Electrostatic spinning polyvinylidene fluoride fiber-based composite nanofiltration membrane as well as preparation method and application thereof

Through electrospinning technology and interfacial polymerization, a polyvinylidene fluoride fiber-based nanofiltration membrane with high porosity and large pore size was prepared, which solved the problems of low flux and complex preparation of nanofiltration membranes, and achieved high throughput and stability Nanofiltration membrane with good properties is suitable for a variety of water treatment applications.

CN118987972APending Publication Date: 2024-11-22ZHEJIANG GREEN NEW MATERIALS
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411099960.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing nanofiltration membrane has low flux and complex preparation process, and the physical and chemical stability of the supporting layer base membrane is poor, making it difficult to meet the needs of treating waste liquids, organic solutions, high-temperature wastewater and other environments containing acid and alkali.

Method used

The polyvinylidene fluoride fiber-based composite nanofiltration membrane was prepared by electrospinning technology. Hydrophilic inorganic nanoparticles were added to the polyvinylidene fluoride spinning liquid, and high-porosity and large-porosity fiber membrane was made by electrospinning. Two interfacial polymerization reactions were carried out to form a nanofiltration membrane with high throughput and good stability.

Benefits of technology

The water permeability flux and pressure resistance of the nanofiltration membrane are improved, the stability and permeability of the separation layer are enhanced, and the scope of application of the nanofiltration membrane in different application fields is broadened.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118987972A_ABST
    Figure CN118987972A_ABST
Patent Text Reader

Abstract

The invention discloses an electrostatic spinning polyvinylidene fluoride fiber-based composite nanofiltration membrane as well as a preparation method and application thereof, and belongs to the technical field of membrane separation. The preparation method comprises the following steps: firstly, preparing a polyvinylidene fluoride spinning solution from polyvinylidene fluoride resin, hydrophilic inorganic nanoparticles and an organic solvent; preparing a polyvinylidene fluoride fiber membrane from the polyvinylidene fluoride spinning solution by using an electrostatic spinning technology, further performing hot pressing to obtain a polyvinylidene fluoride fiber base membrane, and performing two interfacial polymerization reactions on the polyvinylidene fluoride fiber base membrane by using a water phase solution and an organic phase solution to obtain the electrostatic spinning polyvinylidene fluoride fiber-based composite nanofiltration membrane. The polyvinylidene fluoride fiber-based membrane has the characteristics of high porosity, large pore size, good flexibility and the like, a polyamide separation layer prepared by two interfacial polymerization is more perfect, and the obtained product electrostatic spinning polyvinylidene fluoride fiber-based composite nanofiltration membrane has the advantages of excellent water permeation flux, good pressure resistance, high rejection rate on divalent salt ions, good water permeability and good water permeability. The application prospect in the field of water treatment is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of membrane separation, and in particular to an electrostatically spun polyvinylidene fluoride fiber-based composite nanofiltration membrane and a preparation method and application thereof. Background Art

[0002] Nowadays, in order to solve the problems of water shortage and water pollution, water treatment technology has received widespread attention. Membrane separation technology is a simple and efficient water treatment technology. Nanofiltration membrane has the function of salt separation and can also separate organic matter of different molecular weights. It is widely used in industrial wastewater treatment, domestic sewage treatment, ultrapure water preparation and seawater desalination. For example, wastewater from metal plating and alloy production processes usually contains high concentrations of heavy metals such as nickel, iron, copper and zinc. In order to make these wastewaters meet the discharge regulations, nanofiltration membrane technology can be used to remove heavy metals through hydroxide precipitation treatment. Nanofiltration membrane can not only recycle and purify more than 90% of wastewater, but also concentrate the heavy metal ion content by more than 10 times. Nanofiltration membrane can also recycle organic matter in industrial wastewater to achieve "zero discharge" of wastewater. Domestic sewage is usually treated by combining biodegradation and chemical oxidation, but this treatment method has the problems of resource waste and high residue. Adding nanofiltration chain between biodegradation and chemical oxidation can remove small molecules produced during biodegradation and reduce residues. Ultrapure water is an important raw material for the semiconductor, biotechnology and pharmaceutical industries. Ultrapure water requires high water quality. Nanofiltration membranes with negative charges and low wetting angles can reduce the TOC (total organic carbon) content to meet the requirements of ultrapure water. In addition, nanofiltration membrane technology can remove multivalent salts and organic pollutants from seawater, and the retention rate of monovalent salts is relatively low. Compared with reverse osmosis membranes, it can selectively separate monovalent salts and multivalent salts, and requires less energy than reverse osmosis membranes, and also has certain applications in seawater desalination.

[0003] It can be seen that nanofiltration membranes are widely used in the field of water treatment. At present, commercial nanofiltration membranes are generally composite membranes composed of a support layer base membrane and a polyamide separation functional layer. The support layer base membrane is generally a polyethersulfone or polysulfone material with good hydrophilicity. However, the physical and chemical stability of such support layer base membranes is poor, resulting in a relatively single application range and application environment of the corresponding nanofiltration membranes. For the treatment of waste liquids containing acids and alkalis, organic solutions, high-temperature wastewater, etc., the nanofiltration membranes made of such support layer base membranes cannot meet the requirements, and the support layer base membranes are usually prepared by the immersion precipitation phase conversion method, with small membrane pore size, small porosity and poor adjustability.

[0004] Fluorine-containing materials such as polyvinylidene fluoride have good physical and chemical stability, can withstand high temperatures, resist corrosion from various acids, bases and solvents, and resist ultraviolet radiation, and have high mechanical strength, which is very important for the practical application of separation membranes. And because it has a lot of good solvents, it is easy to prepare separation membranes through a simple phase inversion method. Currently, the industrialized polyvinylidene fluoride separation membranes are mainly ultrafiltration membranes, and some studies have also applied it to prepare nanofiltration membranes. For example, the Chinese patent document with the publication number CN108043227A discloses a method for preparing a polyvinylidene fluoride-based nanofiltration membrane, which adopts a phase inversion method to prepare a polyvinylidene fluoride ultrafiltration base membrane using a mixed solution containing polyvinylidene fluoride, a solvent, an additive, and a porogen, and then the ultrafiltration base membrane is immersed in an aqueous phase monomer solution and an oil phase monomer solution respectively by an interfacial polymerization method and subjected to heat treatment to obtain a polyvinylidene fluoride-based nanofiltration membrane; the Chinese patent document with the publication number CN115350603A discloses a polyvinylidene fluoride-based thin layer composite nanofiltration membrane and a preparation method thereof, in the preparation process of the polyvinylidene fluoride-based thin layer, firstly, a hydrophilic poly (N-hydroxyethyl acrylamide) (PHEAA) surface functionalized polyvinylidene fluoride support membrane is prepared by an immersion precipitation phase inversion method, and then a polyamide composite nanofiltration membrane is prepared by interfacial polymerization. However, the polyvinylidene fluoride-based membranes in the above inventions are all prepared by an immersion precipitation phase inversion method, and the membrane pore size is small, which is not conducive to the water permeability of the product membrane, and the addition of a porogen will also increase the types of raw materials. Summary of the invention

[0005] The invention provides a method for preparing an electrostatically spun polyvinylidene fluoride fiber-based composite nanofiltration membrane, which can solve the problems of low flux and complex preparation process of conventional nanofiltration membranes.

[0006] The specific technical solutions adopted are as follows:

[0007] A method for preparing an electrostatically spun polyvinylidene fluoride fiber-based composite nanofiltration membrane comprises the following steps:

[0008] (1) preparing a polyvinylidene fluoride spinning solution using a polyvinylidene fluoride resin, hydrophilic inorganic nanoparticles and an organic solvent; in the polyvinylidene fluoride spinning solution, the mass fraction of the polyvinylidene fluoride resin is 16-24wt%, and the mass ratio of the hydrophilic inorganic nanoparticles to the polyvinylidene fluoride resin is 0.1-0.4:1; the hydrophilic inorganic nanoparticles are at least one of hydrophilic silicon dioxide, zinc oxide, ferric oxyhydroxide, ferrosoferric oxide and titanium dioxide;

[0009] (2) using electrospinning technology to prepare a polyvinylidene fluoride fiber membrane from the polyvinylidene fluoride spinning solution obtained in step (1), and hot-pressing the polyvinylidene fluoride fiber membrane to obtain a polyvinylidene fluoride fiber base membrane;

[0010] (3) Immersing one side surface of the polyvinylidene fluoride fiber-based membrane in an aqueous solution for 5-25 minutes and then taking it out, then immersing the same side surface of the membrane in an organic solution for 1-5 minutes for interfacial polymerization reaction, taking it out and heating and curing it for 2-6 minutes to obtain a nanofiltration membrane with a single interfacial polymerization, and finally repeating the above-mentioned steps of immersing in an aqueous solution - immersing in an organic solution for interfacial polymerization reaction - heating and curing for one side surface of the membrane with interfacial polymerization, to obtain the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane.

[0011] During the electrospinning process, the polyvinylidene fluoride spinning solution is placed in a high-voltage electrostatic field. Under the action of the electric field force, the spinning solution is charged and deformed, forming Taylor cone droplets at the end of the nozzle. When the charge repulsion on the droplet surface exceeds the surface tension, a jet is ejected at high speed on the droplet surface. These jets are stretched at high speed by the electric field force, the solvent evaporates and solidifies, and finally deposited on the receiving plate to form polyvinylidene fluoride nanofibers with hydrophilic inorganic nanoparticles.

[0012] The preparation of polyvinylidene fluoride fiber membrane by electrospinning is simple, easy to operate and pollution-free. The obtained membrane has the characteristics of high porosity, large pore size, good flexibility, etc. After further heat pressing, the polyvinylidene fluoride fiber-based membrane is obtained. The polyvinylidene fluoride fiber-based membrane prepared by the above method provides the possibility for the preparation of high-flux composite nanofiltration membrane. In addition, the polyvinylidene fluoride material itself has excellent physical, chemical and mechanical properties. The product nanofiltration membrane made of polyvinylidene fluoride fiber-based membrane can maintain good shrinkage resistance in the face of harsh environmental conditions (high temperature, acid and alkali, etc.) and mechanical pressure generated by the components in actual applications, avoiding the phenomenon of membrane tearing and flow rate reduction, which can ensure that the product nanofiltration membrane maintains excellent separation effect and stability in different nanofiltration systems, which helps to broaden and enrich the application of nanofiltration membrane in drinking water softening, wastewater purification, food processing and other industries.

[0013] Secondly, the method of the present invention prepares a polyvinylidene fluoride spinning solution of a specific component. When the mass fraction of polyvinylidene fluoride is lower than 16wt%, the viscosity of the casting solution is too low, the silk is not formed during the electrospinning process or the obtained fiber membrane has many defects. When the mass fraction of polyvinylidene fluoride is higher than 24wt%, the polymer molecular chains are tightly entangled, the spinning resistance increases, and fiber nodules are easily formed. The addition of hydrophilic inorganic nanoparticles can improve the hydrophilicity of the polyvinylidene fluoride membrane on the one hand, and can also increase the pressure resistance of the polyvinylidene fluoride membrane. When the mass ratio of the hydrophilic inorganic nanoparticles to the polyvinylidene fluoride resin is 0.1-0.4:1, it is helpful to improve the hydrophilicity and pressure resistance of the polyvinylidene fluoride membrane, and it is easy to disperse in the polyvinylidene fluoride spinning solution, and will not agglomerate to cause waste of hydrophilic inorganic nanoparticles.

[0014] In addition, the method of the present invention carries out a secondary interfacial polymerization process, which is beneficial to the preparation of a more perfect polyamide separation layer, while allowing the polyamide separation layer to better combine with the base membrane, thereby enhancing the structural stability of the composite nanofiltration membrane.

[0015] In step (1), the organic solvent can be selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and chloroform. The organic solvent can also be other substances that can be reasonably selected and adjusted by those skilled in the art based on common sense in the art.

[0016] Preferably, in step (1), the particle size of the hydrophilic inorganic nanoparticles is 10-50 nm, and the hydrophilic inorganic nanoparticles are preferably hydrophilic silicon dioxide or zinc oxide. Adding hydrophilic inorganic nanoparticles to the polyvinylidene fluoride spinning solution can simultaneously improve the hydrophilicity and pressure resistance of the polyvinylidene fluoride membrane, and enhance the stability and permeability of the nanofiltration separation layer obtained by subsequent interfacial polymerization. Experiments have shown that hydrophilic silicon dioxide or zinc oxide has a better effect.

[0017] Preferably, in step (2), the parameters of the electrospinning process are: ambient temperature 20-35°C, ambient humidity 25%-50%, spinning distance 10-20cm, feed rate 0.5-1.0mL / h, spinning voltage 15-20kV.

[0018] Preferably, in step (2), the polyvinylidene fluoride fiber membrane is hot-pressed at 50-100° C. for 15-30 min to obtain a polyvinylidene fluoride fiber base membrane. Hot pressing can enhance the adhesion between the fibers, making the polyvinylidene fluoride fiber base membrane more stable and complete as a whole.

[0019] In step (3), the aqueous phase monomer in the aqueous phase solution is any one of piperazine, polyethyleneimine, p-phenylenediamine, m-phenylenediamine, and ethylenediamine, and the mass concentration of the aqueous phase solution is 0.5-4wt%; the organic phase monomer in the organic phase solution is trimesoyl chloride or isophthaloyl chloride, the solvent is n-hexane and / or xylene, and the mass concentration of the organic phase solution is 0.1-0.3wt%.

[0020] The interfacial polymerization reaction in the above-mentioned specific aqueous phase solution and organic phase solution helps to obtain a complete, defect-free separation layer with moderate thickness. Too much or too little aqueous phase monomer and organic phase monomer will cause the separation layer to be too thick or the surface of the separation layer to have defects, which will reduce the performance of the nanofiltration membrane.

[0021] Preferably, the mass concentration of the aqueous phase solution of the first impregnation is 2-4wt%, the mass concentration of the aqueous phase solution of the first impregnation is higher than the mass concentration of the aqueous phase solution of the second impregnation, and the mass concentration of the aqueous phase solution of the second impregnation is 0.5-3wt%; the mass concentration of the organic phase solution of the first impregnation is 0.1-0.3wt%, the mass concentration of the organic phase solution of the first impregnation is higher than the mass concentration of the organic phase solution of the second impregnation, and the mass concentration of the organic phase solution of the second impregnation is 0.1-0.2wt%. Under the above preferred conditions, a two-step interfacial polymerization reaction is carried out, and a relatively perfect nanofiltration layer is obtained at a higher concentration in the first interfacial polymerization, and the secondary interfacial polymerization can supplement and improve the defects that may exist in the first polymerization nanofiltration layer. If the concentration of the secondary interfacial polymerization is too high, the overall thickness of the nanofiltration layer finally obtained will be thicker, reducing the permeability of the composite nanofiltration membrane.

[0022] Optionally, in step (3), the temperature of heat curing is 40-70°C for 2-6 minutes. The purpose of heat curing is to further improve the cross-linking degree of the polyamide separation layer obtained by interfacial polymerization and improve the nanofiltration layer. If the temperature is too low or the time is too short, the cross-linking degree of the polyamide layer will be low; if the temperature is too high or the time is too long, the cross-linked polyamide will be further hydrolyzed; this will make the nanofiltration layer incomplete and the separation performance will be reduced.

[0023] The present invention also provides an electrostatically spun polyvinylidene fluoride fiber-based composite nanofiltration membrane prepared by the preparation method of the electrostatically spun polyvinylidene fluoride fiber-based composite nanofiltration membrane.

[0024] The electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane comprises a polyvinylidene fluoride fiber-based membrane with strong bonding force and a polyamide separation layer. The polyvinylidene fluoride fiber-based membrane has high porosity, good flexibility, and large pore size, and the polyamide separation layer has a dense structure. The thickness of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane is preferably 80-250μm. When the membrane thickness is less than 80μm, the pressure resistance is poor. When the thickness is higher than 250μm, the overall resistance of the membrane increases, which is not conducive to large-scale treatment of purified water and reduces the water treatment volume.

[0025] The present invention also provides application of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane in the field of water treatment.

[0026] Preferably, the pressure tolerance range of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane is 0-25 bar, further 0-15 bar, and the pure water flux is 15-125 L / (m 2 ·h·bar), the retention rate of divalent salt is greater than 94%, and the retention rate of monovalent salt is 10-80%.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The method of the present invention utilizes a polyvinylidene fluoride spinning solution of a specific component to prepare a polyvinylidene fluoride fiber-based membrane through an electrospinning method. The hydrophilic inorganic nanoparticles added to the polyvinylidene fluoride spinning solution can simultaneously improve the hydrophilicity and pressure resistance of the polyvinylidene fluoride membrane, and enhance the stability and permeability of the nanofiltration separation layer obtained by subsequent interfacial polymerization. The preparation of the polyvinylidene fluoride fiber-based membrane by electrospinning technology is simple, easy to operate and pollution-free. The obtained membrane has the characteristics of high porosity, large pore size, good flexibility, etc., which is conducive to the preparation of high-throughput product composite nanofiltration membranes.

[0029] (2) The present invention prepares an electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane through two interfacial polymerizations. The two interfacial polymerizations are beneficial to preparing a more complete polyamide separation layer, while allowing the polyamide separation layer to better combine with the base membrane, thereby enhancing the structural stability of the composite nanofiltration membrane.

[0030] (3) The electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane prepared by the method of the present invention has excellent water permeation flux, good pressure resistance, and high retention rate for divalent salt ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a surface electron microscope image of the polyvinylidene fluoride fiber membrane after hot pressing made by electrospinning technology in Example 1;

[0032] Figure 2 This is a surface electron microscope image of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane prepared in Example 1. DETAILED DESCRIPTION

[0033] The present invention will be further described below in conjunction with the examples and drawings. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples that do not specify specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer. Contents not described in detail in this specification belong to prior art known to professionals and technicians in the field.

[0034] Example 1

[0035] (1) Add 7.2g of 30nm hydrophilic silica, 32.8g of N-methylpyrrolidone, and 49.2g of N,N-dimethylformamide to a three-necked flask, add 18g of polyvinylidene fluoride resin after ultrasonic treatment for 30 minutes, stir at 60°C for 6 hours to obtain a uniform mixed solution, and let it stand for 8 hours to degas to obtain polyvinylidene fluoride spinning solution. Subsequently, electrospinning was performed at a voltage of 16kV using electrospinning technology, with a feed rate of 0.5mL / h, a spinning distance of 15cm, a spinning ambient temperature of 25°C, and an ambient humidity of 35%. The polyvinylidene fluoride spinning solution was made into a polyvinylidene fluoride fiber membrane, and the polyvinylidene fluoride fiber membrane was placed in a hot press and hot pressed at 60°C for 15 minutes to obtain a polyvinylidene fluoride fiber base membrane. The SEM image of the polyvinylidene fluoride fiber base membrane is shown in the figure. Figure 1 shown.

[0036] (2) The surface of one side of the polyvinylidene fluoride fiber-based membrane was immersed in a 3.5wt% piperazine aqueous solution for 10 minutes and then taken out, and the same side surface (the surface adsorbed with piperazine) was immersed in a 0.3wt% trimesoyl chloride-n-hexane solution for 2 minutes for interfacial polymerization reaction and then taken out, and then the membrane was placed in a 60°C oven for heating and curing for 2 minutes to obtain a nanofiltration membrane with a first interfacial polymerization; the surface of the nanofiltration membrane with a first interfacial polymerization that underwent interfacial polymerization was immersed in a 2.0wt% piperazine aqueous solution for 10 minutes and then taken out, and the same side surface (the surface adsorbed with piperazine) was immersed in a 0.1wt% trimesoyl chloride-n-hexane solution for 2 minutes for a second interfacial polymerization reaction and then taken out, and then the membrane was placed in a 60°C oven for heating and curing for 2 minutes to prepare the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane, and the SEM image of the composite nanofiltration membrane is as shown in FIG. Figure 2 shown.

[0037] After testing, the pure water flux of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane at 3 bar is 20L / (m 2 ·h·bar), and the sodium sulfate retention rate was 97.4%.

[0038] Example 2

[0039] In this embodiment, the preparation method of the polyvinylidene fluoride fiber-based membrane is different from that in Example 1 only in that the mass of the polyvinylidene fluoride resin is 20 g, the mass of N,N-dimethylformamide is 48 g, and the mass of N-methylpyrrolidone is 32 g, and the other process steps are the same.

[0040] The preparation method of the polyamide separation layer is different from that in Example 1 only in that the surface of the nanofiltration membrane on which the interfacial polymerization has occurred is immersed in a 0.5 wt % piperazine aqueous solution for 10 minutes and then taken out. The other process steps are the same.

[0041] After testing, the pure water flux of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane at 3.5 bar is 125L / (m 2 ·h·bar), and the sodium sulfate retention rate was 62.7%.

[0042] Example 3

[0043] In this embodiment, the preparation method of the polyvinylidene fluoride fiber-based membrane is different from that in Embodiment 1 only in that the hydrophilic inorganic nanoparticles are 40 nm iron oxyhydroxide; the other process steps are the same.

[0044] The preparation method of the nanofiltration separation layer is the same as that in Example 1.

[0045] After testing, the pure water flux of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane at 2.5 bar is 35L / (m 2 ·h·bar), and the sodium sulfate retention rate was 92.7%.

[0046] Example 4

[0047] In this embodiment, the preparation method of the polyvinylidene fluoride fiber-based membrane is different from that in Embodiment 1 only in that the hydrophilic inorganic nanoparticles are 20 nm zinc oxide; the other process steps are the same.

[0048] The preparation method of the polyamide separation layer is different from that in Example 1 only in that the surface of the nanofiltration membrane on which the interfacial polymerization occurred is immersed in a 1.0wt% piperazine aqueous solution for 10 minutes and then taken out, and the same surface (the surface adsorbed with piperazine) is immersed in a 0.15wt% trimesoyl chloride-n-hexane solution for 2 minutes for interfacial polymerization reaction and then taken out, and then the membrane is placed in a 60°C oven for heating and curing for 2 minutes to prepare the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane; the other process steps are the same.

[0049] After testing, the pure water flux of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane at 4 bar is 55L / (m 2 ·h·bar), and the sodium sulfate retention rate was 90.1%.

[0050] Example 5

[0051] In this embodiment, the preparation method of the polyvinylidene fluoride fiber-based membrane is the same as that in Embodiment 1.

[0052] The preparation method of the polyamide separation layer is different from that in Example 1 only in that the surface of the nanofiltration membrane on which the interfacial polymerization occurred is immersed in a 2.5wt% piperazine aqueous solution for 10 minutes and then taken out, and the same surface (the surface adsorbed with piperazine) is immersed in a 0.2wt% trimesoyl chloride-n-hexane solution for 2 minutes for interfacial polymerization reaction and then taken out, and then the membrane is placed in an oven at 60°C for heating and curing for 2 minutes to prepare the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane; the other process steps are the same.

[0053] After testing, the pure water flux of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane at 5 bar is 40L / (m 2 ·h·bar), and the sodium sulfate retention rate was 88.5%.

[0054] Example 6

[0055] In this embodiment, the preparation method of the polyvinylidene fluoride fiber-based membrane is different from that in Embodiment 1 only in that the mass of the hydrophilic silica is 3.6 g, and the other process steps are the same.

[0056] The only difference between the preparation method of the polyamide separation layer and that in Example 1 is that the aqueous phase monomer used in the two interfacial polymerization processes is polyethyleneimine, and the other process steps are the same.

[0057] After testing, the pure water flux of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane at 6 bar is 105L / (m 2 ·h·bar), and the sodium sulfate retention rate was 82.4%.

[0058] Comparative Example 1

[0059] In this comparative example, the preparation method of the polyvinylidene fluoride fiber-based membrane is different from that in Example 1 only in that no hydrophilic inorganic nanoparticles are added; the other process steps are the same.

[0060] The preparation method of the polyamide separation layer is the same as that in Example 1.

[0061] After testing, the pure water flux of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane at 1 bar is 8L / (m 2 ·h·bar), and the sodium sulfate retention rate was 74.6%.

[0062] Comparative Example 2

[0063] In this comparative example, the preparation method of the polyvinylidene fluoride fiber-based membrane is the same as that in Example 1.

[0064] The only difference between the preparation method of the polyamide separation layer and Example 1 is that only the first interfacial polymerization is performed, and the other process steps are the same.

[0065] After testing, the pure water flux of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane at 2 bar is 16L / (m 2 ·h·bar), and the sodium sulfate retention rate was 65.3%.

[0066] The embodiments described above provide a detailed description of the technical solutions of the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane, characterized in that: The following steps are involved: (1) preparing a polyvinylidene fluoride spinning solution using a polyvinylidene fluoride resin, hydrophilic inorganic nanoparticles and an organic solvent; in the polyvinylidene fluoride spinning solution, the mass fraction of the polyvinylidene fluoride resin is 16-24wt%, and the mass ratio of the hydrophilic inorganic nanoparticles to the polyvinylidene fluoride resin is 0.1-0.4:1; the hydrophilic inorganic nanoparticles are at least one of hydrophilic silicon dioxide, zinc oxide, ferric oxyhydroxide, ferrosoferric oxide and titanium dioxide; (2) using electrospinning technology to prepare a polyvinylidene fluoride fiber membrane from the polyvinylidene fluoride spinning solution obtained in step (1), and hot-pressing the polyvinylidene fluoride fiber membrane to obtain a polyvinylidene fluoride fiber base membrane; (3) Immersing one side surface of the polyvinylidene fluoride fiber-based membrane in an aqueous solution for 5-25 minutes and then taking it out, then immersing the same side surface of the membrane in an organic solution for 1-5 minutes for interfacial polymerization reaction, taking it out and heating and curing it for 2-6 minutes to obtain a nanofiltration membrane with a single interfacial polymerization, and finally repeating the above-mentioned steps of immersing in an aqueous solution - immersing in an organic solution for interfacial polymerization reaction - heating and curing for one side surface of the membrane with interfacial polymerization, to obtain the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane.

2. The method for preparing an electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane according to claim 1, characterized in that: In step (1), the organic solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone and chloroform.

3. The method for preparing an electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane according to claim 1, characterized in that: In step (1), the particle size of the hydrophilic inorganic nanoparticles is 10-50 nm, and the hydrophilic inorganic nanoparticles are hydrophilic silicon dioxide or zinc oxide.

4. The method for preparing an electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane according to claim 1, characterized in that: In step (2), the parameters of the electrospinning process are: ambient temperature 20-35°C, ambient humidity 25%-50%, spinning distance 10-20cm, feed rate 0.5-1.0mL / h, spinning voltage 15-20kV.

5. The method for preparing an electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane according to claim 1, characterized in that: In step (2), the polyvinylidene fluoride fiber membrane is hot-pressed at 50-100° C. for 15-30 min to obtain a polyvinylidene fluoride fiber-based membrane.

6. The method for preparing an electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane according to claim 1, characterized in that: The aqueous phase monomer in the aqueous phase solution is any one of piperazine, polyethyleneimine, p-phenylenediamine, m-phenylenediamine, and ethylenediamine, and the mass concentration of the aqueous phase solution is 0.5-4wt%; the organic phase monomer in the organic phase solution is trimesoyl chloride or isophthaloyl chloride, the solvent is n-hexane and / or xylene, and the mass concentration of the organic phase solution is 0.1-0.3wt%.

7. The method for preparing an electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane according to claim 1, characterized in that: The mass concentration of the aqueous phase solution of the first impregnation is 2-4wt%, which is higher than that of the aqueous phase solution of the second impregnation, and the mass concentration of the aqueous phase solution of the second impregnation is 0.5-3wt%; the mass concentration of the organic phase solution of the first impregnation is 0.1-0.3wt%, which is higher than that of the organic phase solution of the second impregnation, and the mass concentration of the organic phase solution of the second impregnation is 0.1-0.2wt%.

8. An electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane prepared according to the method for preparing an electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane according to any one of claims 1 to 7.

9. The electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane according to claim 8, characterized in that: The invention comprises a polyvinylidene fluoride fiber-based membrane and a polyamide separation layer.

10. Use of the electrospun polyvinylidene fluoride fiber-based composite nanofiltration membrane according to claim 8 or 9 in the field of water treatment.

Citation Information

Cited By

  • Polyamide composite membrane modified by PDA solution, preparation method of polyamide composite membrane and method for extracting m-cresol from phenol-containing wastewater

    CN120001221A

  • Preparation method of hollow fiber nanofiltration membrane based on polytetrafluoroethylene

    CN120094415A

  • Ferroelectric polymer nanofiber membrane as well as preparation method and application thereof