Battery positive electrode material, preparation method and application thereof, and magnesium ion battery
The battery positive electrode material is prepared by solid-phase sintering method of magnesium, vanadium, manganese sources and dispersant, which solves the problems of magnesium ion polarization and oxide film in magnesium ion batteries, and improves the charge and discharge performance and cycle life of magnesium ion batteries.
Patent Information
- Application Number
- CN202410642318.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The polarization effect of magnesium ions is high, which leads to the barrier of the insertion and release of magnesium ions, which in turn hinders the reduction of the charge and discharge performance and cycle life of magnesium ion batteries. In addition, metal magnesium will produce an oxide film in the electrolyte, affecting the performance of the battery.
The battery positive electrode material is prepared by solid-phase sintering method of magnesium source, vanadium source, manganese source and dispersant. The electronic structure is adjusted through the multivalent conversion capability of vanadium source and manganese source, and the polarization of magnesium ions embedded/detached is reduced, and the polarization of magnesium ions is reduced through The coating of dispersant promotes chemical reactions, forms an optimized positive electrode material structure, and solves the oxide film problem.
It improves the charging and discharging performance and cycle life of magnesium ion batteries, ensures the embedding and disengagement of magnesium ions, reduces polarization, and extends the service life of the battery.
Smart Images

Figure CN118993152A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of magnesium ion batteries, and in particular relates to a battery positive electrode material, a preparation method and application thereof, and a magnesium ion battery. Background Art
[0002] Lithium metal is the main raw material for preparing secondary rechargeable batteries, but lithium metal is expensive and scarce; moreover, when lithium metal is prepared into lithium-ion batteries, in order to reduce costs, it is usually necessary to increase the content of heavy metal nickel in the battery, which will cause environmental pollution.
[0003] Magnesium metal has similar chemical properties to lithium metal, but it is cheap, abundant and less polluting. If magnesium metal can be used to replace scarce lithium metal to prepare secondary rechargeable batteries, it will be of great significance in reducing battery costs and alleviating environmental pollution.
[0004] However, the polarization of magnesium ions is high, which is not conducive to the embedding and extraction of magnesium ions. At the same time, magnesium metal has a relatively active chemical property, which will produce an oxide film in the electrolyte, thereby hindering the embedding and extraction of magnesium ions. The obstruction of the embedding and extraction of magnesium ions will lead to a decrease in the charge and discharge performance and cycle life of magnesium ion batteries, further limiting the application of magnesium ion batteries. Summary of the invention
[0005] The object of the present invention is to provide a battery positive electrode material and a preparation method and application thereof, and a magnesium ion battery. When the battery positive electrode material prepared by the present invention is applied to a magnesium ion battery, it is beneficial to the embedding and extraction of magnesium ions, solves the problem of polarization of magnesium ions and generation of oxide film, and is beneficial to improving the charge and discharge performance and cycle life of the magnesium ion battery.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a positive electrode material for a battery, comprising the following steps:
[0008] A magnesium source, a vanadium source, a manganese source and a dispersant are mixed and solid-phase sintered to obtain the battery positive electrode material.
[0009] Preferably, the magnesium source is magnesium oxide; the vanadium source is at least one of vanadium trioxide and vanadium pentoxide; and the manganese source is manganese dioxide.
[0010] Preferably, the molar ratio of the magnesium source, the vanadium source and the manganese source is 1.33-1.4:1.47-1.57:0.1-0.4.
[0011] Preferably, the dispersant is stearic acid.
[0012] Preferably, the temperature of the solid phase sintering is 100-120°C, the holding time is 5-6h, and the heating rate to the solid phase sintering temperature is 20-25°C / h; the solid phase sintering is carried out in a nitrogen atmosphere; the volume concentration of the nitrogen is ≥98%.
[0013] The present invention provides a battery positive electrode material prepared by the preparation method described in the above technical solution.
[0014] Preferably, the chemical formula of the battery positive electrode material is Mg 1.33~1.4 V 1.47~1.57 Mn 0.1~0.4 O4.
[0015] Preferably, the chemical formula of the battery positive electrode material is Mg 1.33 V 1.57 Mn 0.1 O4 or Mg 1.33 V 1.47 Mn 0.2 O4.
[0016] The present invention provides application of the battery positive electrode material described in the above technical solution in a magnesium ion battery.
[0017] The present invention provides a magnesium ion battery, wherein the electrode active material of the positive electrode plate of the magnesium ion battery comprises the battery positive electrode material described in the above technical solution.
[0018] The present invention provides a method for preparing a positive electrode material for a battery, comprising the following steps: mixing a magnesium source, a vanadium source, a manganese source and a dispersant, and performing solid phase sintering to obtain the positive electrode material for the battery. In the present invention, the magnesium source, the vanadium source and the manganese source provide raw materials for the positive electrode material for the battery, wherein the vanadium in the vanadium source has different valence states (such as V 3+ 、V 4+ 、V 5+ etc.), the manganese in the manganese source also has different valence states (such as Mn 2+ , Mn 3+ , Mn 4+The vanadium source and the manganese source have strong multivalent state conversion capabilities, which are conducive to the rapid transfer of electrons / ions, can adjust the electronic structure of the obtained battery positive electrode material, reduce the polarization of magnesium ion embedding / ejection, and can also enhance the electrochemical activity of the obtained battery positive electrode material in the magnesium ion battery as a whole; the dispersant can coat the raw materials, which is convenient for subsequent solid phase sintering; solid phase sintering can promote chemical reactions between the raw materials to form the required positive electrode material phase, and at the same time, optimize the structure and electrochemical properties of the obtained battery positive electrode material, ensure that the raw materials are evenly dispersed, and remove impurities. The preparation method provided by the present invention is simple and suitable for large-scale production. When the battery positive electrode material prepared by the present invention is applied to a magnesium ion battery, it is conducive to the embedding and extraction of magnesium ions, solves the problems of polarization of magnesium ions and the generation of oxide film, and is conducive to improving the charge and discharge performance and cycle life of the magnesium ion battery.
[0019] Furthermore, the present invention uses magnesium oxide, vanadium trioxide and manganese dioxide as raw materials, uses stearic acid as a dispersant, and adopts a dispersant coating and solid phase sintering synthesis process to prepare a battery positive electrode material (such as Mg 1.33 V 1.47 Mn 0.2 O4). The embodiment shows that the battery positive electrode material prepared by the present invention is in granular form, with a particle size of ≤1μm, and the particles are evenly distributed, crystal clear, and have good morphology. The battery positive electrode material prepared by the present invention is used as a positive electrode material to assemble a magnesium ion battery and then perform a performance test. The results show that the first discharge capacity of the magnesium ion battery obtained by the present invention is 256mAh / g; as the magnesium ion battery is charged and discharged multiple times, that is, Mg 2+ After multiple extraction and embedding reactions, the capacity of the magnesium-ion battery undergoes a significant attenuation change. At the 9th cycle, the specific capacity of the magnesium-ion battery decreases by about 20 mAh / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 This is a SEM image of the battery positive electrode material obtained in Example 1;
[0022] Figure 2 The cycle life results of the positive electrode material of the battery obtained in Examples 1 and 2 in tetraethylene glycol dimethyl ether electrolyte are shown in FIG.
[0023] Figure 3 Mg 1.33 V 1.57 Mn0.2 Cycle life results of O4 / Mg magnesium ion battery;
[0024] Figure 4 Mg 1.33 V 1.57 Mn 0.2 The first charge and discharge curve of O4 / Mg magnesium ion battery;
[0025] Figure 5 Mg 1.33 V 1.57 Mn 0.1 XRD pattern of O4 / Mg magnesium-ion battery. DETAILED DESCRIPTION
[0026] The present invention provides a method for preparing a positive electrode material for a battery, comprising the following steps:
[0027] A magnesium source, a vanadium source, a manganese source and a dispersant are mixed and solid-phase sintered to obtain the battery positive electrode material.
[0028] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or are prepared by methods well known to those skilled in the art.
[0029] The present invention mixes a magnesium source, a vanadium source, a manganese source and a dispersant, and performs solid phase sintering to obtain the battery positive electrode material. In the present invention, the magnesium source is preferably magnesium oxide; the vanadium source is preferably at least one of vanadium trioxide and vanadium pentoxide, more preferably vanadium trioxide; the manganese source is preferably manganese dioxide. In the present invention, the dispersant is preferably stearic acid. The molar ratio of the magnesium source, vanadium source and manganese source in the present invention is preferably 1.33-1.4:1.47-1.57:0.1-0.4, specifically 1.33:1.47:0.1, 1.33:1.47:0.2, 1.33:1.57:0.1 or 1.4:1.57:0.1.
[0030] Before the solid-phase sintering, the present invention preferably mixes the magnesium source, vanadium source, manganese source and dispersant and then crushes them, and dries the obtained crushed material to obtain a dry material. The crushing of the present invention preferably includes grinding and ball milling performed in sequence. In the present invention, the grinding is preferably carried out in a mortar; the grinding agent used for the grinding is preferably anhydrous ethanol; the amount ratio of the magnesium source, vanadium source, manganese source, dispersant (stearic acid) and grinding agent is preferably 22.5-25g: 46-47g: 11-12g: 4-5g: 125-150mL, more preferably 22.5g: 46g: 11g: 4g: 125mL. The grinding time of the present invention is preferably 30-60min, more preferably 45min. In the present invention, the ball milling is preferably carried out in a ball mill; the rotation speed of the ball mill is preferably 180-300rpm, more preferably 240rpm. The ball milling time of the present invention is preferably 240-360min, more preferably 300min. The particle size of the crushed material of the present invention is preferably 50-80 mesh, more preferably 60-70 mesh. The drying of the present invention is preferably carried out in a vacuum drying oven. In the present invention, the drying temperature is preferably 68-72°C, more preferably 70°C, and the drying time is preferably 18-22h, more preferably 20h.
[0031] After obtaining the dried material, the present invention preferably performs solid-phase sintering on the dried material to obtain the battery positive electrode material. The solid-phase sintering of the present invention is preferably performed in a tubular resistance furnace. The solid-phase sintering of the present invention is preferably performed under a nitrogen atmosphere; the volume concentration of the nitrogen is preferably ≥98%. Before performing the solid-phase sintering, the present invention preferably sets the starting temperature of the tubular resistance furnace to 20°C. The temperature of the solid-phase sintering of the present invention is preferably 100-120°C, specifically 100°C, 110°C or 120°C; the insulation time is preferably 5-6h, specifically 5h, 5.5h or 6h; the heating rate to the temperature of the solid-phase sintering is preferably 20-25°C / h, specifically 20°C / h, 22°C / h or 25°C / h. After the solid-phase sintering, the present invention preferably cools the tubular resistance furnace to room temperature, takes out the obtained solid-phase sintered material; and ball mills the solid-phase sintered material to obtain the battery positive electrode material. In the present invention, the particle size of the battery positive electrode material is preferably ≤1 μm.
[0032] The present invention also provides a battery positive electrode material prepared by the preparation method described in the above technical solution. In the present invention, the chemical formula of the battery positive electrode material is preferably Mg 1.33~1.4 V 1.47~1.57 Mn 0.1~0.4 O4, more preferably Mg 1.33 V 1.57 Mn 0.1 O4 or Mg 1.33 V 1.47 Mn0.2 O4.
[0033] The present invention also provides the application of the battery positive electrode material described in the above technical solution in a magnesium ion battery.
[0034] The present invention also provides a magnesium ion battery, wherein the electrode active material of the positive electrode plate of the magnesium ion battery comprises the battery positive electrode material described in the above technical solution. The magnesium ion battery of the present invention preferably also comprises a negative electrode plate and an electrolyte. The negative electrode plate of the magnesium ion battery of the present invention is preferably a magnesium electrode; the electrolyte is preferably a Mg(ClO4)2 / PC electrolyte, a Mg(AlCl2EtBu)2 / THF electrolyte or a tetraethylene glycol dimethyl ether electrolyte.
[0035] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1
[0037] According to the molar ratio of n(Mg):n(V):n(Mn)=1.33:1.57:0.1, weigh 53.6g of MgO, 236.8g of V2O3 and 8.7g of MnO2; also take 5g of stearic acid. Pour the weighed MgO, V2O3, MnO2 and stearic acid into a mortar in turn, add 130mL of anhydrous ethanol and grind for 45min. After grinding, place the obtained material in a ball mill and mill it for 6h at a speed of 240rpm to obtain a crushed material (particle size of 50-80 mesh). Place the crushed material in a vacuum drying oven and dry it at 70℃ for 20h to obtain a dry material. The dried material was placed in a tubular resistance furnace, and in a nitrogen atmosphere with a volume fraction of 98%, the starting temperature of the tubular resistance furnace was set to 20°C, and the temperature was uniformly increased at a rate of 20°C / h for 4 hours. When the temperature of the tubular resistance furnace reached 100°C, the temperature was stopped, and then kept at 100°C for 5 hours. After 6 hours, the temperature of the tubular resistance furnace was naturally reduced to room temperature, the obtained solid material was taken out, and ball-milled to a particle size of ≤1μm to obtain the battery positive electrode material Mg 1.33 V 1.57 Mn 0.1 O4
[0038] Example 2
[0039] According to the molar ratio of n(Mg):n(V):n(Mn)=1.33:1.47:0.2, weigh 53.6g of MgO, 220.8g of V2O3 and 17.4g of MnO2; also take 5g of stearic acid. Pour the weighed MgO, V2O3, MnO2 and stearic acid into a mortar in turn, add 150mL of anhydrous ethanol and grind for 45min. After grinding, place the obtained material in a ball mill and mill it for 6h at a speed of 240rpm to obtain a crushed material (particle size of 50-80 mesh). Place the crushed material in a vacuum drying oven and dry it at 50℃ for 20h to obtain a dry material. The dried material was placed in a tubular resistance furnace, and in a nitrogen atmosphere with a volume fraction of 98%, the starting temperature of the tubular resistance furnace was set to 20°C, and the temperature was uniformly increased at a rate of 20°C / h for 5 hours. When the temperature of the tubular resistance furnace was raised to 120°C, the temperature was stopped, and then kept at 120°C for 5 hours. After 6 hours, the temperature of the tubular resistance furnace was naturally reduced to room temperature, the obtained solid material was taken out, and ball-milled to a particle size of ≤1μm to obtain the battery positive electrode material Mg 1.33 V 1.47 Mn 0.2 O4.
[0040] Test Example 1
[0041] Figure 1 This is a SEM image of the battery positive electrode material obtained in Example 1. Figure 1 It can be seen that the battery positive electrode material prepared by the present invention is in granular form with a particle size of ≤1 μm, the particles are evenly distributed as a whole, are crystal clear and have a good morphology.
[0042] Test Example 2
[0043] The battery positive electrode material Mg obtained in Example 1 1.33 V 1.57 Mn 0.1 O4 and the battery positive electrode material Mg obtained in Example 2 1.33 V 1.47 Mn 0.2 O4 was placed in tetraethylene glycol dimethyl ether electrolyte (containing metallic magnesium), and the cycle life performance test of the battery positive electrode material was carried out at 90°C.
[0044] Figure 2 The cycle life results of the battery positive electrode materials obtained in Examples 1 to 2 in tetraethylene glycol dimethyl ether (containing metal magnesium) electrolyte, wherein (a) is the battery positive electrode material Mg obtained in Example 1 1.33 V 1.57 Mn 0.1 The cycle life results of O4 in tetraethylene glycol dimethyl ether (containing magnesium metal) electrolyte, (b) is the battery positive electrode material Mg obtained in Example 2 1.33 V1.47 Mn 0.2 The cycle life results of O4 in tetraethylene glycol dimethyl ether (containing metallic magnesium) electrolyte.
[0045] The test results show that the battery positive electrode material Mg obtained in Example 1 1.33 V 1.57 Mn 0.1 The initial capacity of O4 was 256 mAh / g, and it showed a maximum discharge capacity of 73 mAh / g at the 13th cycle; the battery positive electrode material Mg obtained in Example 2 1.33 V 1.47 Mn 0.2 The initial capacity of O4 was 238 mAh / g and it showed a maximum discharge capacity of 74 mAh / g at the 14th cycle.
[0046] Depend on Figure 2 It can be seen that the battery positive electrode materials obtained in Examples 1 to 2 have good performance in magnesium ion batteries, providing a basis for further application.
[0047] Application Example 1
[0048] The battery positive electrode material Mg obtained in Example 2 1.33 V 1.47 Mn 0.2 O4 was used as the positive electrode material, Mg electrode was used as the negative electrode material, and tetraethylene glycol dimethyl ether (containing metallic magnesium) was used as the electrolyte to assemble Mg 1.33 V 1.47 Mn 0.2 O4 / Mg magnesium ion battery.
[0049] Test Example 3
[0050] The Mg prepared by the present invention 1.33 V 1.47 Mn 0.2 O4 / Mg magnesium ion battery performance test,
[0051] Figure 3 Mg 1.33 V 1.47 Mn 0.2 Cycle life results of O4 / Mg magnesium ion battery.
[0052] Figure 4 Mg 1.33 V 1.47 Mn 0.2 The first charge and discharge curve of O4 / Mg magnesium ion battery.
[0053] The results show that the first discharge capacity of the magnesium ion battery obtained by the present invention is 256 mAh / g; as the magnesium ion battery is charged and discharged multiple times, that is, Mg 2+After multiple extraction and embedding reactions, the capacity of the magnesium-ion battery undergoes a significant attenuation change. At the 9th cycle, the specific capacity of the magnesium-ion battery decreases by about 20 mAh / g.
[0054] It can be seen that within a certain temperature and time range, the properties of the obtained battery positive electrode material are not affected, and the obtained battery positive electrode material is in good condition and has a high capacity.
[0055] In addition, the present invention also performs the battery positive electrode material Mg obtained in Example 1 1.33 V 1.57 Mn 0.1 O4 was subjected to XRD analysis, and the results were as follows Figure 5 shown.
[0056] Depend on Figure 5 It can be seen that the Mn element has the smallest lattice distortion at the 16d position (d orbital of electrons), making Mg 1.33 V 1.57 Mn 0.1 The crystal structure of O4 is the most stable, which is conducive to improving the capacitance.
[0057] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a positive electrode material for a battery, characterized in that: The following steps are involved: A magnesium source, a vanadium source, a manganese source and a dispersant are mixed and solid-phase sintered to obtain the battery positive electrode material.
2. The preparation method according to claim 1, characterized in that: The magnesium source is magnesium oxide; the vanadium source is at least one of vanadium trioxide and vanadium pentoxide; and the manganese source is manganese dioxide.
3. The preparation method according to claim 1 or 2, characterized in that: The molar ratio of the magnesium source, the vanadium source and the manganese source is 1.33-1.4:1.47-1.57:0.1-0.
4.
4. The preparation method according to claim 1, characterized in that: The dispersant is stearic acid.
5. The preparation method according to claim 1, characterized in that: The temperature of the solid phase sintering is 100-120°C, the holding time is 5-6h, and the heating rate to the solid phase sintering temperature is 20-25°C / h; the solid phase sintering is carried out in a nitrogen atmosphere; the volume concentration of the nitrogen is ≥98%.
6. A battery positive electrode material prepared by the preparation method according to any one of claims 1 to 5.
7. The battery positive electrode material according to claim 6, characterized in that: The chemical formula is Mg 1.33~1.4 V 1.47~ 1.57 Mn 0.1~0.4 O4.
8. The battery positive electrode material according to claim 7, characterized in that: The chemical formula is Mg 1.33 V 1.57 Mn 0.1 O4 or Mg 1.33 V 1.47 Mn 0.2 O4.
9. Use of the battery positive electrode material according to any one of claims 6 to 8 in a magnesium ion battery.
10. A magnesium ion battery, characterized in that: The electrode active material of the positive electrode sheet comprises the battery positive electrode material according to any one of claims 6 to 8.
Citation Information
Cited By
Magnesium vanadium oxide positive electrode material with spinel structure and preparation method of magnesium vanadium oxide positive electrode material
CN120664587A