Biomass charcoal material catalyst, preparation method and application thereof, and acetylene hydrochlorination reaction catalysis method

By supporting active components such as palladium chloride, ruthenium chloride and platinum chloride on biomass carbon materials, an efficient catalyst was prepared, which solved the problem of low catalytic performance of acetylene hydrochlorination reaction, and achieved efficient catalysis and green chemical engineering goal.

CN118988294APending Publication Date: 2024-11-22XINJIANG UNIVERSITY

Patent Information

Application Number
CN202411079887.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing biomass carbon-based catalysts have low catalytic performance on the acetylene hydrochlorination reaction, and traditional catalysts such as Hg are highly toxic and resource-deficient.

Method used

Using biomass carbon materials as support, supporting active components such as palladium chloride, ruthenium chloride and platinum chloride, and preparing catalysts with high specific surface area and pore structure through activation and carbonization treatment, and improving the active group through ultrasonic impregnation technology The carrier adhesion of the fraction is used for acetylene hydrochlorination reaction.

Benefits of technology

It significantly improves the catalytic activity and selectivity of the acetylene hydrochlorination reaction, saves the cost of catalyst preparation, and provides an economically feasible way to recover and utilize agricultural waste, responding to the needs of green chemical development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004985810460000011
    Figure HDA0004985810460000011
  • Figure HDA0004985810460000012
    Figure HDA0004985810460000012
  • Figure HDA0004985810460000021
    Figure HDA0004985810460000021
Patent Text Reader

Abstract

The invention belongs to the technical field of catalytic materials, and particularly relates to a biomass charcoal material catalyst, a preparation method and application thereof, and a catalytic method of acetylene hydrochlorination reaction. The biomass charcoal material catalyst provided by the invention comprises biomass charcoal and active components loaded on the surface and in pores of the biomass charcoal, wherein the active components comprise one or more of palladium chloride, ruthenium chloride and platinum chloride, and the biomass charcoal material catalyst has excellent catalytic performance on acetylene hydrochlorination reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalytic materials, and in particular relates to a biomass carbon material catalyst, a preparation method and application thereof, and a catalytic method for acetylene hydrochlorination reaction. Background Art

[0002] Biomass refers to various organisms produced through photosynthesis, which are renewable resources. They mainly include plants, microorganisms, animals that feed on plants and microorganisms, and their waste products, such as crops, crop waste (such as crop straw, plant shells), wood, and animal manure. Every year, a large amount of agricultural waste is directly incinerated or buried, causing resource waste and environmental pollution. Therefore, the efficient utilization of agricultural waste is of great significance to improving the ecological environment and solving the problem of resource shortage.

[0003] Among agricultural wastes, crop straw accounts for the largest proportion, and among the efficient utilization methods of crop straw, it is mainly used to prepare biochar materials. In recent years, biochar materials have attracted much attention, and relevant research has been carried out both at home and abroad. Biochar materials are solid products after biomass pyrolysis. The biomass raw materials are heated for a specific time at the optimal heating rate and optimal temperature under aerobic or anaerobic conditions. The process mainly follows the chemical, heat transfer and mass transfer processes. At present, the preparation methods of biochar materials mainly include direct carbonization method, physical activation method, template method and chemical activation method. Among them, the chemical activation method is often used in the preparation of biochar materials because of its low activation temperature, short activation time, easy control of activation reaction, and the prepared biochar materials have the advantages of developed pore structure and large specific surface area.

[0004] Vinyl chloride (VCM) is an important synthetic monomer for polyvinyl chloride (PVC). Currently, the acetylene method (full name "acetylene hydrochlorination method") is mainly used to synthesize vinyl chloride. Hg catalyst is the key technology for the acetylene method to synthesize vinyl chloride. Since Hg is highly toxic and harmful to both the human body and the environment, and Hg resources are scarce, the development of mercury-free catalysts is currently the main research direction for the acetylene method to synthesize vinyl chloride. In the development process of catalysts, catalyst carriers play a vital role in the performance of catalysts. Biomass carbon materials (such as walnut shells, soybean meal, wheat flour, bamboo powder) have been used in the research of mercury-free catalysts for acetylene hydrochlorination reactions due to their high specific surface area, controllable pore structure, and good thermal stability. However, the catalytic performance of biomass carbon-based catalysts for acetylene hydrochlorination reactions is currently low. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a biomass carbon material catalyst and its preparation method and application, and a catalytic method for acetylene hydrochlorination reaction. The biomass carbon material catalyst provided by the present invention has excellent catalytic performance for acetylene hydrochlorination reaction.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a biomass carbon material catalyst, comprising biomass carbon and an active component loaded on the surface and pores of the biomass carbon:

[0008] The active component includes one or more of palladium chloride, ruthenium chloride and platinum chloride.

[0009] Preferably, the mass ratio of the active component to the biochar is 0.1 to 10:100.

[0010] Preferably, the specific surface area of ​​the biomass carbon material catalyst is greater than 1000m 2 / g.

[0011] Preferably, the method for preparing biochar comprises the following steps:

[0012] After the biomass and the solution of the activator are mixed and activated, a first washing and a first drying are performed in sequence to obtain a biomass activated material;

[0013] After the biomass activated material is carbonized, a second washing, a second drying and a screening are performed in sequence to obtain the biomass charcoal.

[0014] Preferably, the activator includes one or more of hydrochloric acid, phosphoric acid, sulfuric acid, potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, sodium bicarbonate, potassium permanganate, zinc chloride and ferric chloride.

[0015] Preferably, the biomass includes crop straws; the crop straws include one or more of cotton straws, corn straws, wheat straws, rice straws, highland barley straws and soybean straws.

[0016] Preferably, the carbonization temperature is 300-700° C., and the insulation time is 2-10 hours.

[0017] The present invention also provides a method for preparing the biomass carbon material catalyst described in the above technical solution, comprising the following steps:

[0018] The biomass carbon is immersed in a solution of active components and subjected to ultrasound, and then allowed to stand and dried for a third time in sequence to obtain the biomass carbon material catalyst.

[0019] The present invention also provides the use of the biomass carbon material catalyst described in the above technical solution or the biomass carbon material catalyst prepared by the preparation method described in the above technical solution in the acetylene hydrochlorination reaction.

[0020] The present invention also provides a catalytic method for acetylene hydrochlorination reaction, comprising the following steps: introducing a mixed gas of hydrogen chloride and acetylene into a fixed bed reactor provided with a catalyst to carry out acetylene hydrochlorination reaction to obtain vinyl chloride and recover the catalyst respectively;

[0021] The catalyst is the biomass carbon material catalyst described in the above technical solution or the biomass carbon material catalyst prepared by the preparation method described in the above technical solution.

[0022] The present invention provides a biomass carbon material catalyst, comprising biomass carbon and active components loaded on the surface and pores of the biomass carbon: the active components include one or more of palladium chloride, ruthenium chloride and platinum chloride. The biomass carbon in the biomass carbon material catalyst provided by the present invention has the characteristics of large specific surface area, developed pore structure and strong adsorption capacity, and can adsorb more active substances. By using the biomass carbon as a carrier and loading the active substances, an acetylene hydrochlorination reaction catalyst with excellent performance can be prepared.

[0023] The present invention also provides a method for preparing the above-mentioned biomass carbon material catalyst. The present invention uses agricultural waste biomass as a raw material to prepare biomass carbon, and uses it as a carrier to load active components to prepare a biomass carbon material catalyst. It is economically feasible and low-cost, and not only provides a way to recycle agricultural waste, but also significantly improves the recycling and utilization value of agricultural waste. In addition, the prepared biomass carbon material is used as a carrier to prepare a catalyst through a simple preparation method. It is applied to acetylene hydrochlorination reaction and has excellent catalytic activity and selectivity, which saves the cost of catalyst preparation and responds to the needs of green chemical development. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the pore size distribution curve of the biomass carbon material in Example 1;

[0025] Figure 2 This is a morphology diagram of the biomass carbon material in Example 1;

[0026] Figure 3 The XRD spectra of the biomass carbon material and the catalyst before and after the reaction in Example 1;

[0027] Figure 4 This is the morphology of cotton stalk charcoal without activation treatment in Comparative Example 1;

[0028] Figure 5 This is the morphology of bamboo charcoal after activation treatment in Comparative Example 2. DETAILED DESCRIPTION

[0029] The present invention provides a biomass carbon material catalyst, comprising biomass carbon and an active component loaded on the surface and pores of the biomass carbon:

[0030] The active component includes one or more of palladium chloride, ruthenium chloride and platinum chloride.

[0031] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used in the preparation, and commercially available products known to those skilled in the art can be used.

[0032] The biomass carbon material catalyst provided by the present invention includes biomass carbon.

[0033] In the present invention, the method for preparing biochar preferably comprises the following steps:

[0034] After the biomass and the solution of the activator are mixed and activated, a first washing and a first drying are performed in sequence to obtain a biomass activated material;

[0035] After the biomass activated material is carbonized, a second washing, a second drying and a screening are performed in sequence to obtain the biomass charcoal.

[0036] In the present invention, the biomass preferably includes crop straw; the crop straw preferably includes one or more of cotton straw, corn straw, wheat straw, rice straw, highland barley straw and soybean straw, more preferably cotton straw; the biomass is preferably biomass powder; the particle size of the biomass powder is preferably 1 to 5 mm, more preferably 1 to 2 mm; the preparation method of the biomass powder is preferably: cutting, cleaning, drying and crushing the biomass in sequence to obtain the biomass powder; the drying temperature is preferably 60 to 105°C, more preferably 70 to 90°C; the drying is preferably drying to constant weight. The present invention does not specifically limit the process of cutting, cleaning and crushing, and the process of cutting, cleaning and crushing well known in the art can be used. In an embodiment of the present invention, the cleaning is specifically repeated cleaning with deionized water.

[0037] In the present invention, the activator preferably includes one or more of hydrochloric acid, phosphoric acid, sulfuric acid, potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, sodium bicarbonate, potassium permanganate, zinc chloride and ferric chloride, more preferably phosphoric acid or zinc chloride; the mass concentration of the activator in the solution of the activator is preferably 10-90%, more preferably 30-70%. In the present invention, the activator plays a role in dehydrating and forming pores for the biomass raw material during the activation process.

[0038] In the present invention, the mass of the activator is preferably 1 to 20 times the mass of the biomass, more preferably 2 to 4 times; the activation time is preferably 10 to 40 hours, more preferably 20 to 30 hours; the activation is preferably carried out under natural conditions; the cleaning agent used for the first cleaning is preferably deionized water; the first cleaning is preferably cleaned to neutrality; the temperature of the first drying is preferably 60 to 105°C, more preferably 70 to 90°C; the first drying is preferably dried to constant weight.

[0039] In the present invention, the carbonization temperature is preferably 300-700°C, more preferably 400-600°C, the holding time is preferably 2-10h, more preferably 2-5h; the heating rate to the carbonization temperature is preferably 1-20°C / min, more preferably 5-10°C / min; the carbonization is preferably carried out under a protective atmosphere; the protective atmosphere is preferably nitrogen; after the carbonization, the present invention preferably cools the carbonized product naturally to room temperature.

[0040] The carbonization process in the present invention is the process of preparing biomass raw materials into corresponding biomass carbon materials, which involves dehydration, pore formation and decomposition of cellulose, hemicellulose and lignin in biomass. The biomass carbon obtained after carbonization has a certain pore structure, mechanical strength and adsorption performance.

[0041] In the present invention, the cleaning agents used in the second cleaning are preferably anhydrous ethanol and deionized water, or hydrochloric acid solution and deionized water in sequence; the concentration of the hydrochloric acid solution is preferably 0.2 mol / L; the second cleaning is preferably cleaned to neutrality; the temperature of the second drying is preferably 60 to 105°C, more preferably 70 to 90°C; the second drying is preferably dried to constant weight; the aperture of the sieve used for the screening is preferably 20 to 200 meshes, more preferably 60 to 100 meshes. The present invention does not specifically limit the screening process, and the screening process well known in the art can be used.

[0042] In the present invention, the mass ratio of the active component to the biochar is preferably 0.1 to 10:100, more preferably 0.5 to 5:100.

[0043] In the present invention, the specific surface area of ​​the biomass carbon material catalyst is preferably greater than 1000m 2 / g, more preferably 1000 to 1500 m 2 / g, and most preferably 1000 to 1300 m 2 / g.

[0044] The present invention also provides a method for preparing the biomass carbon material catalyst described in the above technical solution, comprising the following steps:

[0045] The biomass carbon is immersed in a solution of active components and subjected to ultrasound, and then allowed to stand and dried for a third time in sequence to obtain the biomass carbon material catalyst.

[0046] In the present invention, the mass concentration of the active component in the solution of the active component is preferably 0.1-10%, more preferably 0.3-0.5%; the power of the ultrasound is preferably 150-350W, more preferably 200-250W; the temperature of the ultrasound is preferably 15-35°C, more preferably 20-25°C; the time of the ultrasound is preferably 0.5-1.5h, more preferably 1h; the standing time is preferably 8-16h, more preferably 12h; the temperature of the third drying is preferably 60-90°C, more preferably 70°C; the time of the third drying is preferably 8-16h, more preferably 10-12h. The present invention uses ultrasound to allow the active component to enter the pores of the biomass carbon carrier.

[0047] The present invention also provides the use of the biomass carbon material catalyst described in the above technical solution or the biomass carbon material catalyst prepared by the preparation method described in the above technical solution in the acetylene hydrochlorination reaction.

[0048] The present invention also provides a catalytic method for acetylene hydrochlorination reaction, comprising the following steps: introducing a mixed gas of hydrogen chloride and acetylene into a fixed bed reactor provided with a catalyst to carry out acetylene hydrochlorination reaction to obtain vinyl chloride and recover the catalyst respectively;

[0049] The catalyst is the biomass carbon material catalyst described in the above technical solution or the biomass carbon material catalyst prepared by the preparation method described in the above technical solution.

[0050] In the present invention, the volume ratio of hydrogen chloride to acetylene in the hydrogen chloride and acetylene mixture is preferably 1 to 2:1, more preferably 1.25:1; the space velocity of the hydrogen chloride and acetylene mixture is preferably 30 to 3000 h -1 , more preferably 120h -1 The temperature of the acetylene hydrochlorination reaction is preferably 90 to 300°C, more preferably 160°C; the acetylene hydrochlorination reaction is preferably carried out under normal pressure.

[0051] In the present invention, the conversion rate of acetylene is preferably 88-100%, more preferably 99-99.9%; the selectivity of vinyl chloride is preferably 98-100%, more preferably 99%.

[0052] The present invention preferably reuses the recovered catalyst for acetylene hydrochlorination reaction; the number of reuses is preferably ≤ 8 times, more preferably 5 times. The biomass carbon material catalyst in the present invention can be reused, and after being reused 8 times, the maximum acetylene conversion rate is reduced from 99.9% to 85%.

[0053] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention, but they should not be construed as limiting the protection scope of the present invention.

[0054] Example 1

[0055] Weigh 15.00 g of the main part of biomass straw (cotton straw), cut it in sequence, wash it with deionized water, dry it at 70°C to constant weight, crush it into biomass powder with a particle size of 1 to 2 mm, and mix it with phosphoric acid (85wt%) at a mass ratio of 1:20, activate it under natural conditions for 30 hours, wash off the surface phosphoric acid with deionized water, and dry it at 70°C to constant weight to obtain a biomass activated material;

[0056] The activated biomass material was placed in a tubular furnace, heated to 400°C at 10°C / min for 2h in a nitrogen atmosphere for carbonization, cooled naturally to room temperature, washed with anhydrous ethanol and deionized water in sequence until neutral, dried at 70°C to constant weight, and sieved with a sieve aperture of 100 mesh to obtain biomass charcoal;

[0057] The biochar was immersed in a palladium chloride solution (mass fraction of 0.5wt%), ultrasonicated at 25°C with a power of 250W for 1h, allowed to stand for 12h, and dried at 70°C for 12h to obtain a biochar material catalyst, in which the mass percentage of the active component palladium chloride was 0.5% (mass of active component: mass of biochar = 0.5:100).

[0058] Example 2

[0059] Weigh 15.00 g of the main part of biomass straw (cotton straw), cut it in sequence, wash it with deionized water, dry it at 70°C to constant weight, grind it into biomass powder with a particle size of (1-2 mm), and mix it with phosphoric acid (85wt%) at a mass ratio of 1:X (X=1 / 2 / 3 / 4), activate it under natural conditions for 24 hours, and dry it in an oven at 70°C to constant weight to obtain biomass activated material;

[0060] The activated biomass material was placed in a tubular furnace, heated to 400°C at 10°C / min for 2h in a nitrogen atmosphere for carbonization, cooled naturally to room temperature, washed with hydrochloric acid solution (concentration of 0.2mol / L) and deionized water in sequence until neutral, dried at 70°C to constant weight, and sieved with a sieve aperture of 100 mesh to obtain biochar;

[0061] The biochar was immersed in a palladium chloride solution (mass fraction of 0.5wt%), ultrasonicated at 25°C with a power of 250W for 1h, allowed to stand for 12h, and dried at 70°C for 12h to obtain a biochar material catalyst, in which the mass percentage of the active component palladium chloride was 0.5% (mass of active component: mass of biochar = 0.5:100).

[0062] Example 3

[0063] Weigh 15.00 g of the main part of biomass straw (cotton straw), cut it in sequence, wash it with deionized water, dry it at 70°C to constant weight, and then grind it into biomass powder with a particle size of 1 to 2 mm, and mix it with phosphoric acid (10wt% / 30wt% / 50wt% / 70wt%) at a mass ratio of 1:4, activate it under natural conditions for 24 hours, and dry it in an oven at 70°C to constant weight to obtain biomass activated material;

[0064] The activated biomass material was placed in a tubular furnace, heated to 400°C at 10°C / min for 2h in a nitrogen atmosphere for carbonization, cooled naturally to room temperature, washed with hydrochloric acid solution (concentration of 0.2mol / L) and deionized water in sequence until neutral, dried at 70°C to constant weight, and sieved with a sieve aperture of 100 mesh to obtain biochar;

[0065] The biochar was immersed in a palladium chloride solution (mass fraction of 0.5wt%), ultrasonicated at 25°C with a power of 250W for 1h, allowed to stand for 12h, and dried at 70°C for 12h to obtain a biochar material catalyst, in which the mass percentage of the active component palladium chloride was 0.5% (mass of active component: mass of biochar = 0.5:100).

[0066] Example 4

[0067] Weigh 15.00 g of the main part of biomass straw (cotton straw), cut it in sequence, wash it with deionized water, dry it at 70°C to constant weight, crush it into biomass powder with a particle size of 1 to 2 mm, and mix it evenly with a zinc chloride solution (20wt%), the mass ratio of biomass powder to zinc chloride solid is 1:1, activate it under natural conditions for 24 hours, and dry it at 70°C to constant weight to obtain a biomass activated material;

[0068] The activated biomass material was placed in a tubular furnace, heated to 400°C at 10°C / min for 2h in a nitrogen atmosphere for carbonization, cooled naturally to room temperature, washed with anhydrous ethanol and deionized water in sequence until neutral, dried at 70°C to constant weight, and sieved with a sieve aperture of 100 mesh to obtain biomass charcoal;

[0069] The biochar was immersed in a palladium chloride solution (mass fraction of 0.5wt%), ultrasonicated at 25°C with a power of 250W for 1h, allowed to stand for 12h, and dried at 70°C for 12h to obtain a biochar material catalyst, in which the mass percentage of the active component palladium chloride was 0.5% (mass of active component: mass of biochar = 0.5:100).

[0070] Example 5

[0071] Weigh 15.00 g of the main part of biomass straw (cotton straw), cut it in sequence, wash it with deionized water, dry it at 70°C to constant weight, crush it into biomass powder with a particle size of 1 to 2 mm, and mix it evenly with a potassium hydroxide solution (20wt%), the mass ratio of biomass powder to potassium hydroxide solid is 1:1, activate it under natural conditions for 24 hours, and dry it at 70°C to constant weight to obtain a biomass activated material;

[0072] The activated biomass material was placed in a tubular furnace, heated to 400°C at 10°C / min for 2h in a nitrogen atmosphere for carbonization, cooled naturally to room temperature, washed with anhydrous ethanol and deionized water in sequence until neutral, dried at 70°C to constant weight, and sieved with a sieve aperture of 100 mesh to obtain biomass charcoal;

[0073] The biochar was immersed in a palladium chloride solution (mass fraction of 0.5wt%), ultrasonicated at 25°C with a power of 250W for 1h, allowed to stand for 12h, and dried at 70°C for 12h to obtain a biochar material catalyst, in which the mass percentage of the active component palladium chloride was 0.5% (mass of active component: mass of biochar = 0.5:100).

[0074] Comparative Example 1

[0075] The difference from Example 1 is that the activation process is not performed, and the remaining steps are the same as those in Example 1.

[0076] Comparative Example 2

[0077] The difference from Example 1 is that the biomass raw material is bamboo powder, the activator is zinc chloride, and acrylamide is used as a nitrogen source, and no metal active components are added. The specific preparation steps are as follows: the bamboo powder is dried at 80°C for 24h as a carbon source, zinc chloride and acrylamide are weighed and dissolved in water (the mass ratio of zinc chloride to acrylamide to bamboo powder is 1:1), the mixed liquid is added dropwise to the bamboo powder, and after immersion for 8h, it is dried at 80°C for 12h, and the dried sample is calcined at 700°C in an inert atmosphere for 2h, and washed with 2mol / L dilute hydrochloric acid and distilled water in turn to remove zinc chloride and impurities, and the nitrogen-doped carbon catalyst is obtained after drying at 80°C. The reaction is carried out at a reaction temperature of 200°C and an acetylene space velocity of 1.0mL / (min·g).

[0078] Application Example 1

[0079] The biomass carbon material catalyst prepared in Example 1 was placed in a fixed bed reactor, and a mixed gas of hydrogen chloride and acetylene was introduced to carry out acetylene hydrochlorination reaction to obtain vinyl chloride. The acetylene hydrochlorination reaction conditions were: normal pressure, a space velocity of the mixed gas of 120h -1 The volume ratio of hydrogen chloride and acetylene is V(HCl):V(C 2 H 2 )=1.25:1, reaction temperature is 160°C, and the activity of the catalyst in acetylene hydrochlorination reaction is evaluated, the conversion rate of acetylene is 99.9%, and the selectivity of vinyl chloride is 99%.

[0080] Application Example 2

[0081] The difference from Application Example 1 is that the biomass carbon material catalyst prepared in Example 1 is replaced by the biomass carbon material catalyst prepared in Example 2, and the activity of these catalysts in acetylene hydrochlorination reaction is evaluated. The highest acetylene conversion rate is 99.9%, and the highest selectivity of vinyl chloride is 99%.

[0082] Application Example 3

[0083] The difference from Application Example 1 is that the biomass carbon material catalyst prepared in Example 1 is replaced by the biomass carbon material catalyst prepared in Example 3, and the activity of these catalysts in acetylene hydrochlorination reaction is evaluated. The highest acetylene conversion rate is 99.9%, and the highest selectivity of vinyl chloride is 99%.

[0084] Application Example 4

[0085] The difference from Application Example 1 is that the biomass carbon material catalyst prepared in Example 1 is replaced by the biomass carbon material catalyst prepared in Example 4. The activity of the catalyst in acetylene hydrochlorination reaction is evaluated, and the conversion rate of acetylene is 99.06%, and the selectivity of vinyl chloride is 99%.

[0086] Application Example 5

[0087] The difference from Application Example 1 is that the biomass carbon material catalyst prepared in Example 1 is replaced by the biomass carbon material catalyst prepared in Example 5. The activity of the catalyst in acetylene hydrochlorination reaction is evaluated, and the conversion rate of acetylene is 88%, and the selectivity of vinyl chloride is 98%.

[0088] Comparative application example 1

[0089] The difference from Application Example 1 is that the biomass carbon material catalyst prepared in Example 1 is replaced by the biomass carbon material catalyst prepared in Comparative Example 1, and the activity of the catalyst in acetylene hydrochlorination reaction is evaluated, and the conversion rate of acetylene is 15%, and the selectivity of vinyl chloride is 95%.

[0090] Comparative Application Example 2

[0091] The difference from Application Example 1 is that the biomass carbon material catalyst prepared in Example 1 is replaced by the biomass carbon material catalyst prepared in Comparative Example 2, and the activity of the catalyst in acetylene hydrochlorination reaction is evaluated, and the conversion rate of acetylene is 85%, and the selectivity of vinyl chloride is 88%.

[0092] The acetylene conversion rate and vinyl chloride selectivity of the catalysts prepared in Comparative Examples 1 and 2 are both inferior to those in Application Example 1.

[0093] Performance Testing

[0094] Figure 1 This is a pore size distribution curve of the biomass carbon (PCBC) in Example 1, see Table 1 for details.

[0095] Table 1 shows the specific surface area and pore structure distribution results of biochar in Example 1

[0096] sample <![CDATA[Specific surface area / m 2 ·g -1 > <![CDATA[Total pore volume / cm 3 ·g -1 > Average pore size / nm Biomass charcoal (PCBC) 1306.88 1.229 3.76

[0097] Depend on Figure 1 It can be seen from the BET characterization results that PCBC exhibits a large specific surface area and total pore volume, with a specific surface area of ​​1306.88 m 2 ·g -1 , the total pore volume reaches 1.229cm 3 ·g -1 In addition, the pore size distribution curve and the average pore size (3.76nm) show that PCBC is mainly composed of mesopores and mesopores. These conditions lay the foundation for PCBC to be an ideal catalyst carrier material.

[0098] Figure 2 is the morphology of the biomass charcoal (PCBC) in Example 1. Figure 2 It can be seen from the SEM characterization results that PCBC has a smooth surface, rich pore structure, and relatively uniform pore distribution. This provides the basic conditions for PCBC to be used as a catalyst carrier material. The SEM characterization results are consistent with the BET characterization results.

[0099] Figure 3 The XRD spectra of the biomass carbon (PCBC) and the biomass carbon material catalyst (PCBC@Pd) before and after the reaction in Example 1 are shown in FIG. Figure 3It can be seen from the XRD characterization results: the material was diffracted in the range of 10-80°, and the sample showed broad peaks at around 2θ=24° and 44°, which is consistent with the (002) and (101) crystal planes in graphite, indicating that the sample is mainly amorphous. It can be judged that the material is a carbon material with an amorphous structure, which can meet the conditions for being a catalyst carrier.

[0100] Figure 4 This is the morphology of the cotton stalk carbon without activation treatment in Comparative Example 1. Figure 4 It can be seen that the surface of cotton stalk charcoal that has not undergone activation treatment is relatively rough, with only some pores and uneven pore size distribution, which does not meet the basic conditions for being a catalyst carrier.

[0101] Figure 5 This is the morphology of bamboo charcoal after activation treatment in Comparative Example 2. Figure 5 It can be seen that the surface of bamboo powder charcoal is relatively smooth and has more microtubular structures. This special structure can increase the specific surface area of ​​the material and meet the basic conditions for being a catalyst carrier, but it is not the optimal morphological feature of the catalyst carrier.

[0102] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A biomass carbon material catalyst, characterized in that: It includes biomass charcoal and active components loaded on the surface and pores of the biomass charcoal: The active component includes one or more of palladium chloride, ruthenium chloride and platinum chloride.

2. The biomass carbon material catalyst according to claim 1, characterized in that: The mass ratio of the active component to the biochar is 0.1 to 10:

100.

3. The biomass carbon material catalyst according to claim 1, characterized in that: The specific surface area of ​​the biomass carbon material catalyst is greater than 1000m 2 / g.

4. The biomass carbon material catalyst according to any one of claims 1 to 3, characterized in that: The method for preparing biochar comprises the following steps: After the biomass and the solution of the activator are mixed and activated, a first washing and a first drying are performed in sequence to obtain a biomass activated material; After the biomass activated material is carbonized, a second washing, a second drying and a screening are performed in sequence to obtain the biomass charcoal.

5. The biomass carbon material catalyst according to claim 4, characterized in that: The activator includes one or more of hydrochloric acid, phosphoric acid, sulfuric acid, potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, sodium bicarbonate, potassium permanganate, zinc chloride and ferric chloride.

6. The biomass carbon material catalyst according to claim 4, characterized in that: The biomass includes crop straws; the crop straws include one or more of cotton straws, corn straws, wheat straws, rice straws, highland barley straws and soybean straws.

7. The biomass carbon material catalyst according to claim 4, characterized in that: The carbonization temperature is 300-700° C., and the heat preservation time is 2-10 hours.

8. The method for preparing the biomass carbon material catalyst according to any one of claims 1 to 7, characterized in that: The following steps are involved: The biomass carbon is immersed in a solution of active components and subjected to ultrasound, and then allowed to stand and dried for a third time in sequence to obtain the biomass carbon material catalyst.

9. Use of the biomass carbon material catalyst according to any one of claims 1 to 7 or the biomass carbon material catalyst prepared by the preparation method according to claim 8 in acetylene hydrochlorination reaction.

10. A catalytic method for acetylene hydrochlorination, characterized in that: The following steps are involved: Passing a mixed gas of hydrogen chloride and acetylene into a fixed bed reactor provided with a catalyst to carry out acetylene hydrochlorination reaction to obtain vinyl chloride and recover the catalyst respectively; The catalyst is the biomass carbon material catalyst according to any one of claims 1 to 7 or the biomass carbon material catalyst prepared by the preparation method according to claim 8.

Citation Information

Patent Citations

  • Mercury-free catalyst system for acetylene hydrochlorination and use thereof

    CN102380380A

  • Carbon-material supported catalyst for acetylene hydrochlorinate reaction

    CN103495416A

  • Biochar, biochar-based multifunctional soil remediation agent and preparation method of biochar

    CN110734348A

  • Biomass-based nitrogen-doped carbon catalyst and preparation method and application thereof

    CN111450860A

  • Biochar material rich in microporous structure and adjustable in pore volume as well as preparation method and application of biochar material

    CN115709980A

Cited By

  • Preparation method of fishpond filtering composite carbon material and fishpond filtering composite carbon material

    CN121405499A

  • Preparation method of fish pond filtering composite carbon material and fish pond filtering composite carbon material

    CN121405499B

  • Method for applying nitrogen-doped biomass charcoal material to acetylene hydrochlorination

    CN121607179A