Ceramic fiber aerogel heat insulation pad and preparation method thereof

Through the layer-layer structure of the ceramic fiber aerogel thermal insulation pad, the thermal runaway and flame propagation problems of lithium-ion batteries under extreme conditions are solved, and the thermal protection and high-temperature fire protection of the battery cell are realized to ensure safety.

CN118993693APending Publication Date: 2024-11-22FUJIAN TENBOND NEW MATERIALS TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410884816.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Lithium-ion power batteries have the risk of combustion and explosion under extreme conditions. Traditional partitions cannot effectively prevent thermal runaway and flame propagation, causing the battery module to catch fire and explode.

Method used

A ceramic fiber aerogel heat insulation pad is used, which consists of 70-80% tetraethoxysilane TEOS and 20-30% ceramic fiber. A layer-layered cotton-shaped structure is formed through a specific preparation method, with excellent thermal insulation. and buffering function for thermal protection between battery cells.

Benefits of technology

Effectively prevent the battery cell from getting out of control, adapt to the expansion and contraction of the battery cell during charging and discharging, and isolate high temperatures and prevent flames from spilling out during explosions, so as to win time to escape.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993693A_ABST
    Figure CN118993693A_ABST
Patent Text Reader

Abstract

The invention provides a ceramic fiber aerogel heat insulation pad and a preparation method thereof. The ceramic fiber aerogel heat insulation pad comprises the following raw material components in percentage by weight: 70-80% of tetraethoxysilane TEOS and 20-30% of ceramic fibers. The volume ratio of the ethanol to the TEOS is (3-5): 1, and the dosage of the ammonia water is 8-12% of the volume of the TEOS. The preparation method comprises the following steps: mixing TEOS with ethanol, adding ammonia water as a catalyst, and fully mixing and hydrolyzing; after the hydrolysis reaction starts for 5-15 minutes, slowly adding ceramic fibers into the mixture, and uniformly mixing; stirring until the mixture becomes turbid and starts to solidify; when the gel begins to form, pouring the gel into a mold in a layered pouring manner, and pouring the mixture of the next layer after each layer of gel is slightly cured; and finally freeze-drying and forming. The product disclosed by the invention is of a layer-by-layer overlapped cotton-fiber-shaped structure, has excellent heat insulation and buffering functions, can be used for thermal protection between battery cells, can prevent thermal runaway of the cells, and adapts to expansion and contraction changes of the cells in the charging and discharging process of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of new energy power batteries, and in particular to a ceramic fiber aerogel thermal insulation pad and a preparation method thereof. [Background technology]

[0002] At present, electric vehicles mainly use lithium-ion batteries as power batteries. After years of development, the safety of lithium-ion power batteries has been significantly improved, but under extreme conditions, lithium batteries still have the risk of combustion and explosion. When a lithium-ion battery has an internal or external short circuit, the battery releases a large amount of heat in a short period of time, and the temperature rises sharply, leading to thermal runaway. The flammable liquid electrolyte is ignited at high temperatures, causing the battery to catch fire. Through heat diffusion, a single thermal runaway battery triggers thermal runaway in adjacent batteries through heat conduction and flames, causing the entire battery module / battery pack to have thermal runaway, thereby causing a fire and explosion.

[0003] Traditional battery modules use flame-retardant plastic partitions such as PP, ABS, and PVC to separate the single cells from each other, which does not provide thermal isolation protection. It is also easy to cause the battery temperature to be too high, resulting in the dissolution of the partition and fire. Aerogel is the solid material with the lowest thermal conductivity known so far. The thermal insulation performance of aerogel insulation felts, insulation boards, insulation papers and other products can be up to 5 times that of ordinary products. In addition to excellent fire retardancy, softness and impact resistance, sound insulation and noise reduction, in addition to achieving good promotion in the fields of industrial energy conservation and civil insulation, with the development of the aerogel industry, aerogel is also increasingly widely used in the field of batteries. Its application in new energy vehicles can better achieve battery temperature control and electronic control management and improve performance, play a role in thermal insulation and fire prevention, and buy more time for users and passengers to escape from the scene and extinguish the fire. [Summary of the invention]

[0004] One of the technical problems to be solved by the present invention is to provide a ceramic fiber aerogel insulation pad, which is a cotton-like structure stacked layer by layer, has excellent insulation and buffering functions, can be used for thermal protection between battery cells, can prevent thermal runaway of the battery cells, and adapt to the expansion and contraction changes of the battery cells during charging and discharging.

[0005] The present invention achieves one of the above-mentioned technical problems by:

[0006] A ceramic fiber aerogel thermal insulation pad, the raw material components and their weight percentages are as follows: 70-80% tetraethoxysilane TEOS, 20-30% ceramic fiber; the solvent is ethanol, the catalyst is ammonia water, the volume ratio of the ethanol to TEOS is 3-5:1, the amount of the ammonia water is 8-12% of the volume of TEOS; the diameter of the ceramic fiber is 1-10 microns, and the length is 0.5-3 millimeters.

[0007] Furthermore, the volume ratio of ethanol to TEOS is 4:1.

[0008] Furthermore, the amount of ammonia water used is 10% of the volume of TEOS.

[0009] The second technical problem to be solved by the present invention is to provide a method for preparing a ceramic fiber aerogel insulation pad. The prepared product is a cotton-like structure stacked layer by layer, has excellent insulation and buffering functions, can be used for thermal protection between battery cells, can prevent thermal runaway of the battery cells, and adapt to the expansion and contraction changes of the battery cells during charging and discharging.

[0010] The present invention achieves the second of the above technical problems in this way:

[0011] A method for preparing a ceramic fiber aerogel thermal insulation pad as claimed in any one of claims 1 to 3, characterized in that the preparation method comprises the following steps:

[0012] Step 1, pretreatment: TEOS and ethanol are mixed in proportion, and then ammonia water is added as a catalyst, and mixed thoroughly to start the hydrolysis process;

[0013] Step 2, adding ceramic fiber: 5-15 minutes after the hydrolysis reaction begins, slowly add the ceramic fiber to the mixture and mix well;

[0014] Step 3, gel formation: Continue stirring until the mixture becomes cloudy and begins to solidify;

[0015] Step 4, molding: When the gel begins to form, pour the mixture into the mold in layers, with each layer of gel being 2-5 mm thick. After each layer of gel is slightly solidified, pour the next layer of mixture;

[0016] Step 5, freeze drying: directly put the mold containing the gel into a freeze dryer and freeze dry it into a cotton-like structure; the specific freeze drying operation is as follows:

[0017] 5.1. Pre-freezing stage: Place the gel mixture in the mold into the freezer chamber of the freeze dryer, and ensure that the temperature drops quickly to the set low temperature so that the water molecules form ice crystals;

[0018] 5.2. Primary drying and sublimation stage: Raise the temperature by 10-30°C and control the pressure at 0.1-0.2 mbar to sublimate the ice crystals and convert the water directly from solid to gas;

[0019] 5.3. Secondary drying and desorption stage: gradually increase the temperature and control the pressure at 0.01-0.05 mbar to remove the moisture adsorbed on the surface of the material;

[0020] Step 6, post-processing: After the aerogel is dried, remove the excess part of the mold edge.

[0021] Furthermore, the conditions of each drying stage in step 5 are as follows:

[0022] Pre-freezing stage: temperature is -50℃ to -80℃, time is 2-4 hours;

[0023] Primary drying sublimation stage: temperature is -40℃ to -50℃, time is 24-36 hours;

[0024] Secondary drying and desorption stage: temperature is 20℃ to 30℃, time is 12-24 hours.

[0025] The present invention has the following advantages:

[0026] The ceramic fiber aerogel insulation pad of the present invention is a cotton-like structure stacked layer by layer, with excellent insulation and buffering functions, and can be used for thermal protection between battery cells to prevent thermal runaway of the battery cells. It has good compression performance, and while providing insulation, it can also be used as a buffer material between battery cells to adapt to the expansion and contraction changes of the battery cells during the charging and discharging process. At the same time, if an accident occurs, the high-temperature fireproof function of the insulation pad can isolate the high temperature and prevent the spillover of the flame at the moment of the battery cell explosion, thus buying time for the people in the car to escape.

Brief Description of the Drawings

[0027] The present invention will be further described below in conjunction with embodiments with reference to the accompanying drawings.

[0028] Figure 1 It is a schematic diagram of an enlarged cross-sectional structure of a ceramic fiber aerogel thermal insulation pad of the present invention. [Specific implementation method]

[0029] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0030] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0031] The invention relates to a ceramic fiber aerogel thermal insulation pad. The raw material components and their weight percentages are as follows: 70-80% of tetraethoxysilane TEOS and 20-30% of ceramic fiber; the solvent is ethanol, the catalyst is ammonia water, the volume ratio of the ethanol to TEOS is 3-5:1, and the amount of the ammonia water is 8-12% of the volume of TEOS; the diameter of the ceramic fiber is 1-10 microns, and the length is 0.5-3 millimeters.

[0032] In a specific implementation, a preferred embodiment is: the volume ratio of ethanol to TEOS is 4:1.

[0033] In a specific implementation, a preferred embodiment is: the amount of ammonia water used is 10% of the volume of TEOS.

[0034] The present invention also relates to a method for preparing the ceramic fiber aerogel thermal insulation pad, and the steps of the preparation method are as follows:

[0035] Step 1, pretreatment: TEOS and ethanol are mixed in proportion, and then ammonia water is added as a catalyst, and mixed thoroughly to start the hydrolysis process;

[0036] Step 2, adding ceramic fiber: 5-15 minutes after the hydrolysis reaction begins, slowly add the ceramic fiber to the mixture and mix well;

[0037] Step 3, gel formation: Continue stirring until the mixture becomes cloudy and begins to solidify;

[0038] Step 4, molding: When the gel begins to form, pour the mixture into the mold in layers, with each layer of gel being 2-5 mm thick. After each layer of gel is slightly solidified, pour the next layer of mixture;

[0039] Step 5, freeze drying: directly put the mold containing the gel into a freeze dryer and freeze dry it into a cotton-like structure; the specific freeze drying operation is as follows:

[0040] 5.1. Pre-freezing stage: Place the gel mixture in the mold into the freezer chamber of the freeze dryer, and ensure that the temperature drops quickly to the set low temperature so that the water molecules form ice crystals;

[0041] 5.2. Primary drying and sublimation stage: Raise the temperature by 10-30°C and control the pressure at 0.1-0.2 mbar to sublimate the ice crystals and convert the water directly from solid to gas;

[0042] 5.3. Secondary drying and desorption stage: gradually increase the temperature and control the pressure at 0.01-0.05 mbar to remove the moisture adsorbed on the surface of the material;

[0043] Step 6, post-processing: After the aerogel is dried, remove the excess part of the mold edge.

[0044] The conditions of each drying stage in step 5 are as follows:

[0045] Pre-freezing stage: temperature is -50℃ to -80℃, time is 2-4 hours;

[0046] Primary drying sublimation stage: temperature is -40℃ to -50℃, time is 24-36 hours;

[0047] Secondary drying and desorption stage: temperature is 20℃ to 30℃, time is 12-24 hours.

[0048] The following will be combined with the attached Figure 1 The technical scheme of the present invention is clearly and completely described in detail with specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0049] Example:

[0050] (1) The raw material ratio of ceramic fiber aerogel insulation pad is as follows:

[0051] ①Main raw materials: tetraethoxysilane (TEOS) 75%; ceramic fiber 25%;

[0052] ②Solvent: ethanol, the volume ratio of ethanol to TEOS is maintained at 4:1;

[0053] ③ Catalyst: ammonia water, the dosage is 10% of the volume of TEOS;

[0054] (2) A method for preparing a ceramic fiber aerogel thermal insulation pad, comprising the following steps:

[0055] Step 1, pretreatment: TEOS and ethanol are mixed in a ratio of 4:1, and then 10% ammonia water is added as a catalyst and mixed thoroughly to start the hydrolysis process;

[0056] Step 2, adding ceramic fibers: 10 minutes after the hydrolysis reaction begins, slowly add 25% by weight of ceramic fibers to the mixture and mix well to make the ceramic fibers evenly distributed;

[0057] Step 3, gel formation: Continue stirring until the mixture becomes cloudy and begins to solidify;

[0058] Step 4, molding: When the gel begins to form, pour the mixture into the mold in layers, with each layer of gel being 2-5 mm thick. After each layer of gel is slightly solidified, pour the next layer of mixture. The insulation pad gel is layered to achieve a layered structure to improve the cushioning performance of the insulation pad.

[0059] Step 5, freeze drying: directly put the mold containing the gel into a freeze dryer and freeze dry it into a cotton-like structure; the specific freeze drying operation is as follows:

[0060] 5.1. Pre-freezing stage: put the gel mixture in the mold into the freezer of a freeze dryer at -70°C and freeze for 3 hours to ensure that the temperature of the gel mixture drops quickly to the set low temperature so that water molecules form ice crystals;

[0061] 5.2. Primary drying sublimation stage: Raise the temperature to -45°C, control the pressure at 0.1-0.2 mbar, maintain low temperature and low pressure environment, freeze for 30 hours, allow ice crystals to sublime, and convert water directly from solid to gas; this stage is the main stage of freeze drying, which requires stable temperature and pressure control. Through sublimation, ice crystals are directly converted into water vapor, forming a cotton-like structure inside the gel mixture, further improving the buffering performance of the product.

[0062] 5.3. Secondary drying and desorption stage: gradually increase the temperature to 25°C while maintaining low pressure at 0.01-0.05 mbar for 20 hours to ensure that the residual moisture on the surface of the material is completely removed to achieve the final low moisture content;

[0063] During the freeze-drying process, the water molecules in the gel mixture are directly converted from solid sub-ice to gas, thus avoiding a large amount of shrinkage and deformation, thereby forming a cotton-like structure, further improving the cushioning performance of the thermal insulation pad;

[0064] Step 6, post-processing: After the aerogel is dried, remove the excess part of the mold edge to ensure the size consistency, and then roll it up for use.

[0065] (3) Packaging of ceramic fiber aerogel insulation pad:

[0066] The above-prepared product (aerogel roll) is packaged by using high-strength adhesive tape (the main body of the tape structure is acrylic glue + PET + acrylic glue) and roller cutting tools and plastic sealing slicing technology to form a special structure. The steps are as follows:

[0067] Step 1, Aerogel roll: Make sure the surface of the aerogel roll is dry, clean, and free of dust or other impurities. This is crucial to ensure the uniformity and firmness of the tape.

[0068] Step 2: Stick the tape: Spread the PET double-sided tape flat and carefully place the aerogel roll on one side of the tape, making sure the aerogel roll is aligned with the edge of the tape.

[0069] Step 3: Use a roller cutter to cut the aerogel, and use a plastic sealing slicer to laminate the double-sided tape on the upper and lower sides of the aerogel. While cutting the product, cut a sealing notch on one side to ensure that the gas in the insulation pad can be discharged.

[0070] (4) Main technical indicators of the products prepared above:

[0071] ① Thermal conductivity ≤ 0.045W / (m·K)at25℃;

[0072] ② Flame retardant meets UL94V0;

[0073] ③High temperature resistance 1200℃;

[0074] ④Insulation resistance 1000VDC, ≥500MΩ;

[0075] ⑤ Withstand voltage 6000VDC, leakage current ≤1mA;

[0076] ⑥ Environmental protection meets regulations 2011 / 65 / EU (RoHS);

[0077] ⑦ When compressed by 50%, the compressive stress is ≥30KPa.

[0078] The cross-sectional structure of the product prepared above is as follows Figure 1 shown.

[0079] In summary, the present invention adds ceramic fiber to the gel for reinforcement, and adopts a special freeze-drying process, and finally produces a layered aerogel with a cotton-like structure, which has excellent thermal insulation and buffering properties. When the battery cell is charged and discharged and expansion and contraction occur, the thermal insulation pad pasted on the surface of the battery cell will first isolate the heat transfer between the battery cells, and at the same time, the pressure of the expanded battery cell will be absorbed by the middle cotton-like core material, while achieving the buffering and heat insulation effects. The air in the middle of the compressed thermal insulation pad is discharged from the side cutout, which fundamentally eliminates the air sealed in after the thermal insulation pad is packaged. During the compression process, the air has nowhere to be released in the thermal insulation pad, and there is a risk of extrusion and explosion of the thermal insulation. At the same time, if an accident occurs, the moment the battery cell explodes, the high-temperature fireproof function of the thermal insulation pad can isolate the high temperature and prevent the spillover of the flame, so as to gain time for the people in the car to escape.

[0080] Although the specific implementation modes of the present invention are described above, those skilled in the art should understand that the specific implementation modes described are only illustrative and are not intended to limit the scope of the present invention. Equivalent modifications and changes made by those skilled in the art in accordance with the spirit of the present invention should be included in the scope of protection of the claims of the present invention.

Claims

1. A ceramic fiber aerogel thermal insulation pad, characterized in that: The raw material components and their weight percentages are as follows: 70-80% tetraethoxysilane TEOS, 20-30% ceramic fiber; the solvent is ethanol, the catalyst is ammonia water, the volume ratio of the ethanol to TEOS is 3-5:1, and the amount of the ammonia water is 8-12% of the volume of TEOS; the diameter of the ceramic fiber is 1-10 microns, and the length is 0.5-3 millimeters.

2. The ceramic fiber aerogel thermal insulation pad according to claim 1, characterized in that: The volume ratio of ethanol to TEOS is 4:

1.

3. The ceramic fiber aerogel thermal insulation pad according to claim 1, characterized in that: The amount of ammonia water used is 10% of the volume of TEOS.

4. A method for preparing a ceramic fiber aerogel thermal insulation pad according to any one of claims 1 to 3, characterized in that: The preparation method steps are as follows: Step 1, pretreatment: TEOS and ethanol are mixed in proportion, and then ammonia water is added as a catalyst, and mixed thoroughly to start the hydrolysis process; Step 2, adding ceramic fiber: 5-15 minutes after the hydrolysis reaction begins, slowly add the ceramic fiber to the mixture and mix well; Step 3, gel formation: Continue stirring until the mixture becomes cloudy and begins to solidify; Step 4, molding: When the gel begins to form, pour the mixture into the mold in layers, with each layer of gel being 2-5 mm thick. After each layer of gel is slightly solidified, pour the next layer of mixture; Step 5, freeze drying: directly put the mold containing the gel into a freeze dryer and freeze dry it into a cotton-like structure; the specific freeze drying operation is as follows: 5.

1. Pre-freezing stage: Place the gel mixture in the mold into the freezer chamber of the freeze dryer, and ensure that the temperature drops quickly to the set low temperature so that the water molecules form ice crystals; 5.

2. Primary drying and sublimation stage: Raise the temperature by 10-30°C and control the pressure at 0.1-0.2 mbar to sublimate the ice crystals and convert the water directly from solid to gas; 5.

3. Secondary drying and desorption stage: gradually increase the temperature and control the pressure at 0.01-0.05 mbar to remove the moisture adsorbed on the surface of the material; Step 6, post-processing: After the aerogel is dried, remove the excess part of the mold edge.

5. The method for preparing a ceramic fiber aerogel thermal insulation pad according to claim 4, characterized in that: The conditions of each drying stage in step 5 are as follows: Pre-freezing stage: temperature is -50℃ to -80℃, time is 2-4 hours; Primary drying and sublimation stage: temperature is -40℃ to -50℃, time is 24-36 hours; Secondary drying and desorption stage: temperature is 20℃ to 30℃, time is 12-24 hours.

Citation Information

Cited By

  • Fireproof thermal insulation material for new energy automobile battery and preparation method of fireproof thermal insulation material

    CN120118519A

  • System and method for inhibiting thermal runaway of lithium ion battery of new energy automobile

    CN120565861A