Method for preparing microcapsules for marine concrete based on microfluidic technology and application

The marine concrete microcapsules prepared through microfluidic control technology, combined with modified polylactic acid and nanomaterials, solve the problems of poor degradation performance and low strength of existing microcapsules, and realize high-performance and degradable microcapsules, which significantly Improve the performance and environmental friendliness of offshore concrete.

CN118993601APending Publication Date: 2024-11-22ZHEJIANG UNIV

Patent Information

Application Number
CN202411465726.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing microcapsules used for offshore concrete have poor degradation performance and low strength, resulting in poor stability in the marine environment and may cause environmental pollution.

Method used

Microcapsules are prepared by microfluidic control technology, and the mixture of modified polylactic acid and ethyl cellulose is combined with self-healing epoxy resin, nanosilicon dioxide and carbon nanotubes to form high-performance microcapsule core and shell materials. , improve the mechanical strength and self-healing ability of microcapsules, and adjust the pH value through acetic acid to enhance the degradability of microcapsules.

Benefits of technology

It improves the mechanical strength, degradation speed and stability of microcapsules, reduces the risk of environmental pollution, meets the requirements of sustainable development, and significantly improves the performance of offshore concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993601A_ABST
    Figure CN118993601A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing microcapsules for marine concrete based on a microfluidic technology and application, and belongs to the technical field of microcapsule preparation, and the method comprises the following steps: mixing a modified polylactic acid solution and an ethyl cellulose solution, putting into absolute ethyl alcohol, uniformly stirring, and then adjusting the pH value of the solution by using acetic acid to obtain a polymer precursor solution; the preparation method comprises the following steps: putting self-repairing epoxy resin into deionized water, then adding nano silicon dioxide, homogenizing to obtain a mixed solution, then adjusting the pH value of the mixed solution, then adding carbon nanotubes into the mixed solution, and homogenizing to obtain a microcapsule core layer material; dissolving chitosan in acetic acid, stirring to obtain a chitosan solution, and then mixing the chitosan solution with the polymer precursor solution to obtain a microcapsule shell material; based on a micro-fluidic technology, a microcapsule core layer material and a microcapsule shell layer material are respectively pumped into a micro-fluidic chip, and the microcapsule is obtained through liquid dropping, collection and centrifugation. The problems that an existing microcapsule is poor in degradation performance and low in strength are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of microcapsule preparation, and in particular to a method for preparing microcapsules for marine engineering concrete based on microfluidic technology and application thereof. Background Art

[0002] With the continuous development of marine engineering technology, marine concrete is increasingly used in coastal and marine environments. However, marine concrete is often affected by factors such as salt spray erosion, seawater scouring, biological attachment and corrosion in the marine environment, which leads to its performance degradation and shortened service life. In order to overcome this difficulty, researchers are constantly exploring new methods to improve the durability of marine concrete. Among them, microcapsule technology, as an advanced material encapsulation technology, provides a new idea for the protection of marine concrete.

[0003] Microcapsules are a technology that encapsulates solids, liquids or gases in tiny particles, which are called microcapsules. The diameter of microcapsules is usually in the range of micrometers to millimeters, and has the advantages of protecting internal substances, controlling release rate, and improving stability. However, the microcapsules currently used in marine concrete degrade slowly and the degraded materials are prone to environmental pollution, which does not meet the requirements of sustainable development. At the same time, the strength of microcapsules is low, and their application in marine concrete causes problems such as poor stability.

[0004] Therefore, there is an urgent need for a microcapsule with high degradation performance and strength for use in marine concrete. Summary of the invention

[0005] In order to overcome the deficiencies of the prior art, the purpose of the present invention is to provide a method and application of preparing microcapsules for marine concrete based on microfluidic technology, so as to solve the problems of poor degradation performance and low strength of the existing microcapsules.

[0006] To achieve the above object, the present invention provides the following solutions: A method for preparing microcapsules for marine engineering concrete based on microfluidic technology comprises the following steps: S1. Preparation of polymer precursor solution: Mix the modified polylactic acid solution and the ethyl cellulose solution in anhydrous ethanol, stir evenly, and then adjust the pH to 4-6 with acetic acid to obtain a polymer precursor solution; S2. Preparation of microcapsule core layer material: self-healing epoxy resin is placed in deionized water, stirred to obtain a uniform self-healing epoxy resin solution, nano-silicon dioxide is added to the self-healing epoxy resin solution, homogenized to obtain a mixed solution, then the pH value of the mixed solution is adjusted to 6-7, and carbon nanotubes are added to the mixed solution and homogenized to obtain a microcapsule core layer material; S3, preparation of microcapsule shell material: dissolving chitosan in acetic acid, stirring to obtain a chitosan solution, and then mixing the chitosan solution with the prepared polymer precursor solution to obtain a microcapsule shell material; S4, preparing microcapsules: Based on microfluidic technology, the microcapsule core material prepared in step S2 and the microcapsule shell material prepared in step S3 are pumped into two channels of the microfluidic chip respectively, and droplets of inner gel are formed in the microfluidic chip, which are then collected in deionized water and centrifuged to obtain microcapsules.

[0007] Preferably, in S1, the concentration of the modified polylactic acid solution is 10-30% w / v; the concentration of the ethyl cellulose solution is 2-10% w / v; and the volume ratio of the modified polylactic acid solution to the ethyl cellulose solution in S1 is 1-3:1.

[0008] Preferably, in S2, the usage ratio of the self-healing epoxy resin to the nano-silicon dioxide is 1:0.1-1.1; and the usage of the carbon nanotubes is 0.5-5% of the total weight of the self-healing epoxy resin.

[0009] Preferably, in S3, the concentration of the acetic acid is 1-3% v / v, and the ratio of the chitosan to the acetic acid is 1:5-10.

[0010] Preferably, the ratio of the chitosan solution to the polymer precursor solution is 1:1-3.

[0011] Preferably, in S4, the pumping rate of the microcapsule core layer material is 10-100 μL / h, and the pumping rate of the microcapsule shell layer material is 20-300 μL / h; the flow rate ratio of the microcapsule core layer material to the microcapsule shell layer material is 1:2-3.

[0012] Preferably, in S4, after the microcapsules are obtained by centrifugation, the surface of the microcapsules is modified, specifically: the obtained microcapsules are mixed with a modifying agent by a blending method, and the mixture is evenly mixed by mechanical stirring or ultrasonic stirring, and then the modified microcapsules are washed to remove unbound modifying substances to obtain microcapsules with surface modification.

[0013] The present invention also provides an application of microcapsules prepared by the above method for preparing high-performance marine concrete.

[0014] According to the specific embodiments provided by the present invention, the present invention discloses the following technical effects: (1) The present invention prepares a polymer precursor solution with a specific pH environment by mixing modified polylactic acid and ethyl cellulose and adjusting it with anhydrous ethanol and acetic acid, so that the shell layer of the microcapsule has the characteristics of degradability and high strength, thereby improving the performance of the overall material. At the same time, the use of degradable materials such as modified polylactic acid reduces the risk of environmental pollution and meets the requirements of sustainable development.

[0015] (2) The present invention introduces self-healing epoxy resin, nano-silica and carbon nanotubes when preparing microcapsules, which not only improves the mechanical strength and self-healing ability of the microcapsules, but also enhances the conductivity and thermal stability of the microcapsules through nanomaterials.

[0016] (3) The present invention utilizes microfluidic technology to prepare microcapsules, which can accurately control the size, shape and distribution of inner and outer layer materials of the microcapsules, thereby improving the uniformity and stability of the microcapsules. By respectively pumping the core layer material and shell layer material of the microcapsules into different channels of the microfluidic chip, the gelation of the droplets is achieved inside the chip to form microcapsules, which greatly simplifies the process flow, improves production efficiency, and is conducive to the commercial production of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0018] Figure 1 The present invention is a flow chart of a method for preparing microcapsules for marine concrete based on microfluidic technology. DETAILED DESCRIPTION

[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0021] like Figure 1 As shown, the present invention provides a method for preparing microcapsules for marine engineering concrete based on microfluidic technology, comprising the following steps: S1. Preparation of polymer precursor solution: Mix the modified polylactic acid solution and the ethyl cellulose solution in anhydrous ethanol, stir evenly, and then adjust the pH to 4-6 with acetic acid to obtain a polymer precursor solution; Wherein, the concentration of the modified polylactic acid solution is 10-30% w / v; the concentration of the ethyl cellulose solution is 2-10% w / v; and the volume ratio of the modified polylactic acid solution to the ethyl cellulose solution in S1 is 1-3:1.

[0022] S2. Preparation of microcapsule core layer material: self-healing epoxy resin is placed in deionized water, stirred to obtain a uniform self-healing epoxy resin solution, nano-silicon dioxide is added to the self-healing epoxy resin solution, homogenized to obtain a mixed solution, then the pH value of the mixed solution is adjusted to 6-7, and carbon nanotubes are added to the mixed solution and homogenized to obtain a microcapsule core layer material; The ratio of the self-repairing epoxy resin to the nano-silicon dioxide is 1:0.1-1.1; and the amount of the carbon nanotubes is 0.5-5% of the total weight of the self-repairing epoxy resin.

[0023] S3, preparation of microcapsule shell material: dissolving chitosan in acetic acid, stirring to obtain a chitosan solution, and then mixing the chitosan solution with the prepared polymer precursor solution to obtain a microcapsule shell material; Wherein, the concentration of the acetic acid is 1-3% v / v, the ratio of the chitosan to the acetic acid is 1:5-10; the ratio of the chitosan solution to the polymer precursor solution is 1:1-3.

[0024] S4, preparing microcapsules: Based on microfluidic technology, the microcapsule core material prepared in step S2 and the microcapsule shell material prepared in step S3 are pumped into two channels of the microfluidic chip respectively, and droplets of inner gel are formed in the microfluidic chip, which are then collected in deionized water and centrifuged to obtain microcapsules.

[0025] The pumping speed of the microcapsule core material is 10-100 μL / h, and the pumping speed of the microcapsule shell material is 20-300 μL / h; the flow rate ratio of the microcapsule core material to the microcapsule shell material is 1:2-3. In addition, after the microcapsules are obtained by centrifugation, the surface of the microcapsules is modified, specifically: the obtained microcapsules are mixed with the modified agent by a blending method, and the mixture is uniformly mixed by mechanical stirring or ultrasonic stirring, and then the modified microcapsules are washed to remove the unbound modified substances to obtain the surface-modified microcapsules.

[0026] The present invention will be further described below through specific implementation modes.

[0027] Example 1 In this embodiment, the method for preparing microcapsules comprises the following steps: S1. Preparation of polymer precursor solution: Mix the modified polylactic acid solution and the ethyl cellulose solution in anhydrous ethanol, stir evenly, and then adjust the pH to 4-6 with acetic acid to obtain a polymer precursor solution; Among them, the concentration of the modified polylactic acid solution is about 30% w / v; the concentration of the ethyl cellulose solution is about 10% w / v; at this time, the volume ratio of the modified polylactic acid solution and the ethyl cellulose solution in S1 is 3:1.

[0028] S2. Preparation of microcapsule core layer material: self-healing epoxy resin is placed in deionized water, stirred to obtain a uniform self-healing epoxy resin solution, nano-silicon dioxide is added to the self-healing epoxy resin solution, homogenized to obtain a mixed solution, then the pH value of the mixed solution is adjusted to 6-7, and carbon nanotubes are added to the mixed solution and homogenized to obtain a microcapsule core layer material; The usage ratio of the self-repairing epoxy resin to the nano-silicon dioxide is 1:1; and the usage of the carbon nanotubes is 0.5-5% of the total weight of the self-repairing epoxy resin.

[0029] S3, preparation of microcapsule shell material: dissolving chitosan in acetic acid, stirring to obtain a chitosan solution, and then mixing the chitosan solution with the prepared polymer precursor solution to obtain a microcapsule shell material; Wherein, the concentration of the acetic acid is 1% v / v, the ratio of the chitosan to the acetic acid is 1:5; the ratio of the chitosan solution to the polymer precursor solution is 1:2.

[0030] S4, preparing microcapsules: Based on microfluidic technology, the microcapsule core material prepared in step S2 and the microcapsule shell material prepared in step S3 are pumped into two channels of the microfluidic chip respectively, and droplets of inner gel are formed in the microfluidic chip, which are then collected in deionized water and centrifuged to obtain microcapsules.

[0031] The pumping speed of the microcapsule core material is 10~100μL / h. In the initial stage of pumping, the flow rate can be gradually increased from a lower flow rate (10~20μL / h), and the effect of the flow rate on the droplet stability and size can be observed, and the flow rate can be increased again. The pumping speed of the microcapsule shell material is 20~300μL / h; the flow rate ratio of the microcapsule core material to the microcapsule shell material is 1:2. In addition, after the microcapsules are obtained by centrifugation, the surface of the microcapsules is also modified, specifically: the obtained microcapsules are mixed with the modified agent by a blending method, and the mixture is evenly mixed by mechanical stirring or ultrasonic stirring, and then the modified microcapsules are washed to remove the unbound modified substances to obtain surface-modified microcapsules.

[0032] The microcapsules prepared by the above method are spherical with a size of 100 μm, and the self-healing epoxy resin / nano-silicon dioxide / carbon nanotube composite material is wrapped inside.

[0033] Example 2 In this embodiment, the preparation method of microcapsules includes: S1. Preparation of polymer precursor solution: Mix the modified polylactic acid solution and the ethyl cellulose solution in anhydrous ethanol, stir evenly, and then adjust the pH to 4-6 with acetic acid to obtain a polymer precursor solution; Wherein, the concentration of the modified polylactic acid solution is 20% w / v; the concentration of the ethyl cellulose solution is 10% w / v; and the volume ratio of the modified polylactic acid solution to the ethyl cellulose solution in S1 is 2:1.

[0034] S2. Preparation of microcapsule core layer material: self-healing epoxy resin is placed in deionized water, stirred to obtain a uniform self-healing epoxy resin solution, nano-silicon dioxide is added to the self-healing epoxy resin solution, homogenized to obtain a mixed solution, then the pH value of the mixed solution is adjusted to 6-7, and carbon nanotubes are added to the mixed solution and homogenized to obtain a microcapsule core layer material; The ratio of the self-repairing epoxy resin to the nano-silicon dioxide is 1:1.1; and the amount of the carbon nanotubes is 0.5-5% of the total weight of the self-repairing epoxy resin.

[0035] S3, preparation of microcapsule shell material: dissolving chitosan in acetic acid, stirring to obtain a chitosan solution, and then mixing the chitosan solution with the prepared polymer precursor solution to obtain a microcapsule shell material; Wherein, the concentration of the acetic acid is 23% v / v, the ratio of the chitosan to the acetic acid is 1:7; the ratio of the chitosan solution to the polymer precursor solution is 1:1.

[0036] S4, preparing microcapsules: Based on microfluidic technology, the microcapsule core material prepared in step S2 and the microcapsule shell material prepared in step S3 are pumped into two channels of the microfluidic chip respectively, and droplets of inner gel are formed in the microfluidic chip, which are then collected in deionized water and centrifuged to obtain microcapsules.

[0037] The pumping speed of the microcapsule core material is 10-100 μL / h, and the pumping speed of the microcapsule shell material is 20-300 μL / h; the flow rate ratio of the microcapsule core material to the microcapsule shell material is 1:2. In addition, after the microcapsules are obtained by centrifugation, the surface of the microcapsules is modified, specifically: the obtained microcapsules are mixed with the modified agent by a blending method, and the mixture is uniformly mixed by mechanical stirring or ultrasonic stirring, and then the modified microcapsules are washed to remove the unbound modified substances to obtain the surface-modified microcapsules.

[0038] The microcapsules prepared by the above method are spherical with a size of (97.7±6.0) μm, and the self-healing epoxy resin / nano-silica / carbon nanotube composite material is wrapped inside.

[0039] Example 3 In this embodiment, the preparation method of microcapsules includes: S1. Preparation of polymer precursor solution: Mix the modified polylactic acid solution and the ethyl cellulose solution in anhydrous ethanol, stir evenly, and then adjust the pH to 4-6 with acetic acid to obtain a polymer precursor solution; Wherein, the concentration of the modified polylactic acid solution is 10% w / v; the concentration of the ethyl cellulose solution is 5% w / v; and the volume ratio of the modified polylactic acid solution to the ethyl cellulose solution in S1 is 1:1.

[0040] S2. Preparation of microcapsule core layer material: self-healing epoxy resin is placed in deionized water, stirred to obtain a uniform self-healing epoxy resin solution, nano-silicon dioxide is added to the self-healing epoxy resin solution, homogenized to obtain a mixed solution, then the pH value of the mixed solution is adjusted to 6-7, and carbon nanotubes are added to the mixed solution and homogenized to obtain a microcapsule core layer material; The ratio of the self-repairing epoxy resin to the nano-silicon dioxide is 1:0.5; and the amount of the carbon nanotubes is 0.5-5% of the total weight of the self-repairing epoxy resin.

[0041] S3, preparation of microcapsule shell material: dissolving chitosan in acetic acid, stirring to obtain a chitosan solution, and then mixing the chitosan solution with the prepared polymer precursor solution to obtain a microcapsule shell material; Wherein, the concentration of the acetic acid is 3% v / v, the ratio of the chitosan to the acetic acid is 1:10; the ratio of the chitosan solution to the polymer precursor solution is 1:3.

[0042] S4, preparing microcapsules: Based on microfluidic technology, the microcapsule core material prepared in step S2 and the microcapsule shell material prepared in step S3 are pumped into two channels of the microfluidic chip respectively, and droplets of inner gel are formed in the microfluidic chip, which are then collected in deionized water and centrifuged to obtain microcapsules.

[0043] The pumping speed of the microcapsule core material is 10-100 μL / h, and the pumping speed of the microcapsule shell material is 20-300 μL / h; the flow rate ratio of the microcapsule core material to the microcapsule shell material is 1:3. In addition, after the microcapsules are obtained by centrifugation, the surface of the microcapsules is modified, specifically: the obtained microcapsules are mixed with the modified agent by a blending method, and the mixture is uniformly mixed by mechanical stirring or ultrasonic stirring, and then the modified microcapsules are washed to remove the unbound modified substances to obtain the surface-modified microcapsules.

[0044] The microcapsules prepared by the above method are spherical with a size of (96.5±5.7) μm, and the self-healing epoxy resin / nano-silica / carbon nanotube composite material is wrapped inside.

[0045] Comparative Example 1 The difference from Example 1 is that unmodified polylactic acid is used to prepare the obtained microcapsules.

[0046] Comparative Example 2 The difference from Example 1 is that the use of self-healing epoxy resin is eliminated during the preparation process, and other raw materials and processes are the same.

[0047] Comparative Example 3 The difference from Comparative Example 2 is that nano-silicon dioxide and carbon nanotubes are not added to the self-healing epoxy resin in batches during the preparation process.

[0048] The concrete performance test was carried out on the microcapsules prepared according to Examples 1 to 3 and Comparative Examples 1 to 3, and the results obtained are shown in Table 1.

[0049] Referring to Table 1, it can be found that the performance of the microcapsules prepared in Examples 1 to 3 is better than that of Comparative Documents 1 to 3, and the microcapsules prepared in Example 1 are better than those in other embodiments in terms of compressive strength, degradation rate and loading repair amount. This proves that the compressive strength of the microcapsules prepared by the method of the present invention can reach more than 13MPa, while the existing microcapsules can generally reach 8-10MPa, indicating that the preparation method of the present invention can improve its mechanical strength.

[0050] At the same time, according to the degradation rates shown in Examples 1 to 3 and Comparative Examples 1 to 3, it can be found that the microcapsules of the present invention degrade faster, so that when the marine engineering concrete has self-repairing ability, the use of degradable materials such as modified polylactic acid reduces the risk of environmental pollution and meets the requirements of sustainable development.

[0051] Table 1 Comparison of microcapsule properties ;

[0052] In addition, the microcapsules prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were used in marine engineering concrete, and the results obtained are shown in Table 2.

[0053] Table 2 Application effect of marine engineering concrete ;

[0054] From the above results, it can be seen that the microcapsules prepared by the method of the present invention can be applied to marine engineering concrete to greatly enhance the performance of marine engineering concrete. By comparing Examples 1 to 3, it can be seen that the prepared microcapsules solve the problems of poor degradation ability and low strength of existing microcapsules.

[0055] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the system disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0056] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for preparing microcapsules for marine concrete based on microfluidic technology, characterized in that: The following steps are involved: S1. Preparation of polymer precursor solution: Mix the modified polylactic acid solution and the ethyl cellulose solution in anhydrous ethanol, stir evenly, and then adjust the pH to 4-6 with acetic acid to obtain a polymer precursor solution; S2. Preparation of microcapsule core layer material: self-healing epoxy resin is placed in deionized water, stirred to obtain a uniform self-healing epoxy resin solution, nano-silicon dioxide is added to the self-healing epoxy resin solution, homogenized to obtain a mixed solution, then the pH value of the mixed solution is adjusted to 6-7, and carbon nanotubes are added to the mixed solution and homogenized to obtain a microcapsule core layer material; S3, preparation of microcapsule shell material: dissolving chitosan in acetic acid, stirring to obtain a chitosan solution, and then mixing the chitosan solution with the prepared polymer precursor solution to obtain a microcapsule shell material; S4, preparing microcapsules: Based on microfluidic technology, the microcapsule core material prepared in step S2 and the microcapsule shell material prepared in step S3 are pumped into two channels of the microfluidic chip respectively, and droplets of inner gel are formed in the microfluidic chip, which are then collected in deionized water and centrifuged to obtain microcapsules.

2. The method for preparing microcapsules for marine engineering concrete based on microfluidic technology according to claim 1, characterized in that: In the S1, the concentration of the modified polylactic acid solution is 10-30% w / v; the concentration of the ethyl cellulose solution is 2-10% w / v; and the volume ratio of the modified polylactic acid solution to the ethyl cellulose solution in the S1 is 1-3:

1.

3. The method for preparing microcapsules for marine concrete based on microfluidic technology according to claim 1, characterized in that: In S2, the ratio of the self-healing epoxy resin to the nano-silicon dioxide is 1:0.1-1.1; the amount of the carbon nanotubes is 0.5-5% of the total weight of the self-healing epoxy resin.

4. The method for preparing microcapsules for marine concrete based on microfluidic technology according to claim 1, characterized in that: In S3, the concentration of the acetic acid is 1-3% v / v, and the ratio of the chitosan to the acetic acid is 1:5-10.

5. The method for preparing microcapsules for marine concrete based on microfluidic technology according to claim 4, characterized in that: The ratio of the chitosan solution to the polymer precursor solution is 1:1-3.

6. The method for preparing microcapsules for marine concrete based on microfluidic technology according to claim 1, characterized in that: In S4, the pumping speed of the microcapsule core layer material is 10-100 μL / h, and the pumping speed of the microcapsule shell layer material is 20-300 μL / h; the flow rate ratio of the microcapsule core layer material to the microcapsule shell layer material is 1:2-3.

7. The method for preparing microcapsules for marine concrete based on microfluidic technology according to claim 6, characterized in that: In the S4, after the microcapsules are obtained by centrifugation, the surface of the microcapsules is modified. Specifically, the obtained microcapsules are mixed with a modifying agent by a blending method, and the mixture is evenly mixed by mechanical stirring or ultrasonic stirring. The modified microcapsules are then washed to remove unbound modifying substances, thereby obtaining microcapsules with surface modification.

8. Use of microcapsules prepared by the method according to any one of claims 1 to 7, characterized in that: Used to prepare high-performance marine concrete.

Citation Information

Patent Citations

  • Preparation method of chitosan microcapsule with uniform size and controllable size

    CN103721655A

  • Water-environment concrete self-dissolved microcapsule self-repairing system

    CN105645802A

  • Biocompatible water-core microcapsules and preparation method thereof

    CN106975425A

  • Preparation method of epoxy resin microcapsule with self-repairing function

    CN110975773A

  • Hybrid self-repairing microcapsule as well as preparation method and application thereof

    CN113461361A

Cited By

  • Temperature-sensitive microcapsule with internal maintenance and anti-corrosion functions as well as preparation method and application of temperature-sensitive microcapsule

    CN119528475A