Precursor with porous isolation layer, positive electrode material, preparation and application
By designing a precursor with a porous isolation layer in the positive electrode material of sodium ion battery, blocking the propagation of microcracks and releasing stress, the problem of structural instability of the positive electrode material of sodium ion battery during the circulation process is solved, and the circulation performance of the battery is significantly improved .
Patent Information
- Application Number
- CN202411239143.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
AI Technical Summary
The positive electrode material of sodium ion battery is prone to microcracks during charging and discharging, resulting in a decline in electrochemical performance. The existing precursor is unstable during the circulation process and cannot effectively alleviate the volume expansion/shrinkage stress.
A precursor with a porous isolation layer was designed, including the core, the porous isolation layer and the shell. The porous isolation layer has a higher porosity than the core and the shell, blocking the propagation of microcracks, providing more space to release stress, and through co-precipitation reaction Prepare a high density core and shell to form a low density porous isolation layer.
The structural stability and shape maintenance of the positive electrode material during the circulation process is significantly improved, the circulation performance of the battery is improved, and the electrochemical performance decline caused by microcracks is avoided.
Smart Images

Figure CN118993175A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of batteries, and relates to a precursor with a porous isolation layer, and particularly to a precursor with a porous isolation layer, a cathode material, and their preparation and applications. Background Art
[0002] With the rapid growth of the demand for lithium-ion batteries in the fields of consumer electronics, power batteries, and energy storage, the price of lithium resources has been running at a high level and fluctuating for a long time, and the supply has become increasingly tense, which deeply affects the normal development of the industry. The limited reserves and uneven distribution of lithium resources make it difficult for lithium-ion batteries to meet the rapidly growing application demands. Compared with lithium resources, sodium resources are rich in the earth's crust and oceans, widely distributed, and low in cost. Sodium-ion batteries show broad application potential in small power and large-scale electrical energy storage. In addition, although the energy density is relatively low, sodium-ion batteries have certain advantages in many aspects such as cost, safety, rate performance, and low-temperature performance. Under this background, as an alternative route to lithium-ion batteries, the development of sodium-ion batteries has very important economic value and strategic significance.
[0003] Sodium-ion battery transition metal layered oxide cathode materials have excellent comprehensive properties and prominent commercialization prospects. At present, the generation of microcracks during the charge-discharge process is a major technical challenge for the industrialization of sodium-layered oxide cathode materials. During the charge-discharge cycle, due to the insertion and extraction of Na with a relatively large radius, the shrinkage in the c-axis direction leads to an uneven stress distribution within the secondary particles. When the stress accumulation exceeds the yield limit of the particles, cracks are generated between the grain boundaries. As the cycle progresses, the cracks gradually extend from the inside of the secondary particles to the surface, and even cause the particles to pulverize. The formation of microcracks allows the electrolyte to enter the interior of the particles, and then new solid-liquid side reaction interfaces are generated inside the particles. This not only consumes the electrolyte and active materials, but also forms regions that isolate electrons and ions inside the particles, further increasing the impedance and deteriorating the electrochemical performance of the material. y , + During the charge-discharge cycle, due to the insertion and extraction of Na with a relatively large radius, the shrinkage in the c-axis direction leads to an uneven stress distribution within the secondary particles. When the stress accumulation exceeds the yield limit of the particles, cracks are generated between the grain boundaries. As the cycle progresses, the cracks gradually extend from the inside of the secondary particles to the surface, and even cause the particles to pulverize. The formation of microcracks allows the electrolyte to enter the interior of the particles, and then new solid-liquid side reaction interfaces are generated inside the particles. This not only consumes the electrolyte and active materials, but also forms regions that isolate electrons and ions inside the particles, further increasing the impedance and deteriorating the electrochemical performance of the material.
[0004] CN112928250A discloses a nickel-cobalt-manganese ternary material, its precursor, and preparation method and applications. The composition of the nickel-cobalt-manganese ternary material precursor is represented by Ni x Co<00,00003>[ Mn (1-x-y) (OH)2, where 0.30 < x < 0.85, 0.05 < y < 0.35, 0 < x + y < 1; the nickel-cobalt-manganese ternary material precursor includes an inner core, a dense layer, a dense layer connecting layer, and an outer shell from inside to outside in sequence. Both the inner core and the dense layer connecting layer have a loose structure, and both the dense layer and the outer shell have a dense structure.
[0005] CN111732132A discloses a nickel-cobalt-manganese core-shell structured precursor and its preparation method. The precursor has a dense, porous core and a loose outer shell with primary particles arranged radially on the core. This precursor structure facilitates the diffusion of Li ions and the penetration of electrolyte during lithium-ion mixing and sintering. During charge and discharge, it provides a rapid migration channel for Li ions, balancing the requirements of tap density and porous structure.
[0006] Existing cathode material precursors all have certain defects. Batteries containing cathode materials prepared from these precursors are prone to microcracks during charge and discharge. These microcracks lead to cathode material pulverization, an increase in solid-liquid side reaction interfaces, and the formation of regions that isolate electrons and ions, thereby degrading the battery's electrochemical performance. Therefore, developing and designing novel precursors, cathode materials, and their preparation methods is crucial. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the present invention aims to provide a precursor with a porous isolation layer, a cathode material, and their preparation and application. The precursor with a porous isolation layer provided by the present invention has a porous isolation layer, which blocks the propagation of microcracks and provides more space to release the stress accumulated during volume expansion / contraction during deep charge and discharge. This ensures that the cathode material prepared from the precursor has a stable structure and shape during cycling, and improves the cycle performance of batteries containing cathode materials prepared from the precursor.
[0008] To achieve this objective, the present invention adopts the following technical solution:
[0009] In a first aspect, the present invention provides a precursor having a porous isolation layer, the precursor comprising a core, a porous isolation layer covering the core, and a shell covering the porous isolation layer, wherein the porosity of the porous isolation layer is higher than that of the core and the shell.
[0010] The precursor with a porous isolation layer provided by the present invention has a porous isolation layer, which blocks the propagation of microcracks and provides more space to release the stress accumulated by volume expansion / contraction during deep charge and discharge. This ensures that the cathode material prepared by the precursor has a stable structure and shape during cycling, and improves the cycle performance of the battery containing the cathode material prepared by the precursor.
[0011] Preferably, the porosity of the core is 2 to 4%, for example, it can be 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.2%, 3.4%, 3.6%, 3.8% or 4%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0012] Preferably, the porosity of the outer shell is 2% to 4%, for example, it can be 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.2%, 3.4%, 3.6%, 3.8%, or 4%, but it is not limited to the listed values; other unlisted values within this range are also applicable.
[0013] Preferably, the porosity of the porous isolation layer is 5 to 10%, for example, it can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5% or 10%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0014] Preferably, the thickness of the porous isolation layer is 1 to 3 μm, for example, it can be 1 μm, 1.5 μm, 1.8 μm, 2 μm, 2.2 μm, 2.5 μm, 2.8 μm or 3 μm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0015] Preferably, the core is composed of NiFeMn(OH)2 with a layered structure;
[0016] Preferably, the outer shell is composed of NiFeMn(OH)2 having a layered structure;
[0017] Preferably, the components in the porous isolation layer include NiFeMn(OH)2 with a layered structure, and also include any one or a combination of at least two of Zn(OH)2 with an amorphous structure, Cu(OH)2 with an orthorhombic crystal system (Cmc21), or Ti(OH)4 with an amorphous structure.
[0018] In a second aspect, the present invention provides a method for preparing the precursor described in the first aspect, the method comprising:
[0019] (1) Add the first mixed salt solution, precipitant solution and complexing agent solution to the reaction substrate in parallel flow to carry out a co-precipitation reaction and obtain a mixed solution containing the first precipitate;
[0020] (2) Add the second mixed salt solution, precipitant solution and complexing agent solution in parallel to the mixture containing the first precipitate obtained in step (1) to carry out a coprecipitation reaction and obtain a mixture containing the second precipitate.
[0021] The second mixed salt solution includes doped metal ions, and also includes all the metal ions in the first mixed salt solution;
[0022] (3) Add the first mixed salt solution, precipitant solution and complexing agent solution in parallel to the mixture containing the second precipitate obtained in step (2) to carry out a coprecipitation reaction to obtain the precursor.
[0023] In the preparation method provided by the present invention, a core with high density and good crystallinity is obtained in step (1); in step (2), the second mixed salt solution also includes doped metal ions. During the crystal growth process of precipitation, the doped metal ions will generate more dislocations and crystal surface defects, resulting in a porous isolation layer with high porosity; in step (3), a shell with high density and good crystallinity is obtained. The preparation method prepares a precursor with high density of core and shell and low density of porous isolation layer between core and shell, which alleviates the generation of microcracks caused by sodium ion insertion and extraction during charging and discharging, and significantly improves the cycle performance of the cathode material prepared by the precursor.
[0024] The preparation method provided by this invention has a simple preparation process and strong universality. During the production process, only the feed pipe of the mixed salt solution needs to be replaced. The operation is simple and avoids additional steps, thereby avoiding the addition of additional dopants. It has the prospect of high-efficiency and large-scale production.
[0025] Preferably, the doped metal ions in step (2) satisfy the first condition and / or the second condition;
[0026] The first condition is that the difference between the precipitation constant of the doped metal ion and the precipitation constant of all metal ions in the first mixed salt solution is not less than 10. 3 ;
[0027] The second condition is that the crystal structure of the substance formed after the doped metal ions are precipitated is different from the crystal structure of the substance formed after all metal ions are precipitated in the first mixed salt solution.
[0028] The difference between the precipitation constant of the doped metal ion described in the first condition of this invention and the precipitation constant of all metal ions in the first mixed salt solution is not less than 1 × 10⁻⁶. 3 That is, the difference between the precipitation constants of the doped metal ions and Ni, Fe, and Mn ions is not less than 1 × 10⁻⁶. 3 For example, it could be 1×10 3 1.1×10 3 1.2×10 3 1.3×10 3 1.4×10 3 1.5×10 3 1.6×10 3 1.7×10 3 1.8×10 3 1.9×10 3 2×10 3 2.5×10 3 Or 3×10 3However, this does not apply to all values listed; other unlisted values within the same range also apply.
[0029] The crystal structure of the substance formed after precipitation of doped metal ions in the second condition of this invention is different from the crystal structure of the substance formed after precipitation of all metal ions in the first mixed salt solution. That is, the crystal structure of the substance formed after precipitation of doped metal ions is different from the crystal structure of the substance formed by individual precipitation and co-precipitation of Ni ions, Fe ions and Mn ions.
[0030] If the precipitation constants of the doped metal ions and the metal ions in the first mixed salt solution are similar, and the crystal structure of the precipitate after precipitation is consistent, the crystal growth process is relatively complete, and a structure with high density and good crystallinity will be obtained after co-precipitation. If the precipitation constants of the doped metal ions and the metal ions in the first mixed salt solution are somewhat different, or the crystal structure of the precipitate after precipitation is inconsistent, more dislocations and crystal plane defects will be generated during the crystal growth process, resulting in a structure with high porosity.
[0031] In step (2) of the preparation method of the present invention, the doped metal ions in the second mixed salt solution satisfy the first condition and / or the second condition. In step (2), the precipitate will generate more dislocations and crystal surface defects during the crystal growth process, thereby forming a porous isolation layer with high porosity outside the core.
[0032] Preferably, in step (2), the addition rates of the second mixed salt solution, precipitant solution, and complexing agent solution are all higher than the addition rates of the first mixed salt solution, precipitant solution, and complexing agent solution in steps (1) and (3).
[0033] In step (2) of the preparation method provided by the present invention, the flow rates of the metal salt solution, precipitant and complexing agent are increased during the preparation of the porous isolation layer, thereby increasing the growth rate of the precipitate crystals, disrupting the ordered lattice structure arrangement, and promoting the generation of the porous isolation layer.
[0034] Preferably, the addition rate of the second mixed salt solution in step (2) is 40 to 80 L / h, for example, it can be 40 L / h, 45 h, 50 h, 55 h, 60 h, 65 h, 70 h, 75 h or 80 h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0035] Preferably, the addition rate of the precipitant solution in step (2) is 15 to 25 L / h, for example, it can be 15 L / h, 16 L / h, 17 L / h, 18 L / h, 19 L / h, 20 L / h, 21 L / h, 22 L / h, 23 L / h, 24 L / h or 25 L / h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0036] Preferably, the addition rate of the complexing agent solution in step (2) is 2 to 4 L / h, for example, it can be 2 L / h, 2.2 L / h, 2.4 L / h, 2.6 L / h, 2.8 L / h, 3 L / h, 3.2 L / h, 3.4 L / h, 3.6 L / h, 3.8 L / h or 4 L / h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0037] Preferably, the addition rate of the first mixed salt solution in steps (1) and (3) is 10 to 40 L / h, for example, it can be 10 L / h, 12 L / h, 15 L / h, 17 L / h, 20 L / h, 22 L / h, 25 L / h, 27 L / h, 30 L / h, 32 L / h, 35 L / h, 37 L / h or 40 L / h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0038] Preferably, the addition rate of the precipitant solution in steps (1) and (3) is 5 to 15 L / h, for example, it can be 5 L / h, 6 L / h, 7 L / h, 8 L / h, 9 L / h, 10 L / h, 11 L / h, 12 L / h, 13 L / h, 14 L / h or 15 L / h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0039] Preferably, the addition rate of the complexing agent solution in steps (1) and (3) is 0.5 to 1.5 L / h, for example, it can be 0.5 L / h, 0.6 L / h, 0.7 L / h, 0.8 L / h, 0.9 L / h, 1 L / h, 1.1 L / h, 1.2 L / h, 1.3 L / h, 1.4 L / h or 1.5 L / h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0040] Preferably, the temperature during the coprecipitation reaction in steps (1) to (3) is 50 to 70°C, the stirring speed is 200 to 400 rpm, and the pH is 9 to 11.
[0041] The temperature for the coprecipitation reaction in steps (1) to (3) of this invention is 50 to 70°C, for example, it can be 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C or 70°C, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0042] The stirring speed during the coprecipitation reaction in steps (1) to (3) of this invention is 200 to 400 rpm, for example, it can be 200 rpm, 220 rpm, 240 rpm, 260 rpm, 280 rpm, 300 rpm, 320 rpm, 340 rpm, 360 rpm, 380 rpm or 400 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0043] The pH during the coprecipitation reaction in steps (1) to (3) of this invention is 9 to 11, for example, it can be 9, 9.2, 9.4, 9.6, 9.8, 10, 10.2, 10.4, 10.6, 10.8 or 11, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0044] Preferably, the first mixed salt solution in steps (1) and (3) is a nickel-iron-manganese mixed salt solution; the doped metal ions in step (2) include any one or at least two of Zn ions, Cu ions or Ti ions, and typical but non-limiting combinations include the combination of Zn ions and Cu ions, the combination of Cu ions and Ti ions, or the combination of Zn ions, Cu ions and Ti ions.
[0045] Preferably, the total concentration of metal ions in the first mixed salt solution in steps (1) to (3) is 0.5 to 2.0 mol / L, for example, it can be 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L or 2 mol / L, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0046] Preferably, the molar amount of all metal ions in the second mixed salt solution in step (2) is taken as 100%, and the molar amount of the doped metal ions is not higher than 5%, for example, it can be 1%, 2%, 3%, 4%, or 5%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0047] Preferably, in steps (1) and (3), the nickel salt, iron salt, and manganese salt in the first mixed salt solution independently include any one or at least two combinations of sulfate, nitrate, or chloride. Typical but non-limiting combinations include combinations of sulfate and nitrate, nitrate and chloride, or combinations of sulfate, nitrate, and chloride. In step (2), the doped metal ion salt in the second mixed salt solution includes any one or at least two combinations of sulfate, nitrate, or chloride. Typical but non-limiting combinations include combinations of sulfate and nitrate, nitrate and chloride, or combinations of sulfate, nitrate, and chloride.
[0048] Preferably, the precipitant solution in steps (1) to (3) includes NaOH solution and / or KOH solution.
[0049] Preferably, the concentration of the precipitant solution in steps (1) to (3) is 6 to 10 mol / L, for example, it can be 6 mol / L, 6.5 mol / L, 7 mol / L, 7.5 mol / L, 8 mol / L, 8.5 mol / L, 9 mol / L, 9.5 mol / L or 10 mol / L, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0050] Preferably, the complexing agent solution in steps (1) to (3) includes ammonia water and / or sodium citrate solution.
[0051] Preferably, the concentration of the complexing agent solution in steps (1) to (3) is 0.2 to 1 mol / L, for example, it can be 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1 mol / L, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0052] Preferably, steps (1) to (3) are all carried out in a protective atmosphere.
[0053] Preferably, the D50 particle size of the first precipitate obtained in step (1) is 4 to 6 μm, for example, it can be 4 μm, 4.2 μm, 4.4 μm, 4.6 μm, 4.8 μm, 5 μm, 5.2 μm, 5.4 μm, 5.6 μm, 5.8 μm or 6 μm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0054] Preferably, the D50 particle size of the second precipitate obtained in step (2) is 6 to 8 μm, for example, it can be 6 μm, 6.2 μm, 6.4 μm, 6.6 μm, 6.8 μm, 7 μm, 7.2 μm, 7.4 μm, 7.6 μm, 7.8 μm or 8 μm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0055] In this invention, the difference between the D50 particle size of the second precipitate and the D50 particle size of the first precipitate is the thickness of the porous isolation layer.
[0056] Preferably, the D50 particle size of the precursor obtained in step (3) is 8 to 10 μm, for example, it can be 8 μm, 8.2 μm, 8.4 μm, 8.6 μm, 8.8 μm, 9 μm, 9.2 μm, 9.4 μm, 9.6 μm, 9.8 μm or 10 μm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0057] Preferably, the coprecipitation reaction described in step (3) is followed by centrifugation, washing, drying and demagnetization in sequence.
[0058] Thirdly, the present invention provides a cathode material, which is prepared from the precursor described in the first aspect.
[0059] Fourthly, a process for preparing the cathode material described in the third aspect, the process comprising:
[0060] The precursor and sodium source are mixed and sintered to obtain the cathode material.
[0061] Preferably, the sodium source includes Na2CO3 and / or NaOH.
[0062] Preferably, the sintering temperature is 800–900°C and the time is 10–20 h.
[0063] The sintering temperature described in this invention is 800-900℃, for example, it can be 800℃, 810℃, 820℃, 830℃, 840℃, 850℃, 860℃, 870℃, 880℃, 890℃ or 900℃, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0064] The sintering time described in this invention is 10 to 20 hours, for example, it can be 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours or 20 hours, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0065] Compared with the prior art, the present invention has the following beneficial effects:
[0066] (1) The precursor with a porous isolation layer provided by the present invention has a porous isolation layer, which blocks the propagation of microcracks, provides more space to release the stress accumulated by volume expansion / contraction during deep charge and discharge, ensures that the positive electrode material prepared by the precursor has a stable structure and shape during cycling, and improves the cycle performance of the battery containing the positive electrode material prepared by the precursor.
[0067] (2) The preparation method provided by the present invention has prepared a precursor with high density of core and shell and low density of porous isolation layer between core and shell, which alleviates the generation of microcracks caused by sodium ion insertion and extraction during charging and discharging, and significantly improves the cycle performance of the cathode material prepared by the precursor.
[0068] (3) The preparation method provided by the present invention has a simple preparation process and strong universality. During the production process, only the feed pipe of the mixed salt solution needs to be replaced. The operation is simple and avoids additional processes, thereby avoiding the addition of additional dopants. It has the prospect of high-efficiency and large-scale production. Attached Figure Description
[0069] Figure 1 This is a schematic diagram of the structure of the precursor with a porous isolation layer provided in Embodiment 1 of the present invention.
[0070] Figure 2 This is an EPMA diagram of the precursor with a porous isolation layer described in Embodiment 1 of the present invention.
[0071] Among them, 1-core; 2-porous isolation layer; 3-shell. Detailed Implementation
[0072] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0073] Example 1
[0074] This embodiment provides a method such as Figure 1 and Figure 2 The precursor shown has a porous isolation layer 2, the precursor comprising a core 1 with a porosity of 3%, a porous isolation layer 2 with a porosity of 8% covering the core 1, and a shell 3 with a porosity of 3% covering the porous isolation layer 2. The porosity of the porous isolation layer 2 is higher than that of the core 1 and the shell 3.
[0075] The core 1 is composed of NiFeMn(OH)2 with a layered structure;
[0076] The outer shell 3 is composed of NiFeMn(OH)2 with a layered structure;
[0077] The components in the porous isolation layer 2 include NiFeMn(OH)2 with a layered structure and Zn(OH)2 with an amorphous structure.
[0078] The method for preparing the precursor is as follows:
[0079] (1) In a nitrogen atmosphere, a nickel-iron-manganese mixed salt solution with a total metal ion concentration of 1 mol / L (the molar ratio of nickel ions, iron ions and manganese ions is 1:1:1), sodium hydroxide solution and ammonia water are added to the reaction base liquid in parallel flow. The addition rate of the nickel-iron-manganese mixed salt solution is 25 L / h. The co-precipitation reaction is carried out at 60℃, stirring speed of 300 rpm and pH of 10 to obtain a mixed solution containing a first precipitate with a D50 particle size of 6 μm.
[0080] (2) In a nitrogen atmosphere, a second mixed salt solution with a total metal ion concentration of 1 mol / L, a sodium hydroxide solution and ammonia water are added in parallel to the mixed solution containing the first precipitate obtained in step (1). The addition rate of the second mixed salt solution is 60 L / h. The co-precipitation reaction is carried out at 60 °C, a stirring speed of 300 rpm and a pH of 10 to obtain a mixed solution containing a second precipitate with a D50 particle size of 7 μm.
[0081] The second mixed salt solution includes zinc ions, as well as nickel ions, iron ions, and manganese ions; based on the molar amount of all metal ions in the second mixed salt solution as a percentage, the molar amount of zinc ions accounts for 4%, and the molar ratio of nickel ions, iron ions, and manganese ions in the second mixed salt solution is 1:1:1; the amorphous structure of Zn(OH)2 formed after the zinc ions are precipitated is different from the crystal structure of the substance formed after the precipitation of all metal ions in the first mixed salt solution;
[0082] (3) In a nitrogen atmosphere, a nickel-iron-manganese mixed salt solution with a total metal ion concentration of 1 mol / L (the molar ratio of nickel ions, iron ions and manganese ions is 1:1:1), sodium hydroxide solution and ammonia water are added in parallel to the mixed solution containing the second precipitate obtained in step (2). The nickel-iron-manganese mixed salt solution is added at a rate of 25 L / h. The co-precipitation reaction is carried out at 60°C, a stirring speed of 300 rpm and a pH of 10 to obtain the precursor with a D50 particle size of 9 μm.
[0083] Example 2
[0084] This embodiment provides a precursor having a porous isolation layer 2. The precursor includes a core 1 with a porosity of 2%, a porous isolation layer 2 with a porosity of 5% covering the core 1, and a shell 3 with a porosity of 2% covering the porous isolation layer 2. The porosity of the porous isolation layer 2 is higher than that of the core 1 and the shell 3.
[0085] The core 1 is composed of NiFeMn(OH)2 with a layered structure;
[0086] The outer shell 3 is composed of NiFeMn(OH)2 with a layered structure;
[0087] The porous isolation layer 2 comprises NiFeMn(OH)2 with a layered structure, and Cu(OH)2 with an orthorhombic crystal system (Cmc21).
[0088] The method for preparing the precursor is as follows:
[0089] (1) In an argon atmosphere, a nickel-iron-manganese mixed salt solution with a total metal ion concentration of 0.5 mol / L (the molar ratio of nickel ions, iron ions and manganese ions is 1:1:1), potassium hydroxide solution and sodium citrate solution are added to the reaction substrate in parallel flow. The nickel-iron-manganese mixed salt solution is added at a rate of 10 L / h. The co-precipitation reaction is carried out at 70 °C, a stirring speed of 400 rpm and a pH of 11 to obtain a mixed solution containing a first precipitate with a D50 particle size of 5 μm.
[0090] (2) In an argon atmosphere, a second mixed salt solution with a total metal ion concentration of 0.5 mol / L, a potassium hydroxide solution, and a sodium citrate solution are added in parallel to the mixture containing the first precipitate obtained in step (1). The addition rate of the second mixed salt solution is 40 L / h. The co-precipitation reaction is carried out at 70 °C, a stirring speed of 400 rpm, and a pH of 11 to obtain a mixture containing a second precipitate with a D50 particle size of 6 μm.
[0091] The second mixed salt solution includes copper ions, as well as nickel ions, iron ions, and manganese ions; based on the molar amount of all metal ions in the second mixed salt solution as a percentage, the molar amount of copper ions accounts for 2%, and the molar ratio of nickel ions, iron ions, and manganese ions in the second mixed salt solution is 1:1:1; the copper ions precipitate to form Cu(OH)2 with an orthorhombic crystal system (Cmc21), which has a different crystal structure from the substance formed after the precipitation of all metal ions in the first mixed salt solution;
[0092] (3) In an argon atmosphere, a nickel-iron-manganese mixed salt solution with a total metal ion concentration of 0.5 mol / L (molar ratio of nickel ions, iron ions and manganese ions is 1:1:1), a potassium hydroxide solution and a sodium citrate solution are added in parallel to the mixed solution containing the second precipitate obtained in step (2). The nickel-iron-manganese mixed salt solution is added at a rate of 10 L / h. The co-precipitation reaction is carried out at 70 °C, a stirring speed of 400 rpm and a pH of 11 to obtain the precursor with a D50 particle size of 8 μm.
[0093] Example 3
[0094] This embodiment provides a precursor having a porous isolation layer 2. The precursor includes a core 1 with a porosity of 4%, a porous isolation layer 2 with a porosity of 10% covering the core 1, and a shell 3 with a porosity of 4% covering the porous isolation layer 2. The porosity of the porous isolation layer 2 is higher than that of the core 1 and the shell 3.
[0095] The core 1 is composed of NiFeMn(OH)2 with a layered structure;
[0096] The outer shell 3 is composed of NiFeMn(OH)2 with a layered structure;
[0097] The components in the porous isolation layer 2 include NiFeMn(OH)2 with a layered structure and Ti(OH)4 with an amorphous structure.
[0098] The method for preparing the precursor is as follows:
[0099] (1) In an argon atmosphere, a nickel-iron-manganese mixed salt solution with a total metal ion concentration of 2.0 mol / L (the molar ratio of nickel ions, iron ions and manganese ions is 1:1:1), sodium hydroxide solution and ammonia water were added to the reaction base liquid in parallel flow. The nickel-iron-manganese mixed salt solution was added at a rate of 40 L / h. The co-precipitation reaction was carried out at 50 °C, a stirring speed of 200 rpm and a pH of 9 to obtain a mixed solution containing a first precipitate with a D50 particle size of 6 μm.
[0100] (2) In an argon atmosphere, a second mixed salt solution with a total metal ion concentration of 2.0 mol / L, a sodium hydroxide solution and ammonia water are added in parallel to the mixed solution containing the first precipitate obtained in step (1). The addition rate of the second mixed salt solution is 80 L / h. The co-precipitation reaction is carried out at 50 °C, a stirring speed of 200 rpm and a pH of 9 to obtain a mixed solution containing a second precipitate with a D50 particle size of 7 μm.
[0101] The second mixed salt solution includes titanium ions, as well as nickel ions, iron ions, and manganese ions; based on the molar amount of all metal ions in the second mixed salt solution as 100%, the molar amount of the doped metal ions is 5%, and the molar ratio of nickel ions, iron ions, and manganese ions in the second mixed salt solution is 1:1:1; the titanium ions precipitate to form Ti(OH)4 with an amorphous structure, which has a different crystal structure from the substance formed after the precipitation of all metal ions in the first mixed salt solution;
[0102] (3) In an argon atmosphere, a nickel-iron-manganese mixed salt solution with a total metal ion concentration of 2.0 mol / L (molar ratio of nickel ions, iron ions and manganese ions is 1:1:1), sodium hydroxide solution and ammonia water are added in parallel to the mixed solution containing the second precipitate obtained in step (2). The nickel-iron-manganese mixed salt solution is added at a rate of 40 L / h. The co-precipitation reaction is carried out at 50 °C, a stirring speed of 200 rpm and a pH of 9 to obtain the precursor with a D50 particle size of 10 μm.
[0103] Example 4
[0104] This embodiment provides a precursor with a porous isolation layer 2. Except that the porosity of the porous isolation layer 2 is 4%, that is, the addition rate of the second mixed salt solution in step (2) of the preparation method of the precursor is 25 L / h, the rest are the same as in Example 1.
[0105] Example 5
[0106] This embodiment provides a precursor with a porous isolation layer 2. Except that the porosity of the porous isolation layer 2 is 15%, that is, the addition rate of the second mixed salt solution in step (2) of the preparation method of the precursor is 100 L / h, the rest is the same as in Example 1.
[0107] Example 6
[0108] This embodiment provides a precursor with a porous isolation layer 2, which is the same as that in Embodiment 1 except that the thickness of the porous isolation layer 2 is 0.5 μm.
[0109] Example 7
[0110] This embodiment provides a precursor with a porous isolation layer 2, which is the same as that in Embodiment 1 except that the thickness of the porous isolation layer 2 is 4 μm.
[0111] Comparative Example 1
[0112] This comparative example provides a precursor with a porosity of 3% from the inside out. It does not construct a special porous isolation layer 2. Except for replacing the second mixed salt solution in step (2) with the nickel-iron-manganese mixed salt solution in step (1), everything else is the same as in Example 1.
[0113] The precursors provided in the above embodiments and comparative examples were mixed with Na2CO3 and sintered at 850°C for 15 hours to obtain the positive electrode material. The prepared positive electrode material, conductive carbon black, and PVDF binder were weighed according to a mass ratio of 7.5:1.5:1, and the materials were uniformly dispersed in N-methylpyrrolidone (NMP) to prepare a conductive slurry. This slurry was then coated onto aluminum foil, dried at 70°C, cut, and weighed. The battery type was a button cell, model CR2032. The separator was made of glass fiber, the negative electrode was a sodium metal sheet, and the electrolyte was 1M NaPF6 EC / DMC = 1:1. Half-cells were assembled in a glove box filled with Ar gas in the following order: sodium metal sheet, separator, positive electrode sheet, gasket, and spring sheet. The specific capacity of the fabricated CR2032 button cell was tested within a voltage window between 2.0 and 4.1V. The first cycle was performed at 0.1C / 0.1C charge / discharge, followed by 50 cycles at 0.5C / 1C. Cycle stability was expressed as the percentage of the discharge capacity on the 50th cycle divided by the discharge capacity on the first cycle. The test results are shown in Table 1.
[0114] Table 1
[0115]
[0116]
[0117] From Table 1, we can obtain:
[0118] (1) The positive electrode material prepared by the precursor prepared in Examples 1 to 3 of the present invention, and the sodium-ion battery prepared by the positive electrode material, both showed high capacity retention after 300 cycles at 1C and 5C. The battery containing the positive electrode material prepared by the precursor has excellent cycle performance.
[0119] (2) By comparing Example 1 with Examples 4 and 5, it can be seen that the porosity of the core 1 in this invention affects the performance of the precursor and the sodium-ion battery. When the porosity of the porous separator 2 is too low, the capacity retention rate after 50 cycles will be lower. This is because the porosity of the porous separator 2 is similar to that of the core 1 and the shell 3, which cannot effectively block the propagation of microcracks, nor can it provide more space to release the stress accumulated during the volume expansion / contraction process, thus making it difficult to improve the cycle performance of the battery containing the positive electrode material prepared by the precursor. When the porosity of the porous separator 2 is too high, the capacity retention rate will also be reduced. This is because the higher porosity leads to more contact between the active surface of the positive electrode material and the electrolyte, increasing the side reactions and reducing the cycle performance.
[0120] (3) By comparing Example 1 with Examples 6 and 7, it can be seen that the thickness of the porous separator 2 in this invention affects the performance of the precursor and the sodium-ion battery. When the thickness of the porous separator 2 is too small, the capacity retention rate after 50 cycles will be lower. This is because the porous separator 2 with too small a thickness cannot effectively block the propagation of microcracks, nor can it provide more space to release the stress accumulated during the volume expansion / contraction process, thus making it difficult to improve the cycle performance of the battery containing the positive electrode material prepared from the precursor. When the thickness of the porous separator 2 is too large, the capacity retention rate will also be reduced. This is because the porous separator 2 is too thick, resulting in more contact between the active surface of the positive electrode material and the electrolyte, increasing the side reactions and reducing the cycle performance.
[0121] (4) By comparing Example 1 with Comparative Example 1, it can be seen that the precursor with porous isolation layer 2 provided by the present invention has porous isolation layer 2. The porosity of porous isolation layer 2 is higher than that of core 1 and shell 3. Porous isolation layer 2 effectively blocks the propagation of microcracks, provides more space to release the stress accumulated during volume expansion / contraction, ensures that the positive electrode material prepared by the precursor has a stable structure and shape during cycling, and improves the cycle performance of the battery containing the positive electrode material prepared by the precursor.
[0122] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A precursor having a porous isolation layer, characterized in that: The precursor comprises a core, a porous isolation layer covering the core, and an outer shell covering the porous isolation layer. The porosity of the porous isolation layer is higher than the porosity of the core and the outer shell.
2. The precursor according to claim 1, characterized in that The porosity of the inner core is 2-4%; Preferably, the porosity of the shell is 2-4%; Preferably, the porosity of the porous isolation layer is 5-10%; Preferably, the porous isolation layer has a thickness of 1 to 3 μm.
3. The precursor according to claim 1 or 2, characterized in that The core is composed of NiFeMn(OH)2 having a layered structure; Preferably, the shell is composed of NiFeMn(OH)2 having a layered structure; Preferably, the components in the porous isolation layer include NiFeMn(OH)2 with a layered structure, and also include any one or a combination of at least two of Zn(OH)2 with an amorphous structure, Cu(OH)2 of the orthorhombic system (Cmc21) or Ti(OH)4 with an amorphous structure.
4. A method for preparing the precursor according to any one of claims 1 to 3, characterized in that: The preparation method comprises: (1) adding a first mixed salt solution, a precipitant solution and a complexing agent solution to a reaction base liquid in parallel to perform a coprecipitation reaction to obtain a mixed solution containing a first precipitate; (2) adding a second mixed salt solution, a precipitant solution and a complexing agent solution to the mixed solution containing the first precipitate obtained in step (1) in parallel to carry out a coprecipitation reaction to obtain a mixed solution containing a second precipitate; The second mixed salt solution includes doped metal ions and also includes all metal ions in the first mixed salt solution; (3) Adding the first mixed salt solution, the precipitant solution and the complexing agent solution in parallel to the mixed solution containing the second precipitate obtained in step (2) to carry out a co-precipitation reaction to obtain the precursor.
5. The preparation method according to claim 4, characterized in that: The doping metal ions in step (2) satisfy the first condition and / or the second condition; The first condition is that the difference between the precipitation constant of the doped metal ion and the precipitation constant of all metal ions in the first mixed salt solution is not less than 1×10 3 ; The second condition is that the crystal structure of the substance formed after the precipitation of the doped metal ions is different from the crystal structure of the substance formed after the precipitation of all metal ions in the first mixed salt solution.
6. The preparation method according to claim 4 or 5, characterized in that: The addition rate of the second mixed salt solution, precipitant solution and complexing agent solution in step (2) is higher than the addition rate of the first mixed salt solution, precipitant solution and complexing agent solution in step (1) and step (3); Preferably, in step (2), the addition rate of the second mixed salt solution is 40 to 80 L / h; Preferably, in step (1) and step (3), the addition rate of the first mixed salt solution is 10 to 40 L / h; Preferably, the temperature during the coprecipitation reaction in steps (1) to (3) is 50 to 70° C., the stirring speed is 200 to 400 rpm, and the pH is 9 to 11.
7. The preparation method according to any one of claims 4 to 6, characterized in that: In step (1) and step (3), the first mixed salt solution is a nickel-iron-manganese mixed salt solution; in step (2), the doped metal ions include any one of Zn ions, Cu ions or Ti ions, or a combination of at least two thereof; Preferably, the total concentration of metal ions in the first mixed salt solution in steps (1) to (3) is 0.5 to 2.0 mol / L; Preferably, the molar amount of the doped metal ions is not higher than 5% based on the molar amount of all metal ions in the second mixed salt solution in step (2); Preferably, steps (1) to (3) are all carried out in a protective atmosphere; Preferably, the D50 particle size of the first precipitate obtained in step (1) is 4 to 6 μm; Preferably, the D50 particle size of the second precipitate obtained in step (2) is 6 to 8 μm; Preferably, the D50 particle size of the precursor obtained in step (3) is 8 to 10 μm.
8. A positive electrode material, characterized in that The positive electrode material is prepared from the precursor according to any one of claims 1 to 3.
9. A process for preparing the positive electrode material according to claim 8, characterized in that: The preparation process comprises: The precursor is mixed with a sodium source and sintered to obtain the positive electrode material.
10. The preparation process according to claim 9, characterized in that: The sodium source includes Na2CO3 and / or NaOH; Preferably, the sintering temperature is 800-900° C. and the sintering time is 10-20 hours.
Citation Information
Patent Citations
Nickel-cobalt-manganese core-shell structure precursor, preparation method thereof and positive electrode material
CN111732132A
Nickel-cobalt-manganese ternary material, precursor thereof, preparation method of precursor, and application of material
CN112928250A
Cited By
Precursor having porous isolation layer, positive electrode material, and preparation therefor and use thereof