Composite membrane for MABR (Membrane Aerated Baffled Reactor) sewage treatment process and preparation process of composite membrane
By using composite membranes in the MABR sewage treatment process, combining magnetic nanofillers and collagen layers, the microbial adhesion problem caused by the hydrophobicity of hollow breathable membranes is solved, and faster biofilm formation and more efficient sewage treatment effects are achieved.
Patent Information
- Application Number
- CN202411210405.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
The hydrophobic surface of the hollow breathable membrane in the existing MABR sewage treatment process leads to a reduction in microbial adhesion points, affecting the rapid formation of biofilms and sewage treatment efficiency.
Using composite membranes, including hollow hydrophobic membranes and coated modified collagen layers, the surface hydrophilicity and roughness of the membrane are improved by adding magnetic nanofillers and etching treatment, increasing microbial adhesion points and pore sizes, and promoting oxygen transport. and microbial growth.
The time for hanging the biofilm is shortened, the efficiency and stability of wastewater treatment is improved, the oxygen permeability and pollutant removal rate are enhanced, and a more stable and efficient biofilm system is formed.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of feed and preparation thereof, and in particular to a composite membrane for a MABR sewage treatment process and a preparation process thereof. Background Art
[0002] MABR sewage treatment process, namely membrane aerated biofilm reactor sewage treatment process, is an important innovation in contemporary sewage treatment technology. By combining hollow breathable membrane with biofilm method and sewage treatment technology, a new sewage treatment method has been opened up. The core is to use a special hollow breathable membrane, which can continuously provide the required oxygen for the microorganisms on the biofilm. When sewage flows through this biofilm, harmful substances are quickly adsorbed and decomposed, so that the water quality is significantly improved in a short time. In addition, MABR sewage treatment process also shows multiple advantages: low cost, low energy consumption, simple and convenient operation. For this reason, MABR sewage treatment process has gradually received widespread attention in the sewage treatment industry. In MABR sewage treatment process, hollow breathable membrane is not only an oxygen supply element, but also a growth carrier of microorganisms, so it is a key component in MABR sewage treatment process. The hollow breathable membrane of the existing MABR sewage treatment process is mostly hydrophobic. The hydrophobic surface of the hollow hydrophobic membrane has a small contact area with water, which reduces the adhesion points of microorganisms and is not conducive to the rapid formation of microbial membranes. Summary of the invention
[0003] In view of this, the present invention proposes a composite membrane for MABR sewage treatment process and a preparation process thereof to solve the above problems.
[0004] The technical solution of the present invention is implemented as follows: a composite membrane for a MABR sewage treatment process, comprising a hollow hydrophobic membrane and a modified layer coated on the hollow hydrophobic membrane; wherein the hollow hydrophobic membrane comprises the following raw materials in parts by weight: 40-60 parts of hydrophobic polyolefin, 6-10 parts of magnetic nanofiller, and 30-40 parts of 1-ethyl-3-methylimidazolium tetrafluoroborate; wherein the modified layer is a collagen layer, comprising the following raw materials in parts by weight: 20-30 parts of collagen powder and 30-60 parts of deionized water.
[0005] Furthermore, the hydrophobic polyolefin is one or a combination of polyethylene, polypropylene, polybutylene, polytetrafluoroethylene, and polyvinylidene fluoride.
[0006] Furthermore, the magnetic nano-filler is one or a combination of nano-ferroferric oxide, nano-nickel ferrite, nano-cobalt ferrite, nano-strontium ferrite, and nano-barium ferrite, and the particle size of the magnetic nano-filler is 50-100nm.
[0007] Furthermore, a process for preparing a composite membrane for a MABR wastewater treatment process comprises the following steps:
[0008] S1. Preparation of casting solution: Add hydrophobic polyolefin, magnetic nanofiller, and 1-ethyl-3-methylimidazolium tetrafluoroborate to a dissolving tank according to weight, stir and mix evenly, purge with inert gas and heat to dissolve. After dissolution, vacuum stand and degas to obtain casting solution.
[0009] S2. Preparation of hollow hydrophobic membrane: Add the casting liquid into the casting equipment, the casting liquid and the cavity forming gas are discharged through the spinneret of the casting equipment, and enter the coagulation bath for solid phase separation to obtain the hollow hydrophobic membrane for standby use.
[0010] S3. Preparation of collagen solution: Mix collagen powder and deionized water according to weight, stir at 300-500 r / min for 20-40 min at 40-60° C. to obtain a collagen solution.
[0011] S4. Formation of collagen layer: seal both ends of the hollow hydrophobic membrane, immerse the hollow hydrophobic membrane in the collagen solution, and coat the surface of the hollow hydrophobic membrane with a collagen layer to obtain a composite membrane.
[0012] S5. Drying treatment: placing the impregnated composite membrane into an oven for drying treatment.
[0013] S6. Surface etching treatment: The composite film after drying is placed in a laser etching machine to perform etching on its surface.
[0014] Furthermore, when heating and dissolving in S1, the heating temperature is 150-200° C. and the dissolving time is 8-12 hours; when standing and degassing, the temperature is 130-160° C. and the pressure is -0.08 to -0.10 MPa for 50-70 minutes.
[0015] Furthermore, the inert gas in S1 and the cavity forming gas in S2 are one of nitrogen, argon and helium.
[0016] Furthermore, in S2, the flow rate of the casting liquid is 1-3 mL / min, the flow rate of the cavity forming gas is 0.5-1.5 mL / min, the pressure of the spinneret is 0.2-0.4 MPa, and the coagulation bath is a water bath, and the water temperature of the water bath is 40-80°C.
[0017] Further, the hollow hydrophobic membrane in S4 is immersed at 35-40° C. for 4-6 h.
[0018] Furthermore, in S5, the drying process is performed, the drying temperature is set to 35-40° C., and the drying time is 3-5 hours.
[0019] Furthermore, in S6, the laser power is set to 10-20 W, the laser frequency is set to 8000-10000 Hz, and the scanning speed is set to 200-400 mm / s.
[0020] Compared with the prior art, the present invention has the following beneficial effects: the present invention increases the surface energy of the composite membrane by adding magnetic nanofillers, increases the surface roughness, causes the contact angle to decrease, improves the hydrophilicity of the surface, and improves the adhesion between the membrane and the biofilm, so that the biofilm formation time is reduced. In addition, the magnetic nanofillers increase the pore size and porosity of the membrane, can form more microchannels, reduce the transmission resistance of oxygen in the membrane, and are conducive to oxygen molecules passing through the membrane layer more easily, thereby improving the oxygen permeability. In addition, the magnetic nanofillers promote the contact and adhesion of microorganisms with the membrane surface through their magnetic attraction. These factors work together to accelerate the formation process of the biofilm, thereby shortening the biofilm formation time. And the distribution and arrangement of microorganisms can be more orderly through the magnetic effect, thereby forming a more stable and efficient biofilm system.
[0021] The present invention forms a composite membrane by modifying a hollow hydrophobic membrane and coating a collagen layer on its surface, thereby changing the hydrophilicity of the membrane surface and making it more hydrophilic. The improvement of hydrophilicity can promote the dissolved oxygen and organic matter in the sewage to pass through the membrane layer faster, react with the microorganisms in the biofilm, and facilitate the removal of pollutants. By coating the membrane surface with a collagen layer, the biocompatibility of the membrane is improved, which helps the attachment and growth of microorganisms on the membrane surface, thereby forming a more stable and efficient biofilm. At the same time, the collagen layer provides a more favorable growth environment for microorganisms, accelerates the formation of biofilms, and thus improves the efficiency and stability of sewage treatment.
[0022] The etching treatment of the present invention changes the wettability and charge characteristics of the composite membrane surface, thereby reducing the contact angle. The etching treatment forms a tiny concave-convex structure on the membrane surface, increases the surface roughness of the membrane, and also increases the specific surface area of the membrane, providing more contact points for oxygen, thereby enhancing the oxygen permeability. Through the etching treatment, tiny textures and grooves are created on the membrane surface, providing more attachment points for microorganisms, which is conducive to the formation and stability of the biofilm and reduces the biofilm hanging time. The surface structure formed by the etching treatment also affects the flow state of water when it passes through the membrane surface, reduces the water flow resistance, improves the efficiency of fluid passing through the membrane, and is conducive to the removal of pollutants. DETAILED DESCRIPTION
[0023] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.
[0024] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.
[0025] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.
[0026] Example 1
[0027] A composite membrane for an MABR sewage treatment process comprises a hollow hydrophobic membrane and a modified layer coated on the hollow hydrophobic membrane; wherein the hollow hydrophobic membrane comprises the following raw materials in parts by weight: 40 parts of hydrophobic polyolefin, which is polyethylene, 6 parts of magnetic nanofiller, which is nano-ferrosoferric oxide with a particle size of 50 nm, and 30 parts of 1-ethyl-3-methylimidazole tetrafluoroborate; wherein the modified layer is a collagen layer, comprising the following raw materials in parts by weight: 20 parts of collagen powder and 30 parts of deionized water.
[0028] Example 2
[0029] A composite membrane for an MABR sewage treatment process comprises a hollow hydrophobic membrane and a modified layer coated on the hollow hydrophobic membrane; wherein the hollow hydrophobic membrane comprises the following raw materials in parts by weight: 60 parts of hydrophobic polyolefin, which is a combination of polypropylene and polytetrafluoroethylene in a mass ratio of 1:1, 10 parts of magnetic nanofillers with a particle size of 100 nm, which is a combination of nano-ferrosoferric oxide and nano-nickel ferrite in a mass ratio of 1:1, and 40 parts of 1-ethyl-3-methylimidazole tetrafluoroborate; wherein the modified layer is a collagen layer, which comprises the following raw materials in parts by weight: 30 parts of collagen powder and 60 parts of deionized water.
[0030] Example 3
[0031] A composite membrane for an MABR sewage treatment process comprises a hollow hydrophobic membrane and a modified layer coated on the hollow hydrophobic membrane; wherein the hollow hydrophobic membrane comprises the following raw materials in parts by weight: 50 parts of hydrophobic polyolefin, which is a combination of polybutene and polyvinylidene fluoride in a mass ratio of 1:1, 8 parts of magnetic nanofillers with a particle size of 75 nm, which is a combination of nano-ferrosoferric oxide and nano-cobalt ferrite in a mass ratio of 1:1, and 35 parts of 1-ethyl-3-methylimidazole tetrafluoroborate; wherein the modified layer is a collagen layer, which comprises the following raw materials in parts by weight: 25 parts of collagen powder and 45 parts of deionized water.
[0032] The preparation process of a composite membrane for a MABR sewage treatment process described in Examples 1-3 comprises the following steps:
[0033] S1. Preparation of casting solution: Add hydrophobic polyolefin, magnetic nanofiller, and 1-ethyl-3-methylimidazolium tetrafluoroborate to a dissolving tank by weight, stir and mix evenly, purge with inert gas, and heat and dissolve at 175°C for 10 hours, wherein the inert gas is nitrogen. After dissolution, stand and degas for 60 minutes at 145°C and -0.09MPa pressure to obtain casting solution.
[0034] S2. Preparation of hollow hydrophobic membrane: Add the casting liquid into the film casting equipment, and the casting liquid and the cavity forming gas are discharged through the spinneret of the film casting equipment, wherein the cavity forming gas is nitrogen, the casting liquid flow rate is 2mL / min, the cavity forming gas flow rate is 1mL / min, the spinneret pressure is 0.3MPa and enters into the coagulation bath for solid phase separation, and the coagulation bath is a water bath, and the water temperature of the water bath is 60°C, to obtain a hollow hydrophobic membrane for use.
[0035] S3. Preparation of collagen solution: Mix collagen powder and deionized water according to weight, stir at 400 r / min at 50° C. for 30 min to obtain a collagen solution.
[0036] S4. Formation of collagen layer: seal both ends of the hollow hydrophobic membrane, immerse the hollow hydrophobic membrane in the collagen solution, soak at 38° C. for 5 hours, coat the surface of the hollow hydrophobic membrane with a collagen layer, and obtain a composite membrane.
[0037] S5. Drying treatment: Place the impregnated composite membrane in an oven for drying. The drying temperature is set to 38° C. and the drying time is 4 hours.
[0038] S6. Surface etching treatment: Place the dried composite film in a laser etching machine for etching of its surface. The laser power is set to 15W, the laser frequency is set to 9000Hz, and the scanning speed is set to 300mm / s.
[0039] Example 4
[0040] Compared with Example 3, this example differs in that the preparation process of a composite membrane for a MABR sewage treatment process comprises the following steps:
[0041] S1. Preparation of casting solution: Add hydrophobic polyolefin, magnetic nanofiller, and 1-ethyl-3-methylimidazolium tetrafluoroborate to a dissolving tank by weight, stir and mix evenly, use inert purge and heat to dissolve at 150°C for 12 hours, wherein the inert gas is argon. After the dissolution is completed, stand and degas for 70 minutes at 130°C and -0.08MPa pressure to obtain a casting solution.
[0042] S2. Preparation of hollow hydrophobic membrane: Add the casting liquid into the film casting equipment, and the casting liquid and the cavity forming gas are discharged through the spinneret of the film casting equipment, wherein the cavity forming gas is argon, the casting liquid flow rate is 1mL / min, the cavity forming gas flow rate is 0.5mL / min, the spinneret pressure is 0.24MPa, and enters into the coagulation bath to undergo solid phase separation, and the coagulation bath is a water bath, and the water temperature of the water bath is 40°C, to obtain a hollow hydrophobic membrane for use.
[0043] S3. Preparation of collagen solution: Mix collagen powder and deionized water according to weight, stir at 300 r / min at 40° C. for 40 min to obtain a collagen solution.
[0044] S4. Collagen layer formation: seal both ends of the hollow hydrophobic membrane, immerse the hollow hydrophobic membrane in the collagen solution, soak at 35° C. for 6 hours, coat the surface of the hollow hydrophobic membrane with a collagen layer, and obtain a composite membrane.
[0045] S5. Drying treatment: Place the impregnated composite membrane into an oven for drying treatment, set the drying temperature to 35°C, and dry for 5 hours.
[0046] S6. Surface etching treatment: Place the dried composite film in a laser etching machine for etching of its surface. The laser power is set to 10W, the laser frequency is set to 8000Hz, and the scanning speed is set to 200mm / s.
[0047] Example 5
[0048] Compared with Example 3, this example differs in that the preparation process of a composite membrane for a MABR sewage treatment process comprises the following steps:
[0049] S1. Preparation of casting solution: Add hydrophobic polyolefin, magnetic nanofiller, and 1-ethyl-3-methylimidazolium tetrafluoroborate to a dissolving tank by weight, stir and mix evenly, purge with inert gas, and heat and dissolve at 200°C for 8 hours, wherein the inert gas is helium. After dissolution, stand and degas at 160°C and -0.10MPa pressure for 50 minutes to obtain casting solution.
[0050] S2. Preparation of hollow hydrophobic membrane: Add the casting liquid into the film casting equipment, and the casting liquid and the cavity forming gas are discharged through the spinneret of the film casting equipment, wherein the cavity forming gas is helium, the casting liquid flow rate is 3mL / min, the cavity forming gas flow rate is 1.5mL / min, the spinneret pressure is 0.4MPa, and enters the coagulation bath to undergo solid phase separation, and the coagulation bath is a water bath, and the water temperature of the water bath is 80°C, to obtain a hollow hydrophobic membrane for use.
[0051] S3. Preparation of collagen solution: Mix collagen powder and deionized water according to weight, stir at 500 r / min at 60° C. for 20 min to obtain a collagen solution.
[0052] S4. Formation of collagen layer: seal both ends of the hollow hydrophobic membrane, immerse the hollow hydrophobic membrane in the collagen solution, soak at 40° C. for 4 hours, and coat the surface of the hollow hydrophobic membrane with a collagen layer to obtain a composite membrane.
[0053] S5. Drying treatment: Place the impregnated composite membrane into an oven for drying. The drying temperature is set to 40° C. and the drying time is 3 hours.
[0054] S6. Surface etching treatment: Place the dried composite film in a laser etching machine for etching of its surface. The laser power is set to 20W, the laser frequency is set to 10000Hz, and the scanning speed is set to 400mm / s.
[0055] Comparative Example 1
[0056] This comparative example is compared with Example 3, except that 1-ethyl-3-methylimidazolium tetrafluoroborate is replaced with cyclohexanone in equal parts by weight. That is, the hollow hydrophobic membrane comprises the following raw materials in parts by weight: 50 parts of hydrophobic polyolefin, which is a combination of polybutene and polyvinylidene fluoride in a mass ratio of 1:1, 8 parts of magnetic nanofiller with a particle size of 75 nm, which is a combination of nano-ferrosoferric oxide and nano-cobalt ferrite in a mass ratio of 1:1, and 35 parts of cyclohexanone.
[0057] Comparative Example 2
[0058] Compared with Example 3, the difference between this comparative example and Example 3 is that the raw material of the hollow hydrophobic membrane does not contain magnetic nanofiller, that is, the hollow hydrophobic membrane includes the following raw materials in parts by weight: 50 parts of hydrophobic polyolefin, which is a combination of polybutene and polyvinylidene fluoride in a mass ratio of 1:1, and 35 parts of 1-ethyl-3-methylimidazole tetrafluoroborate.
[0059] Comparative Example 3
[0060] The difference between this comparative example and Example 3 is that no etching treatment is performed on the surface of the composite film, that is, the treatment of step S6 is not performed.
[0061] Comparative Example 4
[0062] Compared with Example 3, the difference between this comparative example and Example 3 is that the collagen layer is not coated on the surface of the hollow hydrophobic membrane. That is, a composite membrane for MABR sewage treatment process is a hollow hydrophobic membrane, comprising the following raw materials in parts by weight: 50 parts of hydrophobic polyolefin, which is a combination of polybutene and polyvinylidene fluoride in a mass ratio of 1:1, 8 parts of magnetic nanofiller with a particle size of 75nm, which is a combination of nano-ferrous oxide and nano-cobalt ferrite in a mass ratio of 1:1, and 35 parts of 1-ethyl-3-methylimidazole tetrafluoroborate.
[0063] The above-mentioned process for preparing a composite membrane for MABR sewage treatment process comprises the following steps:
[0064] S1. Preparation of casting solution: Add hydrophobic polyolefin, magnetic nanofiller, and 1-ethyl-3-methylimidazolium tetrafluoroborate to a dissolving tank by weight, stir and mix evenly, purge with inert gas, and heat and dissolve at 175°C for 10 hours, wherein the inert gas is nitrogen. After dissolution, stand and degas for 60 minutes at 145°C and -0.09MPa pressure to obtain casting solution.
[0065] S2. Preparation of hollow hydrophobic membrane: The casting liquid is added into the film casting equipment, and the casting liquid and the cavity forming gas are discharged through the spinneret of the film casting equipment, wherein the cavity forming gas is nitrogen, the casting liquid flow rate is 2mL / min, the cavity forming gas flow rate is 1mL / min, the spinneret pressure is 0.3MPa and enters into a coagulation bath for solid phase separation, and the coagulation bath is a water bath, and the water temperature of the water bath is 60°C to obtain a hollow hydrophobic membrane.
[0066] S3. Drying treatment: Place the hollow hydrophobic membrane in an oven for drying treatment, set the drying temperature to 38°C, and dry for 4 hours.
[0067] S4. Surface etching treatment: Place the dried hollow hydrophobic membrane into a laser etching machine for etching of its surface. The laser power is set to 15W, the laser frequency is set to 9000Hz, and the scanning speed is set to 300mm / s.
[0068] Performance Testing
[0069] The composite membranes prepared in Examples 1-5 and Comparative Examples 1-4 were measured by contact angle meter in accordance with GB / T 30693-2014 Measurement of contact angle between plastic film and water, oxygen permeability was measured by oxygen permeator in accordance with GB / T 19789-2021 Test method for oxygen permeability of packaging materials-coulometric detection method, and surface roughness was measured by roughness meter in accordance with GB / T 7220-2004 Technical Specification for Geometric Quantity of Products (GPS) Surface Structure Profile Method Surface Roughness Terminology Parameter Measurement, and each example and comparative example was tested 5 times, and the average value was recorded in Table 1. The composite membranes prepared in Examples 1-5 and Comparative Examples 1-4 were respectively placed in MABR bioreactors, and biofilm was formed under the same conditions, and the time required for each composite membrane to form a uniform and dense biofilm was observed and recorded. Each example and comparative example was tested 3 times, and the average value was recorded in Table 1.
[0070] Table 1
[0071]
[0072] It can be seen from Table 1 that the composite membranes prepared in Examples 1-5 of the present invention have short biofilm formation times, and thus can achieve rapid biofilm formation, especially Example 3 which takes the shortest time.
[0073] Compared with Comparative Example 1 through Example 3, 1-ethyl-3-methylimidazole tetrafluoroborate can not only dilute polyolefin but also affect the polarity of the film surface during the film-making process, making the film surface more hydrophilic, that is, reducing the contact angle. 1-ethyl-3-methylimidazole tetrafluoroborate is less volatile, has high thermal stability and good electrical conductivity relative to cyclohexanone, which helps to promote the orderly arrangement of polymer chains during the film-making process, forming a more uniform and stable film structure, thereby forming a more regular film pore, which is conducive to the permeation of oxygen. At the same time, 1-ethyl-3-methylimidazole tetrafluoroborate also reduces the crystallinity of the film during the film-making process, increases the amorphous region, thereby improving the permeability of oxygen. In addition, 1-ethyl-3-methylimidazole tetrafluoroborate increases the polarity of the film surface, making it easier for oxygen molecules to be adsorbed on the film surface and permeate the film layer. Due to good oxygen permeability and small contact angle, it is conducive to the adsorption and biofilm of microorganisms, so the biofilm time of Example 3 is shorter than the time used in Comparative Example 1.
[0074] Compared with comparative example 2 by embodiment 3, the addition of magnetic nano filler increases the surface energy of the membrane, resulting in a decrease in the contact angle. Due to its high specific surface area and special physical properties, the magnetic nano filler can enhance the polarity of the membrane surface and improve the hydrophilicity of the surface. In addition, the addition of magnetic nano filler changes the microstructure of the membrane surface, making the membrane surface rough, and further reducing the contact angle. The magnetic nano filler forms tiny protrusions and depressions on the membrane surface, thereby increasing the roughness of the membrane surface, helping to improve the adhesion between the membrane and the biofilm, and is conducive to the reduction of the biofilm time. In addition, the magnetic nano filler increases the pore size and porosity of the membrane, can form more tiny channels, reduce the transmission resistance of oxygen in the membrane, and is conducive to oxygen molecules passing through the membrane layer more easily, thereby improving oxygen permeability. Because the magnetic nano filler increases the roughness and hydrophilicity of the membrane surface, microorganisms are more likely to adhere to the membrane surface. In addition, the magnetic nano filler promotes the contact and adhesion of microorganisms with the membrane surface through its magnetic attraction. These factors work together to accelerate the formation process of the biofilm, thereby shortening the biofilm time. The magnetic effect can make the distribution and arrangement of microorganisms more orderly, thus forming a more stable and efficient biofilm system. Moreover, the addition of magnetic nanofillers can significantly improve the mechanical strength and durability of the membrane, and can enhance the tensile strength and compressive strength of the membrane material, thereby extending the service life of the membrane.
[0075] By comparing Example 3 with Comparative Example 3, the etching treatment changes the wettability and charge characteristics of the membrane surface, thereby reducing the contact angle. The etching treatment forms a tiny concave-convex structure on the surface of the composite membrane, increases the surface roughness of the composite membrane, and also increases the specific surface area of the composite membrane, providing more contact points for oxygen, thereby enhancing the oxygen permeability. The etching treatment creates microscopic textures and grooves on the surface of the composite membrane, which is conducive to the flow of oxygen and improves the oxygen transfer efficiency. Through the etching treatment, tiny textures and grooves are created on the surface of the composite membrane, providing more attachment points for microorganisms, which is conducive to the formation and stability of the biofilm and reduces the biofilm time.
[0076] Compared with comparative example 4 by embodiment 3, collagen layer changes the hydrophilicity of composite membrane surface, makes it more hydrophilic, so contact angle is reduced.At the same time, the improvement of hydrophilicity can promote dissolved oxygen and organic matter in sewage to pass through membrane layer faster, react with microorganisms in biofilm, and be conducive to the removal of pollutants.Composite membrane is formed by coating collagen layer on membrane surface, improves the biocompatibility of composite membrane, helps microorganisms to adhere and grow on composite membrane surface, so as to form more stable and more efficient biofilm.At the same time, collagen layer provides more favorable growth environment for microorganisms, accelerates the formation of biofilm, and then improves the efficiency and stability of sewage treatment.Although the roughness of composite membrane surface coated collagen layer is reduced, due to the reduction of contact angle and the improvement of biocompatibility, the overall biofilm time is greatly reduced compared with comparative example 4.In addition, collagen layer may also reduce the wear and tear on composite membrane surface, improve the durability of composite membrane.
[0077] Pollutant removal test
[0078] The composite membranes prepared in Examples 1-5 and Comparative Examples 1-4 were respectively placed in MABR bioreactors to treat domestic sewage in a certain area of Hainan Province. After 30 days of operation, the removal rates of COD, ammonia nitrogen, total nitrogen and total phosphorus were tested. The results are shown in Table 2.
[0079] Table 2
[0080]
[0081] It can be seen from Table 2 that the composite membrane prepared by the present invention has a good removal effect on COD, ammonia nitrogen, total nitrogen and total phosphorus.
[0082] The present invention uses 1-ethyl-3-methylimidazolium tetrafluoroborate as a diluent raw material, adds magnetic nanofillers, modifies the membrane surface by coating a collagen layer, and uses etching to treat the composite membrane surface. Multiple means effectively form a uniform and stable biofilm on the composite membrane surface, greatly improving the removal effect of COD, ammonia nitrogen, total nitrogen, and total phosphorus in sewage. The nanomagnetic fillers in the composite membrane promote the movement of ions and molecules in the water through the magnetic field, thereby accelerating the migration of pollutants to the membrane surface and further improving the removal efficiency. The surface structure formed by the etching treatment also affects the flow state of water when it passes through the composite membrane surface, reduces water flow resistance, improves the efficiency of fluid passing through the membrane, and is conducive to the removal of pollutants. At the same time, the collagen layer enhances the removal effect of pollutants in sewage through its unique physical and chemical properties, such as adsorption and complexation. The solution of the present invention is integrated, synergistic and efficient. Through the joint action of multiple means, the COD removal rate reaches 93.1-95.7%, the ammonia nitrogen removal rate reaches 90.0-92.5%, the total nitrogen removal rate reaches 84.1-86.7%, and the total phosphorus removal rate reaches 83.9-85.9%, with excellent pollutant removal effect.
[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite membrane for MABR sewage treatment process, characterized in that: It comprises a hollow hydrophobic membrane and a modified layer coated on the hollow hydrophobic membrane; the hollow hydrophobic membrane comprises the following raw materials in parts by weight: 40-60 parts of hydrophobic polyolefin, 6-10 parts of magnetic nanofiller, and 30-40 parts of 1-ethyl-3-methylimidazole tetrafluoroborate; the modified layer is a collagen layer, comprising the following raw materials in parts by weight: 20-30 parts of collagen powder and 30-60 parts of deionized water.
2. A composite membrane for MABR sewage treatment process according to claim 1, characterized in that: The hydrophobic polyolefin is one or a combination of polyethylene, polypropylene, polybutylene, polytetrafluoroethylene, and polyvinylidene fluoride.
3. A composite membrane for MABR sewage treatment process according to claim 1, characterized in that: The magnetic nano filler is one or a combination of nano ferroferric oxide, nano nickel ferrite, nano cobalt ferrite, nano strontium ferrite and nano barium ferrite, and the particle size of the magnetic nano filler is 50-100nm.
4. The process for preparing a composite membrane for a MABR sewage treatment process according to claim 1, characterized in that: The following steps are involved: S1. Preparation of casting solution: Add hydrophobic polyolefin, magnetic nanofiller, and 1-ethyl-3-methylimidazolium tetrafluoroborate to a dissolving tank by weight, stir and mix evenly, purge with inert gas and heat to dissolve; after dissolution, stand in vacuum to degas to obtain a casting solution; S2. Preparation of a hollow hydrophobic membrane: The casting liquid is added to a casting device, the casting liquid and the cavity gas are discharged through a spinneret of the casting device, and enter a solidification bath for solid phase separation to obtain a hollow hydrophobic membrane for standby use; S3. Preparation of collagen solution: Mix collagen powder and deionized water by weight, stir at 300-500 r / min for 20-40 min at 40-60° C. to obtain a collagen solution; S4. Collagen layer formation: sealing both ends of the hollow hydrophobic membrane, immersing the hollow hydrophobic membrane in the collagen solution, coating the surface of the hollow hydrophobic membrane with a collagen layer to obtain a composite membrane; S5. Drying treatment: placing the impregnated composite film into an oven for drying; S6. Surface etching treatment: placing the composite film after the drying treatment into a laser etching machine to perform etching treatment on its surface.
5. A process for preparing a composite membrane for a MABR sewage treatment process as claimed in claim 4, characterized in that: In the S1, the heating temperature for dissolving is 150-200° C. and the dissolving time is 8-12 hours; and the degassing is performed at 130-160° C. and a pressure of -0.08 to -0.10 MPa for 50-70 minutes.
6. A process for preparing a composite membrane for a MABR sewage treatment process as claimed in claim 4, characterized in that: The inert gas in S1 and the cavity forming gas in S2 are one of nitrogen, argon and helium.
7. The process for preparing a composite membrane for a MABR sewage treatment process according to claim 4, characterized in that: The flow rate of the casting liquid in S2 is 1-3 mL / min, the flow rate of the cavity forming gas is 0.5-1.5 mL / min, the pressure of the spinneret is 0.2-0.4 MPa, the coagulation bath is a water bath, and the water temperature of the water bath is 40-80°C.
8. The process for preparing a composite membrane for a MABR sewage treatment process according to claim 4, characterized in that: The S4 is immersed at 35-40° C. for 4-6 hours.
9. The process for preparing a composite membrane for a MABR sewage treatment process according to claim 4, characterized in that: In the drying process in S5, the drying temperature is set to 35-40° C. and the drying time is 3-5 hours.
10. The process for preparing a composite membrane for a MABR sewage treatment process according to claim 4, characterized in that: In the S6, the laser power is set to 10-20 W, the laser frequency is set to 8000-10000 Hz, and the scanning speed is set to 200-400 mm / s.