.5-3.5kg / t. The converter terminal molten steel temperature is 1630-1670℃, oxygen content is 0.045%-0.065%, S content ≤0.005%, and slide plate is used to block slag during steel tapping.

[0035] Step 3: When the converter is tapped, aluminum ingots, 70%-85% manganese alloy, 70%-85% silicon alloy, and all ferrochrome alloys are added to the ladle in sequence for deoxidation and alloying. The components of the aluminum ingot include Al≥98%, P≤0.010%, and the rest are Fe and other inevitable impurities; the components of the manganese alloy include Mn≥98%, P≤0.010%, and the rest are Fe and other inevitable impurities; the silicon alloy Si: 75%-80%, P≤0.015%, and the rest are Fe and other inevitable impurities; the ferrochrome alloy Cr: 55%-65%, P≤0.015%, C: 0.1%-0.5%, and the rest are Fe and other inevitable impurities; the amount of calcium aluminate synthetic slag added is 7-9kg / t, and the components include CaO: 45%-55%, Al2O3: 30%-40%, SiO2≤5%, and other inevitable components. The bottom blowing flow rate is 200-300NL / min. When 65%-75% of the steel is tapped, all the alloy is added, and then lime and calcium aluminate are added to make slag, and the slag CaO / Al2O3 ratio is controlled to be 1.7-2.2. The bottom blowing flow rate is 300-500NL / min at the end of steel tapping, and after stirring for 3-5 minutes, it is transported to LF for treatment. The mass M of aluminum ingot added to the converter during steel production satisfies the following relationship with the converter end point: , When the S content at the converter end point is higher than 0.01%: , When the S content at the converter end point is less than 0.01%: , Where: w [O] represents the oxygen content of steel tapped from the converter, in ppm; M1 represents the weight of molten steel, in t; w [Al] represents the target Al content, unit: %; Indicates Al yield, unit: %; Δ w [Al] represents the aluminum loss from slag, air, etc., in units of %; λ represents the Al loss coefficient, which is related to the converter end temperature and the end S content; T represents the converter end temperature, in units of K; w[S] represents the S content at the converter end point, in %.

[0036] Step 4: LF furnace refining, the ladle is opened with small and medium bottom blowing argon throughout the whole process, lime (lime CaO ≥ 95%, the rest are inevitable impurities), calcium aluminate synthetic slag (addition amount 0.5-1kg / t, components include CaO: 45%-55%, Al2O3: 30%-40%, SiO2≤5%, and other inevitable components) and alkali metal carbonate slag making, alkali metal carbonate Na2CO3: 60%-70%, CaO: 20%-30%, and other inevitable components. The basicity of the final slag is controlled above 20, CaO: 50%-60%, Al2O3: 30%-40%, SiO2≤2%, Na2O: 5%-10%, T.Fe+MnO≤1% in the slag, the refining process is powered on to increase the temperature, and metal aluminum, silicon alloy, manganese alloy, chromium iron alloy are added. After the molten steel composition and temperature are all adjusted to meet the standards, it is transported to RH for treatment.

[0037] Step 5: RH furnace refining, vacuum chamber pressure is controlled at 5-50mbar, riser gas flow rate is 80-120Nm 3 / h, holding time 12min or more, RH calcium treatment, soft stirring time ≥10min, calming time ≥5min after treatment. Then transport to continuous casting.

[0038] Step 6: Continuous casting, using slab continuous casting machine for pouring, full protection pouring, large ladle long nozzle argon flow rate 150-200NL / min, middle ladle upper nozzle argon flow rate 3-8NL / min, stopper rod argon flow rate 5-10NL / min; continuous casting tundish pouring tonnage ≥45t; normal pouring tundish tonnage ≥60t; continuous casting tundish tonnage ≥45t when changing large ladle; immersion nozzle insertion depth 120-180mm, continuous casting speed controlled at 1.2-1.5m / min. Control the superheat of molten steel in the tundish at 25-35℃, the crystallizer liquid level fluctuation at ±2mm, the crystallizer electromagnetic stirring frequency 5-10Hz, the current 400-600A.

[0039] Several specific embodiments of the present invention are given below: High-purity high-aluminum steel is produced according to the process flow of KR molten iron pretreatment → converter smelting → converter tapping → LF furnace refining → RH furnace refining → continuous casting.

[0040] (1) KR hot metal pretreatment: Before KR desulfurization, the chemical composition of the hot metal, in terms of mass percentage, of C, Si, P, and S, is shown in Table 1. The remainder is Fe and other unavoidable impurities. The hot metal temperature, S content of the hot metal after desulfurization, and slag removal rate are also shown in Table 1.

[0041] Table 1 Hot metal conditions of each heat, S content of hot metal after desulfurization, and slag removal rate

[0042] (2) Converter smelting, the scrap steel ratio added to the converter and the mass content of P and S elements in the clean scrap steel are shown in Table 2. The rest of the scrap steel is C, Si, Al, Mn, Fe, and other unavoidable impurity elements. At the same time, ferromolybdenum is added together with the scrap steel, as shown in Table 2. The final molten steel temperature, oxygen mass content and S mass content of the converter are also shown in Table 2. The sliding plate is used to block the slag during the steel tapping process.

[0043] Table 2 BOF scrap steel, scrap steel ratio and BOF endpoint parameters

[0044] (3) When the converter tapping is 30%, aluminum ingots, part of the manganese alloy, part of the silicon alloy and all of the ferrochrome alloy are added to the ladle in turn for deoxidation and alloying. The appropriate bottom blowing flow rate is controlled for deoxidation and alloying, as shown in Table 3. When the tapping is 65%-75%, all the alloys are added, and then lime and calcium aluminate synthetic slag are added to make slag, and the slag CaO / Al2O3 is controlled. After the tapping is completed, the appropriate bottom blowing flow rate is controlled, and after stirring for a certain period of time, it is transported to the LF for furnace treatment. The detailed parameters are shown in Table 4. The chemical compositions of aluminum ingots, manganese alloys, silicon alloys and ferrochrome alloys are shown in Table 5. The main chemical compositions of calcium aluminate synthetic slag are shown in Table 6.

[0045] Table 3 Deoxidation alloying alloy and bottom blowing flow rate of each furnace

[0046] Table 4 Deoxidation alloying alloy and bottom blowing flow rate of each furnace

[0047] Table 5 Main chemical composition of alloys in each heat

[0048] Table 6 Main chemical components of calcium aluminate synthetic slag

[0049] (4) LF furnace refining, the ladle is opened with small and medium bottom argon blowing throughout the whole process, lime, calcium aluminate synthetic slag and alkali metal carbonate are added during the refining process to make slag, the basicity of the final slag is controlled to be above 20, and the final slag composition is shown in the table; during the refining process, the power is turned on to increase the temperature, and metal aluminum, silicon alloy, manganese alloy and ferrochrome alloy are added. After the molten steel composition and temperature are all adjusted to meet the standards, it is transported to RH for treatment. The chemical composition of alkali metal carbonate, lime and calcium aluminate synthetic slag is shown in the table.

[0050] Table 7 The amount of calcium aluminate synthetic slag added during the refining process and the main chemical composition of the final slag

[0051] Table 8 Main chemical components of synthetic slag of alkali metal carbonate, lime and calcium aluminate

[0052] (5) RH furnace refining, the RH furnace vacuum chamber pressure is controlled at 5-50mbar, and the riser gas flow rate is 80-120Nm 3 / h, holding time is more than 12min, then breaking the air for calcium treatment, the feeding amount of pure calcium wire is 120-180m / furnace, after the treatment, the soft stirring time is ≥10min, the calming time is ≥5min, and then it is transported to continuous casting. The specific parameters of each embodiment are shown in Table 9.

[0053] Table 9 RH vacuum treatment, calcium treatment and soft stirring sedation time

[0054] (6) Continuous casting: slab continuous casting machine is used for casting. The casting is protected throughout the continuous casting process. The long water inlet of the large ladle, the upper water inlet of the middle ladle and the argon flow rate of the stopper are shown in Table 10; the tonnage of the continuous casting tundish, the tonnage of the tundish during normal casting and the tonnage of the tundish when the large ladle is replaced during continuous casting are shown in Table 10; the insertion depth of the immersion water inlet is 120-180mm, and the continuous casting speed is controlled at 1.2-1.5m / min. The superheat of the molten steel in the tundish is controlled at 25-35℃, the fluctuation of the crystallizer liquid level is controlled at ±2mm, the crystallizer electromagnetic stirring frequency is 5-10Hz, and the current is 400-600A.

[0055] Table 10 Argon flow rate of each component and tundish tonnage under various conditions

[0056] Table 11 Continuous casting speed, superheat and other parameters

[0057] (7) The chemical composition of the high aluminum steel produced through the above steps and the aluminum element yield are shown in Table 12. The mechanical properties test results of the steel plate are shown in Table 13.

[0058] Table 12 Chemical composition of high aluminum steel

[0059] Table 12 Chemical composition of high aluminum steel and aluminum recovery rate

[0060] Table 13 Test results of mechanical properties of steel plates

[0061] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing high-purity high-aluminum steel, characterized in that: The production is carried out according to the process flow of KR hot metal pretreatment → converter smelting → converter tapping → LF furnace refining → RH furnace refining → continuous casting. The total amount of dissolved aluminum is calculated based on the content of metallic aluminum in the continuous casting billet and the total amount of metallic aluminum added. The recovery rate of metallic aluminum element is above 85%, which specifically includes: Step 1: KR hot metal pretreatment, before desulfurization, the chemical composition of hot metal includes by mass percentage: C: 3.8%-4.5%, Si: 0.2%-0.7%, P≤0.12%, S≤0.03%, and the rest is Fe and other inevitable impurities; temperature 1350-1430℃; after desulfurization, the S content of hot metal is ≤0.0030%, and the slag removal rate is ≥95%; Step 2: Converter smelting, using the molten iron and clean scrap steel from step 1, the converter terminal molten steel temperature is 1630-1670°C, the oxygen mass content is 0.045%-0.065%, the S mass content is ≤0.005%, and the slide plate is used to block the slag during the steel tapping process; Step 3: When the converter taps steel, when 30% of the steel is tapped, aluminum ingots, silicon alloys, manganese alloys, and ferrochrome alloys are added to the ladle in sequence for deoxidation and alloying, and the bottom blowing flow rate is 200-300NL / min; when 65%-75% of the steel is tapped, all the alloys are added, and then lime and calcium aluminate are added to synthesize slag to control the slag CaO / Al2O3 ratio of 1.7-2.

2. When the tapping is completed, the bottom blowing flow rate is 300-500NL / min, and after stirring for 3-5 minutes, it is transported to the LF for furnace treatment; Step 4: LF furnace refining, the ladle is opened with small and medium bottom blowing argon throughout the whole process, lime, calcium aluminate synthetic slag and alkali metal carbonate are added in the refining process to make slag, the basicity of the final slag is controlled above 20, CaO: 50%-60%, Al2O3: 30%-40%, SiO2≤2%, Na2O: 5%-10%, T.Fe+MnO≤1% in the slag, the refining process is powered on to increase the temperature, and metal aluminum, silicon alloy, manganese alloy, chromium iron alloy are added, and after the composition and temperature of the molten steel are all adjusted to meet the standards, it is transported to the RH for treatment; Step 5: RH furnace refining, the RH furnace vacuum chamber pressure is controlled at 5-50mbar, and the riser gas flow rate of the RH vacuum chamber is 80-120Nm 3 / h, keep for more than 12min, then break the air for calcium treatment, the feeding amount of pure calcium wire is 120-180m / furnace, soft stirring, calming treatment, and then transported to continuous casting; Step 6: Continuous casting, using slab continuous casting machine for casting, protecting the casting throughout the whole process, controlling the superheat of the molten steel in the tundish to 25-35°C, the crystallizer liquid level fluctuation to ±2mm, the crystallizer electromagnetic stirring frequency to 5-10Hz, and the current to 400-600A.

2. The method for preparing high-purity high-aluminum steel according to claim 1, characterized in that: The clean scrap steel added in the converter smelting in step 2 accounts for 10%-15%. The components of the clean scrap steel used in the converter include: P mass content ≤0.015%, S mass content ≤0.010%, and the rest are C, Si, Al, Mn, Fe elements, and other unavoidable impurity elements, and 2.5-3.5 kg / t of ferromolybdenum is also provided.

3. The method for preparing high-purity high-aluminum steel according to claim 1, characterized in that: In step 3, the mass M of aluminum ingot added to the converter for steel production and the converter end point satisfy the following relationship: , When the S mass content at the converter end point is greater than or equal to 0.01%: , When the S mass content at the converter end point is less than 0.01%: , Where: w [O] represents the oxygen content of steel tapped from the converter, in ppm; M1 represents the weight of molten steel, in t; w [Al] represents the target Al content, unit: %; Indicates Al yield, unit: %; Δ w [Al] represents the aluminum loss from slag, air, etc., in units of %; λ represents the Al loss coefficient, which is related to the converter end temperature and the end S content; T represents the converter end temperature, in units of K; w [S] represents the S content at the converter end point, in %.

4. The method for preparing high-purity high-aluminum steel according to claim 1, characterized in that: In step 3, when 30% of the steel is tapped from the converter, aluminum ingots, 70%-85% of the manganese alloy, 70%-85% of the silicon alloy and all of the ferrochrome alloy are added.

5. The method for preparing high-purity high-aluminum steel according to claim 1, characterized in that: The chemical composition of the aluminum ingot in step 3 includes, by mass percentage: Al≥98%, P≤0.010%, and the rest is Fe and other inevitable impurity components; The chemical composition of manganese alloy includes, by mass percentage: Mn ≥ 98%, P ≤ 0.010%, and the rest is Fe and other inevitable impurity components; The chemical composition of silicon alloy includes by mass percentage: Si: 75%-80%, P≤0.015%, and the rest is Fe and other inevitable impurity components; The chemical composition of ferrochrome alloy includes, by mass percentage: Cr: 55%-65%, P≤0.015%, C: 0.1%-0.5%, and the rest is Fe and other inevitable impurities; The addition amount of calcium aluminate synthetic slag is 7-9kg / t, and the chemical composition by mass percentage includes: CaO: 45%-55%, Al2O3: 30%-40%, SiO2≤5%, and other inevitable components.

6. The method for preparing high-purity high-aluminum steel according to claim 1, characterized in that: In the step 4, the CaO mass content in the lime added in the LF furnace refining process is ≥95%, and the rest are inevitable impurity components; the amount of calcium aluminate synthetic slag added is 0.5-1kg / t, and the components include, by mass percentage, CaO: 45%-55%, Al2O3: 30%-40%, SiO2≤5%, and other inevitable components; the alkali metal carbonate components include, by mass percentage, Na2CO3: 60%-70%, CaO: 20%-30%, and other inevitable components.

7. The method for preparing high-purity high-aluminum steel according to claim 1, characterized in that: After the RH calcium treatment in step 5 is completed, the soft stirring time is ≥10 min, and the sedation time is ≥5 min.

8. The method for preparing high-purity high-aluminum steel according to claim 1, characterized in that: In step 6, the continuous casting is protected throughout the casting process, the argon flow rate of the long water inlet of the large ladle is 150-200NL / min, the argon flow rate of the upper water inlet of the medium ladle is 3-8NL / min, and the argon flow rate of the stopper rod is 5-10NL / min; the tonnage of the continuous casting tundish is ≥45t; the tonnage of the tundish during normal casting is ≥60t; the tonnage of the tundish when continuously casting and changing the large ladle is ≥45t; the insertion depth of the immersion water inlet is 120-180mm, and the continuous casting pulling speed is controlled at 1.2-1.5m / min.

9. A high-purity high-aluminum steel, characterized in that: The high-purity high-aluminum steel is prepared by the preparation method of any one of claims 1 to 8, wherein the chemical composition of the high-purity high-aluminum steel includes, by mass percentage: C: 0.06%-0.15%, Si: 0.20%-0.50%, Mn: 0.45%-0.85%, Cr: 0.8%-1.3%, Mo: 0.15%-0.25%, Al: 0.60%-0.90%, S≤0.005%, P≤0.015%, Ni≤0.02%, Cu≤0.015%, TO≤0.0010%, N≤0.0025%, H≤0.0002%, and the rest are Fe and other inevitable impurity components.

Citation Information

Patent Citations

  • High-aluminum steel as well as preparation method and product thereof

    CN115961118A

  • Large-specification seawater-corrosion-resistant high-aluminum steel continuous casting billet and production method thereof

    CN116377335A

  • Corrosion-resistant fatigue spring steel wire, wire rod and production method thereof

    CN116770191A

  • Smelting method for rapid vacuum denitrification of high-aluminum manganese steel

    CN117660728A

  • Smelting process for preparing 38CrMoAlA high-aluminum steel based on ecological electric furnace short process

    CN117758133A