Preparation method of VOCs oxidation catalyst
Through the combination of multi-stage pore structure support and metal active components of spherical molecular sieve, a VOCs oxidation catalyst with high reactivity and moisture resistance was prepared, which solved the problem of insufficient catalyst activity and water resistance in the prior art, and achieved different Efficient and selective removal of VOCs.
Patent Information
- Application Number
- CN202310554004.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-17
AI Technical Summary
The existing VOCs oxidation catalysts have shortcomings in terms of reactivity and water resistance, especially in the face of different VOCs contamination sources, which lack the selective catalytic oxidation capacity of large and small molecular components.
Spherical molecular sieve is used to form a multi-stage pore structure support through hydrothermal reaction, and use metals such as manganese, cobalt, iron or copper as active components to prepare VOCs oxidation catalysts through impregnation and calcination steps to adjust the pore volume of mesoporous and micropores The valence state of metal is increased to improve the reactivity and moisture resistance of the catalyst.
The reactivity of the catalyst and the VOCs removal efficiency are significantly improved, and the selective catalysis of different VOCs is achieved, especially the efficient removal performance in high humidity environments.
Smart Images

Figure BDA0004232320820000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field related to environmental protection and air pollution control, and also belongs to the technical field related to catalysts, and specifically relates to a method for preparing a VOCs oxidation catalyst. Background Art
[0002] Volatile Organic Compounds (VOCs) refer to organic compounds with a saturated vapor pressure greater than 70Pa at room temperature and a boiling point of less than 260°C at normal pressure. VOCs are a common air pollutant, mainly from industries such as printing, coating, pharmaceuticals, furniture manufacturing, and petrochemicals. Most of these organic waste gases are flammable and explosive, and are often accompanied by odors and stench in the air. At low solubility, they can irritate the human eyes, nose, and respiratory system, and can even induce cancer and mutations in the human body.
[0003] Commonly used VOCs emission reduction technologies include adsorption condensation, direct oxidation, catalytic combustion, photocatalytic oxidation and biofiltration membrane. Catalytic combustion refers to the process of flameless combustion of VOCs components in exhaust gas at a relatively low ignition temperature (<500°C) in the presence of a catalyst, and complete oxidation of the components into CO2 and H2O. This method has the characteristics of low auxiliary fuel cost, low operating temperature, small equipment size, high purification efficiency, low energy consumption and no secondary pollution. It is one of the most promising VOCs pollution control technologies. The development of an efficient catalytic combustion catalyst is one of the keys to the widespread application of this technology in VOCs pollution treatment.
[0004] CN113401918A relates to a Ag removal method for removing sulfur-containing volatile organic matter + Loaded multi-level pore molecular sieve, preparation method and application thereof. The microporous molecular sieve is modified by alkali treatment to form a mesoporous structure inside. Ion exchange loading Ag + , with both mesoporous and microporous structures and loaded with Ag + In the USY molecular sieve, the silicon-aluminum molar ratio is 10-30, and the specific surface area is 500-1000m 2 ·g -1 The ratio of the pore volume of the mesoporous structure to the pore volume of the microporous structure is 0.5-2.5.
[0005] CN104174425A relates to a catalyst for catalytic oxidation of volatile organic compounds and a preparation method thereof. The active component of the catalyst is Pd or Pt, and the carrier is a molecular sieve such as multi-level pore SBA-15 or KIT-6 with a macroporous-mesoporous structure.
[0006] CN113184878A relates to a multi-level pore zeolite molecular sieve and its preparation method and application. Na-SSZ-13 zeolite is first treated with alkali solution, and then pickled with acid solution to obtain a multi-level pore zeolite molecular sieve. Small molecular amine compounds occupy the interior of the zeolite pores by pre-adsorption to form an "inner protection" layer to resist the rapid diffusion and disordered etching of alkali in the zeolite micropores, so that the SSZ-13 zeolite is treated with alkali to construct multi-level pores while its zeolite skeleton can be better protected.
[0007] There is a continuous demand for improvement in VOCs oxidation catalysts in this field, especially improving the reaction activity and water resistance of the catalyst, as well as improving the selective catalytic oxidation ability of the catalyst for large molecular components and small molecular components when facing different VOCs pollution sources. Summary of the invention
[0008] In view of the problems existing in the above-mentioned prior art, the present invention provides a method for preparing a VOCs oxidation catalyst. The catalyst prepared by the method of the present invention improves the reaction activity and water resistance of the catalyst and realizes the efficient removal of specific volatile organic compounds.
[0009] To achieve its purpose, the present invention adopts the following technical solutions:
[0010] In one aspect of the present invention, a method for preparing a VOCs oxidation catalyst is provided, comprising the following steps:
[0011] (1) immersing the spherical molecular sieve in a mixed solution of alkali and sodium silicate for hydrothermal reaction to obtain a spherical molecular sieve carrier with a multi-level pore structure and drying the carrier;
[0012] (2) placing the spherical molecular sieve carrier obtained in step (1) in a precursor salt solution containing an active component for immersion to obtain a molecular sieve carrier loaded with a precursor salt;
[0013] (3) drying and calcining the molecular sieve carrier loaded with the precursor salt obtained in step (2) to obtain the VOCs oxidation catalyst;
[0014] The active component is one or more of manganese, cobalt, iron and copper.
[0015] In a specific embodiment of the present invention, in step (1), the spherical molecular sieve is one or more of CHA type zeolite molecular sieve, MFI type zeolite molecular sieve and BEA type zeolite molecular sieve.
[0016] In a preferred embodiment of the present invention, the CHA type zeolite molecular sieve is SSZ-13 zeolite molecular sieve and / or SAPO zeolite molecular sieve, the MFI type zeolite molecular sieve is ZSM-5 zeolite molecular sieve and / or S-1 zeolite molecular sieve, and the BEA type zeolite molecular sieve is Beta zeolite molecular sieve (β molecular sieve).
[0017] In a specific embodiment of the present invention, in step (1), the diameter of the spherical molecular sieve is 2-5 mm, for example, about 2 mm, about 3 mm, about 4 mm, about 5 mm, etc.
[0018] In a preferred embodiment of the present invention, the spherical molecular sieve is ultrasonically washed with water to remove surface impurities before use.
[0019] In a specific embodiment of the present invention, in step (1), the base is one or more of an organic amine (such as methylamine, ethanolamine, aniline, ethylenediamine, etc.), sodium hydroxide and potassium hydroxide.
[0020] In a specific embodiment of the present invention, in step (1), the mass fraction of alkali in the mixed solution is 1-5%, for example, 2%, 3%, 4%, etc.; the mass fraction of sodium silicate is 2-10%, for example, 3%, 4%, 5%, 6%, 7%, 8%, 9%, etc.; the mass ratio of spherical molecular sieve to the mixed solution is 1-1:3, for example, 1:2.
[0021] In a preferred embodiment of the present invention, in step (1), the pH value of the mixed solution is 11-14, such as 12, 13, etc.
[0022] In a specific embodiment of the present invention, in step (1), the temperature of the hydrothermal reaction is 80-200°C, for example, 100°C, 120°C, 140°C, 160°C, 180°C, etc.; the time is 5-168h, for example, 10h, 25h, 50h, 75h, 100h, 125h, 150h, etc.
[0023] In a specific embodiment of the present invention, in step (1), the mass loss of the spherical molecular sieve is controlled to be 1-3%, such as 2%.
[0024] In a specific embodiment of the present invention, in step (1), the silicon-aluminum ratio of the obtained spherical molecular sieve carrier is 100-300, such as 150, 200, 250, etc.
[0025] In a specific embodiment of the present invention, in step (1), the mesopore volume of the obtained spherical molecular sieve carrier accounts for 10%-50% of the total pore volume, for example, 15%, 20%, 25%, 30%, 35%, 40%, 45%, etc.
[0026] In a specific embodiment of the present invention, in step (2), the manganese salt in the precursor salt solution is one or more of manganese nitrate, manganese chloride, manganese acetate and manganese sulfate; the cobalt salt is one or more of cobalt nitrate, cobalt chloride, cobalt acetate and cobalt sulfate; the iron salt is one or more of ferric nitrate, ferric chloride, ferrous chloride, ferrous sulfate, ferric acetate and ferric sulfate; the copper salt is one or more of copper nitrate, copper chloride, copper acetate and copper sulfate.
[0027] In a specific embodiment of the present invention, in step (2), the concentration of the precursor saline solution is 0.001-0.03M, more preferably 0.0025-0.005M, for example 0.0015M, 0.002M, 0.0035M, 0.004M, 0.0045M, 0.0055M, 0.01M, 0.015M, 0.02M, 0.025M, etc.
[0028] In a specific embodiment of the present invention, in step (2), the mass ratio of the precursor salt solution to the spherical molecular sieve carrier is 15-40:1, preferably 20-30:1, such as 25:1.
[0029] In a specific embodiment of the present invention, in step (2), the immersion time is 0.5-5h, for example, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, etc.; the immersion liquid temperature is 40-80°C, for example, 50°C, 60°C, 70°C, etc.
[0030] In a specific embodiment of the present invention, in step (3), the drying temperature is 50-120° C., and the drying time is 2-10 h; the roasting temperature is 400-600° C., and the roasting time is 3-8 h.
[0031] In another aspect of the present invention, it relates to a VOCs oxidation catalyst obtained according to the above preparation method.
[0032] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in the following aspects:
[0033] The catalyst with the meso-micro multi-level pore structure molecular sieve as a carrier prepared by the present invention can improve the catalyst reaction activity, improve the VOCs removal efficiency, and significantly reduce T90;
[0034] Microporous channels can achieve selective adsorption and removal of VOCs, and improve the dispersibility of active components by anchoring active components, thereby improving the VOCs removal efficiency; mesoporous channels can shorten the mass transfer path, increase the specific surface area and pore volume, increase the VOCs adsorption rate, and increase the adsorption capacity;
[0035] Without being bound by any theory, the inventors have found that when the pore volume ratio of mesopores and micropores is relatively high and / or the metal is in a higher valence state, a higher removal effect is achieved for macromolecular organic substances such as toluene; when the pore volume ratio of mesopores and micropores is relatively low and / or the metal is in a lower valence state, a higher removal effect is achieved for small molecular organic substances such as ethylene, and the process of the present invention can achieve the adjustment of the pore volume ratio of mesopores and micropores and / or the valence state of the metal;
[0036] The microporous channels are conducive to the desorption of water molecules in the micropores, improving the moisture resistance of the molecular sieve, and can be used for VOCs removal in high humidity environments; by introducing sodium silicate, the silicon-aluminum ratio is further increased, which increases the moisture resistance of the molecular sieve and can be used for the selective removal of VOCs in high-humidity flue gas. DETAILED DESCRIPTION
[0037] The present invention is further described below in conjunction with embodiments, but the present invention is not limited to the listed embodiments, and should also include equivalent improvements and modifications of the technical solutions defined in the claims attached to the present application.
[0038] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0039] raw material
[0040] Molecular sieves were purchased from Tianjin Nanhua Catalyst Co., Ltd., MFI type zeolite molecular sieves selected ZSM-5 zeolite molecular sieves, and BEA type zeolite molecular sieves selected Beta zeolite molecular sieves; organic amines (including ethanolamine H2NCH2CH2OH, ethylenediamine H2NCH2CH2NH2), sodium silicate, sodium hydroxide and inorganic salts (such as manganese nitrate, iron nitrate and copper nitrate) were purchased from Sinopharm Chemical Reagent Co., Ltd. Unless otherwise specified, the raw materials appearing in this article are all conventional commercially available raw materials.
[0041] Test Method
[0042] Silicon-aluminum ratio measurement: using high-resolution solid MAS 29 The Si-NMR method is used to determine the framework silicon-to-aluminum ratio of the molecular sieve, and the solid nuclear magnetic resonance spectrum simulation program can automatically calculate the framework silicon-to-aluminum ratio.
[0043] Mesopore and micropore volume test of molecular sieve: N2 was used as the adsorption medium, and the micropores and mesopores were measured by BET physical adsorption instrument.
[0044] Valence state analysis of metal elements: The valence state of metal elements on the catalyst surface was analyzed by X-ray photoelectron spectroscopy (XPS).
[0045] Catalyst component analysis: The content of metal oxides in the catalyst was analyzed by X-ray fluorescence spectroscopy (XRF).
[0046] Detection of ethylene and toluene concentrations at the inlet and outlet of the reaction device: The ethylene and toluene concentrations at the inlet and outlet of the reaction device are detected by a Fourier infrared multi-component gas analyzer.
[0047] Example
[0048] Example 1
[0049] (1) 10 g of spherical molecular sieve (ZSM-5, silicon-aluminum ratio of 20) with a diameter of 2 mm was ultrasonically washed with clean water to remove surface impurities; the washed spherical molecular sieve was immersed in a mixed solution of sodium hydroxide (mass fraction of 1%) and sodium silicate (mass fraction of 2%), and the mixed solution was placed in a reactor for hydrothermal reaction at a temperature of 80° C. for a reaction time of 5 h, wherein the mass ratio of the spherical molecular sieve to the mixed solution was 1:1, and a spherical molecular sieve carrier with a multi-level pore structure was obtained, which was dried for standby use; the mass loss of the obtained spherical molecular sieve carrier was about 1%, the silicon-aluminum ratio was about 100, and the mesopore volume accounted for about 10% of the total pore volume;
[0050] (2) The spherical molecular sieve carrier with a multi-level pore structure was immersed in 200 mL of an aqueous solution of manganese nitrate (molar concentration of 0.0025 M) for 30 min, the immersion liquid temperature was 40 ° C, the mass ratio of the manganese nitrate aqueous solution to the spherical molecular sieve carrier was 20:1, and the molecular sieve carrier loaded with the precursor salt was taken out;
[0051] (3) The molecular sieve carrier loaded with the precursor salt was placed in an oven at 50° C. for 10 h and then calcined in a tube furnace at 400° C. for 3 h to obtain a VOCs oxidation catalyst.
[0052] After XRF composition analysis, MnO x Accounting for 2% of the catalyst mass, XPS detected Mn 4+ / Mn(total) is 30%, Mn 3+ / Mn(total) is 40%, Mn 2+ / Mn(total) is 30%.
[0053] Example 2
[0054] (1) 10 g of spherical molecular sieve (Beta molecular sieve, silicon-aluminum ratio of 20) with a diameter of 2 mm was ultrasonically washed with clean water to remove surface impurities; the washed spherical molecular sieve was immersed in a mixed solution of sodium hydroxide (mass fraction of 5%) and sodium silicate (mass fraction of 10%), and the mixed solution was placed in a reactor for hydrothermal reaction at a temperature of 200° C. for a reaction time of 168 h, wherein the mass ratio of the spherical molecular sieve to the mixed solution was 1:3, and a spherical molecular sieve carrier with a multi-level pore structure was obtained, which was dried for standby use; the mass loss of the obtained spherical molecular sieve carrier was about 3%, the silicon-aluminum ratio was about 300, and the mesopore volume accounted for about 50% of the total pore volume;
[0055] (2) The spherical molecular sieve carrier with a multi-level pore structure was immersed in 200 mL of an aqueous solution of manganese nitrate (molar concentration of 0.005 M) for 5 h, the immersion temperature was 80 ° C, the mass ratio of the manganese nitrate aqueous solution to the spherical molecular sieve carrier was 30:1, and the molecular sieve carrier loaded with the precursor salt was taken out;
[0056] (3) The molecular sieve carrier loaded with the precursor salt was placed in an oven and dried at 120° C. for 2 h, and then placed in a tube furnace and calcined at 600° C. for 8 h to obtain a VOCs oxidation catalyst.
[0057] After XRF composition analysis, MnO x Accounting for 5% of the catalyst mass, Mn 4+ / Mn(total) is 50%, Mn 3 + / Mn(total) is 30%, Mn 2+ / Mn(total) is 20%.
[0058] Example 3
[0059] The catalyst was prepared in the same manner as in Example 1, except that:
[0060] The washed spherical molecular sieve and the mixed solution were placed in a reactor for hydrothermal reaction at a temperature of 150°C and a reaction time of 80 h;
[0061] The spherical molecular sieve carrier with a multi-level pore structure was immersed in 200 mL of an aqueous solution of manganese nitrate (molar concentration of 0.0025 M) and ferric nitrate (molar concentration of 0.0025 M) for 30 min. The immersion liquid temperature was 40 ° C. The mass ratio of the aqueous solution to the spherical molecular sieve carrier was 20:1. The molecular sieve carrier loaded with the precursor salt was taken out.
[0062] The mass loss of the prepared spherical molecular sieve carrier is about 1.5%, the silicon-aluminum ratio is about 120, and the mesopore volume accounts for about 15%.
[0063] After XRF composition analysis, MnO x 2.5% of the catalyst mass, FeO x It accounts for 0.5% of the catalyst mass. After XPS detection, Mn 4+ / Mn(total) is 30%, Mn 3+ / Mn(total) is 40%, Mn 2+ / Mn(total) is 30%.
[0064] Example 4
[0065] The catalyst was prepared by the same method as in Example 2, except that the washed spherical molecular sieve was immersed in a mixed solution of ethanolamine (mass fraction 4%) and sodium silicate (mass fraction 8%); and the mass ratio of the manganese nitrate aqueous solution to the spherical molecular sieve carrier was 28:1.
[0066] The mass loss of the prepared spherical molecular sieve carrier is about 2.8%, the silicon-aluminum ratio is about 270, and the mesopore volume accounts for about 45%.
[0067] After XRF composition analysis, MnO x It accounts for 4.5% of the catalyst mass. After XPS detection, Mn 4+ / Mn(total) is 50%, Mn 3+ / Mn(total) is 30%, Mn 2+ / Mn(total) is 20%.
[0068] Example 5
[0069] The catalyst was prepared by the same method as in Example 1, except that the washed spherical molecular sieve was immersed in a mixed solution of ethylenediamine (3% by mass) and sodium silicate (5% by mass).
[0070] The mass loss of the prepared spherical molecular sieve carrier is about 1.2%, the silicon-aluminum ratio is about 110, and the mesopore volume accounts for about 12%.
[0071] After XRF composition analysis, MnO x It accounts for 2.0% of the catalyst mass. After XPS detection, Mn 4+ / Mn(total) is 50%, Mn 3+ / Mn(total) is 30%, Mn 2+ / Mn(total) is 20%.
[0072] Example 6
[0073] The catalyst was prepared in the same manner as in Example 2, except that:
[0074] (2) The spherical molecular sieve carrier with a multi-level pore structure is immersed in 200 mL of an aqueous solution of manganese nitrate (molar concentration of 0.003 M) and copper nitrate (molar concentration of 0.003 M) for 2 h, the immersion liquid temperature is 60 ° C, the mass ratio of the manganese nitrate aqueous solution to the spherical molecular sieve carrier is 30:1, and the molecular sieve carrier loaded with the precursor salt is taken out;
[0075] (3) The molecular sieve carrier loaded with the precursor salt was placed in an oven and dried at 120° C. for 2 h, and then placed in a tube furnace and calcined at 600° C. for 5 h to obtain a VOCs oxidation catalyst.
[0076] The mass loss of the prepared spherical molecular sieve carrier is about 3%, the silicon-aluminum ratio is about 300, and the mesopore volume accounts for about 50%.
[0077] After XRF composition analysis, MnO x CuO accounts for 4.6% of the catalyst mass x It accounts for 1.0% of the catalyst mass. After XPS detection, Mn 4+ / Mn(total) is 40%, Mn 3+ / Mn(total) is 32%, Mn 2+ / Mn(total) is 28%.
[0078] Comparative Example 1
[0079] The preparation of spherical molecular sieve carriers having a multi-level pore structure is not carried out.
[0080] (1) 10 g of spherical molecular sieve (ZSM-5, silicon-aluminum ratio of 20) with a diameter of 2 mm was immersed in 200 mL of an aqueous solution of manganese nitrate (molar concentration of 0.0025 M) for 30 min, the immersion solution temperature was 40° C., the mass ratio of the manganese nitrate aqueous solution to the spherical molecular sieve carrier was 20:1, and a molecular sieve carrier loaded with a precursor salt was obtained; the silicon-aluminum ratio was 20; and the mesopore volume accounted for 0%;
[0081] (2) The molecular sieve carrier loaded with the precursor salt was dried at 100° C. for 2 h, and calcined in a tube furnace at 400° C. for 3 h to obtain a catalyst.
[0082] After XRF composition analysis, MnO x It accounts for 2% of the catalyst mass. After XPS detection, Mn 4+ / Mn(total) is 30%, Mn 3 + / Mn(total) is 40%, Mn 2+ / Mn(total) is 30%.
[0083] Comparative Example 2
[0084] The catalyst was prepared by the same method as in Example 1, except that only sodium hydroxide solution (mass fraction 1%) was used in the hydrothermal reaction in step (1), and sodium silicate was not included. The mass loss of the prepared spherical molecular sieve carrier was about 1%, the silicon-aluminum ratio was about 20, and the mesopore volume accounted for about 10% of the total pore volume. After XRF composition analysis, MnO x Accounting for 2% of the catalyst mass, XPS detected Mn 4+ / Mn(total) is 30%, Mn 3+ / Mn(total) is 40%, Mn 2+ / Mn(total) is 30%.
[0085] After the catalysts in the above examples and comparative examples were obtained, the catalyst performance test was carried out under the following test conditions.
[0086] Test conditions:
[0087] The VOCs flue gas composition is ethylene 800ppm, toluene 800ppm, O2 3%, H2O 5%, and the rest is nitrogen. Space velocity: 20000h -1 , measure the removal rate of VOCs at 200℃, 250℃, and 300℃. Sampling points are configured at the inlet and outlet of the reaction device, and the concentrations of ethylene and toluene at the inlet and outlet are tested to calculate the removal rate. Calculation formula: Ethylene removal rate = 1-(C 进口C2H4 -C 出口C2H4 ) / C 进口C2H4 ; Toluene removal rate = 1-(C 进口C7H8 -C 出口C7H8 ) / C 进口C7H8 The results are shown in Table 1 below.
[0088] Table 1
[0089]
[0090] Although the present invention has been described in detail for the purpose of illustration in the foregoing text, it should be understood that these detailed descriptions are only for illustration and can be modified by those skilled in the art without departing from the spirit and scope of the present invention. The present invention is limited only by the claims.
Claims
1. A method for preparing a VOCs oxidation catalyst, comprising the following steps: (1) immersing the spherical molecular sieve in a mixed solution of alkali and sodium silicate for hydrothermal reaction to obtain a spherical molecular sieve carrier with a multi-level pore structure and drying the carrier; (2) placing the spherical molecular sieve carrier obtained in step (1) in a precursor salt solution containing an active component for immersion to obtain a molecular sieve carrier loaded with a precursor salt; (3) drying and calcining the molecular sieve carrier loaded with the precursor salt obtained in step (2) to obtain the VOCs oxidation catalyst; The active component is one or more of manganese, cobalt, iron and copper.
2. The preparation method according to claim 1, wherein In step (1), The spherical molecular sieve is one or more of CHA type zeolite molecular sieve, MFI type zeolite molecular sieve and BEA type zeolite molecular sieve; preferably, the CHA type zeolite molecular sieve is SSZ-13 zeolite molecular sieve and / or SAPO zeolite molecular sieve, the MFI type zeolite molecular sieve is ZSM-5 zeolite molecular sieve and / or S-1 zeolite molecular sieve, and the BEA type zeolite molecular sieve is Beta zeolite molecular sieve.
3. According to the preparation method of claim 1 or 2, the diameter of the spherical molecular sieve is 2-5 mm; preferably, the spherical molecular sieve is ultrasonically washed with water to remove surface impurities before use.
4. The preparation method according to any one of claims 1 to 3, wherein In step (1), The base is one or more of an organic amine, sodium hydroxide and potassium hydroxide; The mass fraction of the alkali in the mixed solution is 1-5%, the mass fraction of the sodium silicate is 2-10%, and the mass ratio of the spherical molecular sieve to the mixed solution is 1-1:
3.
5. The preparation method according to any one of claims 1 to 4, wherein In step (1), the temperature of the hydrothermal reaction is 80-200° C. and the time is 5-168 hours.
6. The preparation method according to any one of claims 1 to 5, wherein In step (1), The mass loss of spherical molecular sieve is controlled to 1-3%; The silicon-aluminum ratio of the obtained spherical molecular sieve carrier is 100-300; The pore volume of the mesopores in the obtained spherical molecular sieve carrier accounts for 10%-50% of the total pore volume.
7. The preparation method according to any one of claims 1 to 6, wherein In step (2), The manganese salt in the precursor salt solution is one or more of manganese nitrate, manganese chloride, manganese acetate and manganese sulfate; the cobalt salt is one or more of cobalt nitrate, cobalt chloride, cobalt acetate and cobalt sulfate; the iron salt is one or more of ferric nitrate, ferric chloride, ferrous chloride, ferrous sulfate, ferric acetate and ferric sulfate; the copper salt is one or more of copper nitrate, copper chloride, copper acetate and copper sulfate; The concentration of the precursor saline solution is 0.001-0.03M, more preferably 0.0025-0.005M; The mass ratio of the precursor salt solution to the spherical molecular sieve carrier is 15-40:1, preferably 20-30:
1.
8. The preparation method according to any one of claims 1 to 7, wherein In step (2), the immersion time is 0.5-5 hours, and the immersion liquid temperature is 40-80°C.
9. The preparation method according to any one of claims 1 to 8, wherein In step (3), the drying temperature is 50-120° C., and the drying time is 2-10 hours; the roasting temperature is 400-600° C., and the roasting time is 3-8 hours.
10. The VOCs oxidation catalyst obtained according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Base metal load type multistage pore zeolite molecular sieve catalyst of efficient catalytic combustion soot particles and preparation and application of catalyst
CN104383962A
Preparation method for supported catalyst for catalyzing combustion of VOCs (Volatile Organic Compounds)
CN105879901A
Catalyst for catalytic oxidation of ethylene and preparation method thereof
CN112642468A
VOCs catalytic oxidation catalyst and preparation method and application thereof
CN112844459A
Cited By
VOCs catalyst as well as preparation method and application thereof
CN119869598A