High-temperature-resistant battery and preparation process thereof
By using lithium cobalt oxide electrode, molybdenum disulfide doped graphene electrode, boron nitride composite polyimide separator and optimized electrolyte in lithium batteries, gases caused by nickel and manganese reactions at high temperatures are solved. This has caused problems, achieving stable operation and safety improvement of the battery in the range of 60-100℃, and expanding its application scope.
Patent Information
- Application Number
- CN202411058387.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
Conventional lithium batteries are prone to gases caused by the reaction of nickel and manganese in high temperature environments, resulting in battery performance and safety issues, limiting their application scope.
Using lithium cobalt oxide electrode, molybdenum disulfide doped graphene electrode, boron nitride composite polyimide separator and optimized electrolyte, including fluorovinyl carbonate, vinyl sulfite and lithium hexafluorophosphate, combined with aluminum-plastic film and insulation to ensure the stable operation of the battery within the range of 60-100℃.
It improves the battery's conductivity, lithium storage capacity, structural stability and safety performance, extends the battery's service life, and broadens its application range to high-temperature environment.
Smart Images

Figure BDA0004977084840000091 
Figure BDA0004977084840000101
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium batteries, and more specifically, to a high temperature resistant battery and a preparation process thereof. Background Art
[0002] Lithium batteries, as an important energy storage and power supply technology, have played an indispensable role in modern life. With its high energy density, long life, low self-discharge rate, and no memory effect, it is widely used in mobile phones, laptops, electric vehicles, energy storage systems and other fields.
[0003] The origin of lithium batteries can be traced back to the 1970s, when researchers began to explore the possibility of using lithium metal as the negative electrode of the battery. However, the high activity of lithium metal makes it easy to form lithium dendrites during the charging and discharging process, causing the battery to short-circuit or even catch fire. Therefore, early lithium batteries were not widely used.
[0004] It was not until the 1990s that the emergence of lithium-ion batteries really promoted the development of lithium battery technology. Lithium-ion batteries use embedded compounds as positive and negative electrode materials, avoiding the direct use of lithium metal, thus greatly improving the safety and stability of the battery.
[0005] As lithium batteries become more mature, their application products and scenarios are becoming more and more extensive. Conventional lithium battery products are only suitable for room temperature or -10℃~60℃ ambient temperature range, while many Asian and African regions or automotive products, outdoor products such as solar lamps, and ship transportation may face high-temperature charging and discharging or high-temperature storage environments. Since conventional ternary materials contain nickel and manganese components, these two elements are sensitive and active to moisture and temperature. When the battery is placed in an environment with a temperature exceeding 60℃ for a long time, the electrolyte inside the battery reacts with the nickel and manganese elements of the positive electrode to produce gas, causing the battery to loosen or swell due to gas production, which poses a hidden danger to product performance and safety. Therefore, the development of high-temperature resistant batteries has become a very necessary technical demand and market prospect. Summary of the invention
[0006] In order to solve the above problems, the present application provides a high temperature resistant battery and a preparation process thereof.
[0007] In the first part, the application provides a high temperature resistant battery adopting the following technical solution: A high temperature resistant battery comprises a positive electrode sheet, a negative electrode sheet, a diaphragm, an electrolyte, an aluminum-plastic film, an insulating glue, a positive electrode ear and a negative electrode ear, wherein the positive electrode sheet comprises a lithium cobalt oxide electrode, the negative electrode sheet comprises a molybdenum disulfide-doped graphene electrode, the diaphragm comprises a boron nitride composite polyimide diaphragm, the electrolyte comprises fluoroethylene carbonate, vinyl sulfite and lithium hexafluorophosphate, the positive electrode comprises an aluminum electrode ear, and the negative electrode comprises a nickel electrode ear.
[0008] By adopting the above technical solution, lithium cobalt oxide is relatively more stable. By optimizing the formula of the electrolyte, fluoroethylene carbonate, vinyl sulfite and lithium hexafluorophosphate are used to maintain good ionic conductivity and stability at high temperatures. It is not easy to have problems such as thermal runaway, short circuit or gas generation in a high temperature environment. This makes it difficult for such batteries to produce gas due to chemical reactions when stored in the range of 60-100°C, and the hardness, charge and discharge performance and safety performance of the battery cell are guaranteed.
[0009] MoS2-doped graphene electrodes combine the excellent conductivity of graphene and the excellent lithium storage performance of MoS2, improving the conductivity and lithium storage capacity of the electrode. MoS2-doped graphene electrodes have high structural stability and cycle stability, which helps to reduce the volume expansion and structural damage of electrode materials and extend the service life of the battery. The high thermal stability of boron nitride improves the stability and tolerance of the diaphragm in high temperature environments and reduces the aging and damage of the diaphragm caused by high temperature. Boron nitride composite polyimide diaphragm has good electrolyte barrier properties, which can effectively prevent ion short circuits in the electrolyte and prevent battery overheating.
[0010] This high temperature resistant battery solution enables the battery to be used in a wider range of ambient temperatures, and is particularly suitable for high temperature environments such as Asia and Africa, automotive products, outdoor products such as solar lamps, and ship transportation. This will greatly broaden the application range of the battery.
[0011] Optionally, the preparation method of the boron nitride composite polyimide diaphragm is: A1. Disperse 50-100 parts of nano boron nitride by weight in 150-200 parts of acetone, add 180-200 parts of diamine monomer and 200-220 parts of anhydride monomer, stir evenly, pressurize at 1-3atm at 50-90°C, and use infrared radiation for in-situ polymerization to obtain a precursor solution; A2. Coat the precursor solution on a glass substrate with a gap of 20-60 μm using an automatic doctor blade coater, transfer the coated glass substrate to a vacuum drying oven, heat it to 250-300°C at a rate of 5-15°C / min at room temperature of 25°C, and keep it warm for 2-4 hours to obtain a boron nitride composite polyimide diaphragm.
[0012] By adopting the above technical scheme, the preparation method comprehensively uses the steps of dispersion mixing, in-situ polymerization, coating and drying, effectively realizing the preparation of boron nitride composite polyimide diaphragm, and has good process controllability and stability.
[0013] Optionally, the nano boron nitride needs to be surface modified before step A1, and the surface modification method is: B1. Mix the dried nano boron nitride with a sodium hydroxide solution having a mass concentration of 10-15% in a mass ratio of 1:(2-3), and react the boron nitride nanosheets with the sodium hydroxide solution for 1-3 hours under continuous stirring at 20-50 r / min; B2, separating the reacted nano boron nitride from the sodium hydroxide solution by centrifugation, washing with deionized water and then vacuum drying to obtain surface hydroxylated nano boron nitride; B3, mixing and stirring the surface hydroxylated nano boron nitride with toluene to form a uniform dispersion, adding diisocyanate to the dispersion, the mass ratio of diisocyanate to nano boron nitride being (1-5):1, stirring and reacting at 40-80° C. for 4-8 hours, so that the diisocyanate and the hydroxyl groups on the surface of the boron nitride nanosheets undergo a covalent grafting reaction; B4. Separate the reacted nano-boron nitride from the solution by centrifugal filtration, wash with deionized water, and vacuum dry after washing to obtain surface-modified nano-boron nitride.
[0014] By adopting the above technical scheme, the surface of nano-boron nitride is modified by sodium hydroxide solution, and the hydroxylation reaction is introduced, which helps to improve the hydrophilicity and surface activity of nano-boron nitride. Through centrifugal separation and deionized water washing, the surface hydroxylated nano-boron nitride is effectively separated, and the residual sodium hydroxide solution is removed to ensure the purity and stability of the surface-modified nano-boron nitride. The diisocyanate undergoes a covalent grafting reaction with the hydroxylated nano-boron nitride, which improves the surface chemical properties of the nano-boron nitride and enhances its compatibility with the polyimide monomer, which is beneficial to the subsequent preparation and performance improvement of the diaphragm.
[0015] Optionally, the nano boron nitride is selected from hexagonal boron nitride or cubic boron nitride.
[0016] By adopting the above technical solution, hexagonal boron nitride has high thermal conductivity and thermal stability, which helps to improve the thermal conductivity of battery separators and improve the heat dissipation effect of batteries at high temperatures. In addition, hexagonal boron nitride can provide better surface flatness and chemical reaction activity, which helps to improve the surface properties and stability of the separator and improve the stability and tolerance of the battery in high temperature environments.
[0017] Cubic boron nitride has high hardness and chemical stability, which helps to improve the wear resistance and chemical stability of the diaphragm, protect the structural integrity of the battery at high temperatures, provide better protection, effectively prevent the external environment from corroding and damaging the battery, and improve the safety and stability of the battery in high temperature environments.
[0018] Optionally, the electrolyte further comprises nano silicon carbide, 1-ethyl-3-methylimidazolium tetrafluoroborate and benzotriazole, and the mass ratio of the nano silicon carbide, 1-ethyl-3-methylimidazolium tetrafluoroborate, benzotriazole and fluoroethylene carbonate is (1-2):(2-3):1:6.
[0019] By adopting the above technical solutions, nano silicon carbide can improve the conductivity of the electrolyte, promote ion transmission, and help improve the charging and discharging efficiency of the battery. Nano silicon carbide has high chemical stability, which helps to improve the cycle stability and durability of the battery. 1-Ethyl-3-methylimidazolium tetrafluoroborate can improve the ion conductivity of the electrolyte, which helps to improve the performance and response speed of the battery. The ionic liquid has good thermal stability and chemical stability, which helps to improve the stability and safety of the battery in a high temperature environment. Benzotriazole effectively inhibits the oxidation reaction in the electrolyte, prolongs the cycle life of the battery, improves the stability of the electrolyte, reduces the oxidation rate of the battery in a high temperature environment, and improves the safety of the battery.
[0020] Optionally, the specific preparation steps of the molybdenum disulfide doped graphene electrode are: C1. Mixing nano-molybdenum disulfide and graphene powder in a mass ratio of (1-3):10, and mixing by high-speed mechanical mixing at 2000-2500 r / min to obtain a mixed powder; C2, placing the mixed powder in a high temperature furnace, performing heat treatment under an inert atmosphere, the heat treatment temperature being 800-1000° C., and cooling to room temperature after the heat treatment to obtain molybdenum disulfide-doped graphene; C3, mixing molybdenum disulfide-doped graphene with carbon black, polytetrafluoroethylene, and ethanol in a mass ratio of 8:(1-3):(0.5-1.5):8, stirring to prepare a uniform electrode material slurry, and coating the electrode material slurry on a glass fiber board to form a uniform electrode film; C4, placing the coated electrode film in a vacuum drying oven for drying to remove the solvent and fix the electrode material on the substrate; C5. Place the dried electrode film into a hot press for hot pressing at a pressure of 0.5-1.5 MPa and a temperature of 120-160°C. After separating the electrode film from the substrate, a molybdenum disulfide-doped graphene electrode is obtained.
[0021] By adopting the above technical solutions, high-speed mechanical mixing can help to fully mix nano-molybdenum disulfide and graphene powder, thereby improving the uniformity of the material. High-temperature heat treatment helps the interaction and doping of molybdenum disulfide and graphene, thereby improving the performance of the material. Heat treatment helps to improve the stability and structural integrity of the material. The addition of carbon black, polytetrafluoroethylene, etc. helps to improve the adhesion and conductivity of the electrode material and improve the electrode performance. Drying and hot pressing can help to fix the electrode material on the substrate, thereby improving the stability and contact performance of the electrode. Hot pressing can regulate the morphology and structure of the electrode film, thereby improving the conductivity and charge-discharge performance of the electrode.
[0022] In a second aspect, the present application provides a preparation process of a high temperature resistant battery, which adopts the following technical solution: A preparation process of a high temperature resistant battery comprises the following steps: S1. Weld the positive electrode tab to the positive electrode sheet by ultrasonic welding, and weld the negative electrode tab to the negative electrode sheet; S2. Arrange the positive and negative electrode sheets and the separator neatly in the order of positive electrode sheet - separator - negative electrode sheet - separator, and wind the arranged positive and negative electrode sheets and the separator by a winding machine, and obtain the battery cell after the winding is completed; S3, baking the battery cell in a high vacuum oven to remove moisture from the core; S4. After baking, the electrolyte is injected into the battery cell, and the battery cell is encapsulated with an aluminum-plastic film. In addition, insulating glue is used to insulate and seal the connection between the battery cell and the positive and negative pole ears to obtain a high temperature resistant battery.
[0023] By adopting the above technical solution, the positive and negative electrode sheets and separators are neatly arranged and wound by a winding machine, which helps to maintain the uniformity and stability of the battery structure. The winding process can effectively utilize space, improve the energy density of the battery, and achieve a higher performance battery design. Removing internal moisture helps to reduce the humidity inside the battery, improve the stability and cycle life of the battery, and reduce the risk of electrolyte loss in the electrolyte and internal short circuit of the battery. The use of aluminum-plastic film for packaging can effectively protect the battery and reduce the impact of the external environment on the battery. The use of insulating glue can effectively isolate the positive and negative ears, improve the safety of the battery, and prevent short circuits and leakage.
[0024] Optionally, the separator is 1.5-2.5 mm wider than the negative electrode sheet, and the negative electrode sheet is 1-2 mm wider than the positive electrode sheet.
[0025] By adopting the above technical solution and increasing the width of the diaphragm, direct contact between the negative electrode and the positive electrode can be effectively prevented, the risk of short circuit can be reduced, and the safety of the battery can be improved. The increase in the width of the diaphragm can increase the diffusion path of the electrolyte between the positive and negative electrode sheets, which helps to improve the diffusion uniformity of the electrolyte and improve the performance stability of the battery. The negative electrode sheet is slightly wider than the positive electrode sheet, which helps to balance the current distribution between the positive and negative electrodes, reduce the difference in current density, and improve the charge and discharge efficiency and cycle life of the battery.
[0026] Optionally, the high vacuum oven maintains a vacuum degree of (-95%)-(-99%) and a temperature of 80°C±0.5°C when drying the battery cells.
[0027] By adopting the above technical solution, the high vacuum oven can maintain a good vacuum degree and precise temperature control, which can effectively remove the moisture and gas inside the battery cell and ensure the stability and safety of the battery cell during the drying process. The precisely controlled temperature helps to improve the drying efficiency, avoid the impact of overheating on the battery cell materials, and ensure the quality and performance of the battery cell.
[0028] In summary, this application has the following beneficial effects: 1. Due to the high energy density and stability of the lithium cobalt oxide electrode used in this application, the energy density and cycle life of the battery are improved; the molybdenum disulfide doped graphene electrode enhances the conductivity and high temperature resistance of the battery; the boron nitride composite polyimide diaphragm ensures the safety and stability of the battery at high temperatures with its high thermal stability and barrier properties; and the optimized electrolyte improves the high temperature resistance and charge transfer rate of the battery. In addition, the stable connection of the positive and negative ears further enhances the performance and safety of the battery. In summary, the high temperature resistant battery realizes efficient, stable and safe operation of the battery in a high temperature environment, providing a reliable energy solution for high temperature application scenarios.
[0029] 2. The preferred introduction of nano silicon carbide in this application improves the conductivity and chemical stability of the electrolyte, thereby enhancing the charge and discharge efficiency, cycle stability and durability of the battery. At the same time, the application of 1-ethyl-3-methylimidazolium tetrafluoroborate ionic liquid significantly improves the ionic conductivity of the electrolyte, ensuring the excellent performance and safety of the battery in a high temperature environment. In addition, the addition of benzotriazole effectively inhibits the oxidation reaction in the electrolyte, further prolongs the cycle life of the battery and improves its overall stability. The combined application of these technologies enables the battery to perform well in a high temperature environment, providing an efficient and safe energy solution for various high temperature application scenarios.
[0030] 3. The method of the present application uses a winding machine to wind the positive and negative electrodes and the separator in an orderly manner, ensuring the uniformity and stability of the battery structure and improving the energy density of the battery. At the same time, removing internal moisture enhances the stability and cycle life of the battery and reduces the risk of electrolyte loss and internal short circuit. The use of aluminum-plastic film packaging and insulating glue further protects the battery and improves the safety of the battery. These processes and technical measures jointly optimize the performance of the battery and ensure its stable and reliable operation in various application scenarios. DETAILED DESCRIPTION
[0031] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.
[0032] Lithium cobalt oxide electrode materials and nano-silicon carbide are purchased from Wuhan Szhuanke Biotechnology Co., Ltd., with an active ingredient content of ≥99%; fluoroethylene carbonate is purchased from Shandong Shengcang Chemical Technology Co., Ltd., with a purity of ≥99%; vinyl sulfite is purchased from Shanghai Zhuoli Materials Co., Ltd., with a purity of ≥99%; lithium hexafluorophosphate is purchased from Shanghai McLean Biochemical Technology Co., Ltd., with a purity of ≥99.5%; 1-ethyl-3-methylimidazole tetrafluoroborate is purchased from Hubei Wei's Reagent, with a purity of >95%; benzotriazole is purchased from Shandong Qiansheng Chemical Co., Ltd., with an active ingredient content of >99%; the positive and negative ears are purchased from Shenzhen Liyou New Energy Technology Co., Ltd.; and the aluminum-plastic film is purchased from Boxiang Optical Materials Co., Ltd.
[0033] Preparation example of boron nitride composite polyimide diaphragm Preparation Example 1 Preparation method of boron nitride composite polyimide diaphragm: A1. Disperse 8 kg of nano hexagonal boron nitride in 18 kg of acetone, add 19 kg of 4,4'-diaminodiphenyl ether and 21 kg of pyromellitic anhydride, stir evenly with a magnetic stirrer, pressurize at 2 atm at 70 ° C, and irradiate the mixture with 1500 W of infrared radiation for 1.5 h to perform in-situ polymerization to obtain a precursor solution; A2. The precursor solution is coated on a glass substrate with a gap of 40 μm ± 5 μm by an automatic scraper coater, and the coated glass substrate is transferred to a vacuum drying oven, and the temperature is increased to 280°C at a rate of 10°C / min at room temperature of 25°C, and kept warm for 3 hours to obtain a boron nitride composite polyimide diaphragm.
[0034] Preparation Example 2 Preparation method of boron nitride composite polyimide diaphragm: The difference from Preparation Example 1 is that in step A1, 5 kg of nano hexagonal boron nitride is dispersed in 18 kg of acetone.
[0035] Preparation Example 3 Preparation method of boron nitride composite polyimide diaphragm: The difference from Preparation Example 1 is that in step A1, 10 kg of nano hexagonal boron nitride is dispersed in 15-20 kg of acetone.
[0036] Preparation Example 4 Preparation method of boron nitride composite polyimide diaphragm: A1. 8 kg of dried nano hexagonal boron nitride was mixed with 16-24 kg of sodium hydroxide solution with a mass concentration of 12%. The nano hexagonal boron nitride and the sodium hydroxide solution were reacted for 2 hours under the condition of continuous stirring at 40 r / min. After the reaction was completed, the nano hexagonal boron nitride after the reaction was separated from the sodium hydroxide solution by a centrifuge, washed with deionized water and then vacuum dried to obtain surface hydroxylated nano boron nitride. The surface hydroxylated nano boron nitride was mixed with 5 kg of toluene and stirred to form a uniform dispersion. 8-40 kg of diisocyanate was added to the dispersion, stirred and reacted at 40-80° C. for 4-8 hours to cause the diisocyanate to covalently graft with the hydroxyl groups on the surface of the boron nitride nanosheets. The nano boron nitride after the reaction was separated from the solution by centrifugal filtration, washed with deionized water, and vacuum dried after washing to obtain surface-modified nano boron nitride. A2, dispersing the surface-modified nano-boron nitride in 18 kg of acetone, adding 19 kg of 4,4'-diaminodiphenyl ether and 21 kg of pyromellitic anhydride, stirring evenly with a magnetic stirrer, pressurizing at 2 atm at 70 ° C, and irradiating the mixed solution with 1500 W of infrared radiation for 1.5 hours to perform in-situ polymerization to obtain a precursor solution; A3. Coat the precursor solution on the glass substrate with a gap of 40 μm ± 5 μm by an automatic scraper coater, transfer the coated glass substrate to a vacuum drying oven, heat it to 280°C at a rate of 10°C / min at room temperature of 25°C, and keep it warm for 3 hours to obtain a boron nitride composite polyimide diaphragm.
[0037] Preparation Example 5 The preparation method of boron nitride composite polyimide diaphragm is different from that of Preparation Example 1 in that cubic boron nitride is used as nano boron nitride.
[0038] Preparation example of MoS2-doped graphene electrode Preparation Example 6 The specific preparation steps of MoS2-doped graphene electrode are as follows: C1. 2 kg of nano-molybdenum disulfide and 10 kg of graphene powder were mixed in a container, and mechanically mixed by a high-speed stirrer at 2200 r / min to obtain a mixed powder; C2, placing the mixed powder in a high temperature furnace, and performing heat treatment in a helium atmosphere at a temperature of 900° C. After the heat treatment is completed, cooling to room temperature is performed to obtain molybdenum disulfide-doped graphene; C3, mixing molybdenum disulfide-doped graphene with carbon black, polytetrafluoroethylene, and ethanol in a mass ratio of 8:(1-3):(0.5-1.5):8, preparing a uniform electrode material slurry by magnetic stirring, and coating the electrode material slurry on a glass fiber board with a gap of 20 μm±5 μm by an automatic doctor blade coater to form a uniform electrode film; C4, placing the coated electrode film in a vacuum drying oven for drying to remove the solvent and fix the electrode material on the substrate; C5. Place the dried electrode film into a hot press for hot pressing at a pressure of 1 MPa and a temperature of 140°C. After separating the electrode film from the substrate, a molybdenum disulfide-doped graphene electrode is obtained.
[0039] Preparation Example 7 Preparation method of molybdenum disulfide doped graphene electrode: The difference from Preparation Example 5 is that 1 kg of nano molybdenum disulfide, 10 kg of graphene powder, 2.75 kg of carbon black, 1.35 kg of polytetrafluoroethylene, and 11 kg of ethanol are used.
[0040] Preparation Example 8 Preparation method of molybdenum disulfide doped graphene electrode: The difference from Preparation Example 5 is that 3 kg of nano molybdenum disulfide, 10 kg of graphene powder, 3.25 kg of carbon black, 1.625 kg of polytetrafluoroethylene, and 13 kg of ethanol are used.
[0041] Preparation Example 9 Preparation method of molybdenum disulfide doped graphene electrode: The difference from Preparation Example 5 is that step C5 is not performed. Example
[0042] Example 1 A preparation process of a high temperature resistant battery: S1. Mix 1kg of polyvinylidene fluoride with 4kg of lithium cobalt oxide powder and coat it on the substrate with a coating thickness of 40-60μm. After drying, obtain the lithium cobalt oxide electrode, prepare the positive and negative electrode ears and the positive and negative electrode sheets, align the aluminum electrode ear with the welding point of the lithium cobalt oxide electrode, align the nickel electrode ear with the welding point of the molybdenum disulfide doped graphene electrode, start the ultrasonic welding equipment to weld the positive and negative electrode ears to the positive and negative electrode sheets.
[0043] S2. Cut the welded positive electrode sheet, negative electrode sheet and boron nitride composite polyimide separator into pieces with a length of 1 m and a width of 0.2 m, and arrange them neatly in the feeding area of the winding machine in the order of positive electrode sheet - separator - negative electrode sheet - separator. Start the winding machine, and after the winding is completed, obtain the battery cell.
[0044] S3. Place the battery cell in a high vacuum oven, start the vacuum pump, maintain the vacuum degree at (-95%) - (-99%), and the temperature at 80℃±0.5℃, bake for 3 hours. After baking, turn off the heating system and let the oven cool naturally to room temperature.
[0045] S4. Mix 600g of fluoroethylene carbonate, 200g of ethylene sulfite and 200g of lithium hexafluorophosphate and disperse them by 48KHz ultrasonic dispersion to obtain an electrolyte. Slowly inject the electrolyte into the battery cell to prevent the electrolyte from overflowing. Put the battery cell injected with electrolyte into the aluminum-plastic film and use a heat sealer to heat seal the aluminum-plastic film to ensure that the battery cell is completely sealed. Apply 20g of insulating glue at the connection between the battery cell and the positive and negative ears respectively.
[0046] Among them, the boron nitride composite polyimide membrane is prepared by Preparation Example 1, and the molybdenum disulfide doped graphene electrode is prepared by Preparation Example 6.
[0047] Example 2 A preparation process for a high temperature resistant battery: The difference from Example 1 is that in step S4, 600 g of fluoroethylene carbonate, 200 g of ethylene sulfite, 200 g of lithium hexafluorophosphate, 150 g of nano-silicon carbide, 250 g of 1-ethyl-3-methylimidazolium tetrafluoroborate, and 100 g of benzotriazole are mixed and dispersed by 48 KHz ultrasound to obtain an electrolyte.
[0048] Example 3 A preparation process for a high temperature resistant battery: The difference from Example 2 is that in step S2, the negative electrode sheet is cut to a length of 1 m and a width of 0.2 m, the separator is 1.5-2.5 mm wider than the negative electrode sheet, and the negative electrode sheet is 1-2 mm wider than the positive electrode sheet.
[0049] Example 4 A preparation process for a high temperature resistant battery: The difference from Example 1 is that the boron nitride composite polyimide diaphragm is prepared by Preparation Example 2.
[0050] Example 5 A preparation process for a high temperature resistant battery: The difference from Example 1 is that the boron nitride composite polyimide separator is prepared by Preparation Example 3.
[0051] Example 6 A preparation process for a high temperature resistant battery: The difference from Example 1 is that the boron nitride composite polyimide separator is prepared by Preparation Example 4.
[0052] Example 7 A preparation process for a high temperature resistant battery: The difference from Example 1 is that the boron nitride composite polyimide separator is prepared by Preparation Example 5.
[0053] Example 8 A preparation process for a high temperature resistant battery: The difference from Example 1 is that the molybdenum disulfide doped graphene electrode is prepared by Preparation Example 7.
[0054] Example 9 A preparation process for a high temperature resistant battery: The difference from Example 1 is that the molybdenum disulfide doped graphene electrode is prepared by Preparation Example 8.
[0055] Comparative Example Comparative Example 1 A preparation process of a high temperature resistant battery: The difference from Example 1 is that the negative electrode sheet adopts a graphene electrode purchased from Foshan Nanhai Baotan Graphite Products Co., Ltd.
[0056] Comparative Example 2 A preparation process for a high temperature resistant battery: The difference from Example 1 is that the molybdenum disulfide doped graphene electrode is prepared by Preparation Example 8.
[0057] Comparative Example 3 A preparation process of a high temperature resistant battery: The difference from Example 1 is that a polyimide membrane is selected as the diaphragm, which is purchased from Dongguan Benxiang Electronic Materials Co., Ltd.
[0058] Performance testing Detection Methods After being fully charged, the batteries prepared in Examples 1-9 and Comparative Examples 1-3 were placed in 65° C., 85° C., and 105° C. environments for 16 hours, respectively, and the thickness expansion rate of the batteries was measured.
[0059] Table 1 Experimental data Combining Example 1 and Comparative Example 1 with Table 1, it can be seen that compared with ordinary graphene electrodes, molybdenum disulfide can effectively resist thermal decomposition and oxidation in a high temperature environment and maintain structural integrity. This thermal stability enables the graphene electrode doped with molybdenum disulfide to maintain good performance under high temperature conditions. When molybdenum disulfide is combined with graphene, the two can form a synergistic effect, further improving the high temperature resistance of the electrode.
[0060] Combining Example 1 and Comparative Example 2 with Table 1, it can be seen that drying and hot pressing can help fix the electrode material on the substrate and improve the stability and contact performance of the electrode. Hot pressing can regulate the morphology and structure of the electrode film and improve the conductivity and charge-discharge performance of the electrode.
[0061] It can be seen from Example 1 and Comparative Example 3 and Table 1 that, compared with ordinary polyimide diaphragms, when boron nitride is compounded with polyimide to form a diaphragm, the two can produce a synergistic effect, further improving the high temperature resistance of the diaphragm. The introduction of boron nitride not only enhances the thermal stability of the diaphragm, but also improves the thermal conductivity of polyimide, thereby more effectively dispersing and transferring heat and reducing the damage to the diaphragm caused by high temperature. Boron nitride composite polyimide diaphragm also has better mechanical properties and chemical stability, making it more resistant to deformation and chemical corrosion in high temperature environments.
[0062] From Examples 1-2 and Table 1, it can be seen that by introducing nano-silicon carbide, 1-ethyl-3-methylimidazolium tetrafluoroborate and benzotriazole into the electrolyte, the conductivity is enhanced, the ion conductivity is improved and the oxidation reaction is inhibited, which significantly improves the high temperature resistance of the battery, ensuring that the battery can still maintain a stable, efficient and safe working state in a high temperature environment.
[0063] It can be seen from Examples 1 and 2 and Table 1 that by making the diaphragm 1.5-2.5 mm wider than the negative electrode sheet and the negative electrode sheet 1-2 mm wider than the positive electrode sheet, the internal heat distribution of the lithium battery can be effectively optimized, the working heat can be reduced, the heat dissipation efficiency can be improved, and the structural stability of the battery can be enhanced, thereby improving the high temperature resistance of the lithium battery in a high temperature environment and ensuring that it works more stably and safely.
[0064] It can be seen from Example 1, Examples 4-7 and Table 1 that the high temperature resistance of the diaphragm can be further improved by changing the amount of boron nitride added, and the diisocyanate undergoes a covalent grafting reaction with the hydroxylated nano-boron nitride, which improves the surface chemical properties of the nano-boron nitride and enhances its compatibility with the polyimide monomer, which helps to improve the high temperature resistance of the boron nitride composite polyimide diaphragm.
[0065] It can be seen from Example 1, Examples 8-9 and Table 1 that the high temperature resistance of the lithium battery can be further improved by adjusting the doping amount of nano-molybdenum disulfide.
[0066] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high temperature resistant battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte, an aluminum-plastic film, an insulating glue, a positive electrode ear and a negative electrode ear. The positive electrode sheet comprises a lithium cobalt oxide electrode, the negative electrode sheet comprises a molybdenum disulfide-doped graphene electrode, the separator comprises a boron nitride composite polyimide separator, and the electrolyte comprises fluoroethylene carbonate, vinyl sulfite and lithium hexafluorophosphate in a mass ratio of 6:2:(1-3).
2. The high temperature resistant battery according to claim 1, characterized in that: The preparation method of the boron nitride composite polyimide diaphragm is as follows: A1. Disperse 50-100 parts of nano boron nitride by weight in 150-200 parts of acetone, add 180-200 parts of diamine monomer and 200-220 parts of anhydride monomer, stir evenly, pressurize at 1-3atm at 50-90°C, and use infrared radiation for in-situ polymerization to obtain a precursor solution; A2. Coat the precursor solution on a glass substrate with a thickness of 20-60 μm, transfer the coated glass substrate to a vacuum drying oven, heat it to 250-300° C. at a rate of 5-15° C. / min at room temperature of 25° C., and keep it warm for 2-4 hours to obtain a boron nitride composite polyimide diaphragm.
3. The high temperature resistant battery according to claim 2, characterized in that: The nano boron nitride needs to be surface modified before step A1, and the surface modification method is as follows: B1. Mix the dried nano boron nitride with a sodium hydroxide solution having a mass concentration of 10-15% in a mass ratio of 1:(2-3), and react the boron nitride nanosheets with the sodium hydroxide solution for 1-3 hours under continuous stirring at 20-50 r / min; B2, separating the reacted nano boron nitride from the sodium hydroxide solution by centrifugation, washing with deionized water and then vacuum drying to obtain surface hydroxylated nano boron nitride; B3, mixing and stirring the surface hydroxylated nano boron nitride with toluene to form a uniform dispersion, adding diisocyanate to the dispersion, the mass ratio of diisocyanate to nano boron nitride being (1-5):1, stirring and reacting at 40-80° C. for 4-8 hours, so that the diisocyanate and the hydroxyl groups on the surface of the boron nitride nanosheets undergo a covalent grafting reaction; B4. Separate the reacted nano-boron nitride from the solution by centrifugal filtration, wash with deionized water, and vacuum dry after washing to obtain surface-modified nano-boron nitride.
4. The high temperature resistant battery according to claim 3, characterized in that: The nano boron nitride is selected from hexagonal boron nitride or cubic boron nitride.
5. The high temperature resistant battery according to claim 1, characterized in that: The electrolyte also includes nano silicon carbide, 1-ethyl-3-methylimidazolium tetrafluoroborate, and benzotriazole. The mass ratio of the nano silicon carbide, 1-ethyl-3-methylimidazolium tetrafluoroborate, benzotriazole and fluoroethylene carbonate is (1-2):(2-3):1:
6.
6. The high temperature resistant battery according to claim 1, characterized in that: The specific preparation steps of the molybdenum disulfide doped graphene electrode are: C1. Mixing nano-molybdenum disulfide and graphene powder in a mass ratio of (1-3):10, and mixing by high-speed mechanical mixing at 2000-2500 r / min to obtain a mixed powder; C2, placing the mixed powder in a high temperature furnace, performing heat treatment under an inert atmosphere, the heat treatment temperature being 800-1000° C., and cooling to room temperature after the heat treatment to obtain molybdenum disulfide-doped graphene; C3, mixing molybdenum disulfide-doped graphene with carbon black, polytetrafluoroethylene, and ethanol in a mass ratio of 8: (1-3): (0.5-1.5): 8, stirring to prepare a uniform electrode material slurry, and coating the electrode material slurry on a glass fiber board to form a uniform electrode film; C4, placing the coated electrode film in a vacuum drying oven for drying to remove the solvent and fix the electrode material on the substrate; C5. Place the dried electrode film into a hot press for hot pressing at a pressure of 0.5-1.5 MPa and a temperature of 120-160°C. After separating the electrode film from the substrate, a molybdenum disulfide-doped graphene electrode is obtained.
7. A process for preparing a high temperature resistant battery according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Weld the positive electrode tab to the positive electrode sheet and the negative electrode tab to the negative electrode sheet by ultrasonic welding; S2. In the order of positive electrode sheet - separator - negative electrode sheet - separator, the positive and negative electrode sheets and separator are stacked, and the stacked positive and negative electrode sheets and separator are wound to obtain a battery cell; S3, baking the battery cell in a high vacuum oven to remove moisture from the core; S4. After baking, the electrolyte is injected into the battery cell, the battery cell is encapsulated with an aluminum-plastic film, and insulating glue is used to insulate and seal the connection between the battery cell and the positive and negative pole ears to obtain a high temperature resistant battery.
8. The high temperature resistant battery according to claim 7, characterized in that: The separator is 1.5-2.5 mm wider than the negative electrode sheet, and the negative electrode sheet is 1-2 mm wider than the positive electrode sheet.
9. The high temperature resistant battery according to claim 7, characterized in that: The high vacuum oven maintains a vacuum degree of (-95%)-(-99%) and a temperature of 80°C±0.5°C when drying the battery cells.
Citation Information
Cited By
Polyimide-based high-temperature hot-melt metal substrate and preparation method thereof
CN120547757A
A polyimide-based high-temperature hot-melt metal substrate and a method for manufacturing the same
CN120547757B
Preparation method of high-temperature-resistant lithium battery cell
CN120767287A
A method for preparing a high-temperature-resistant lithium battery cell
CN120767287B