Method for preparing cyclohexanone through selective oxidation of cyclohexanol

By using transition metal modified graphite phase carbon nitride catalysts, catalyzing oxidation of cyclohexanol under solvent-free conditions of oxygen or air oxidant, the problems of low catalyst activity, high cost and environmental pollution in the prior art are solved, and the ring is realized The efficient conversion of hexanol and the high selectivity of cyclohexanone are suitable for industrial production.

CN118993857APending Publication Date: 2024-11-22HUNAN NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411080317.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the catalyst prepared by cyclohexanone by one-step oxidation method of cyclohexanol is weak in activity, low efficiency, high cost, poor recycling and environmental pollution problems, making it difficult to meet the needs of industrial production.

Method used

Using transition metal-modified graphite phase carbon nitride as a catalyst, using oxygen or air as an oxidizing agent to catalyze oxidize cyclohexanol under the conditions of organic solvents and additives, the catalyst preparation method is simple, low cost, strong activity, Good thermal stability and recyclable.

Benefits of technology

The high conversion rate of cyclohexanol and the high selectivity of cyclohexanone were achieved. The catalyst still maintained good activity after recycling for more than 8 times. The reaction system was simple, green and efficient, reducing production costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to a method for preparing cyclohexanone by selective oxidation of cyclohexanol, which adopts transition metal modified graphite phase carbon nitride as a catalyst and oxygen or air as an oxidizing agent to catalytically oxidize cyclohexanol to prepare cyclohexanone. The preparation method of the catalyst is simple and convenient, low in production cost and suitable for industrial production, and the 1% V / g-C3N4 catalyst has the advantages of being high in catalytic activity, high in catalytic efficiency, good in thermal stability, convenient to recycle, stable in catalytic performance after being recycled for 8 times and the like; according to the method, oxygen or air is adopted as an oxidizing agent, the use of hydrogen peroxide, nitric acid, chromium trioxide, potassium permanganate and other oxidizing agents which are not easy to prepare, flammable and explosive, harmful to the environment and high in cost is avoided, other solvents and additives do not need to be added in the reaction process, and the whole reaction system is simple, green and efficient, so that the method is an environment-friendly catalytic oxidation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysis, and in particular relates to a method for preparing cyclohexanone by selective oxidation of cyclohexanol. Background Art

[0002] Cyclohexanone has excellent properties such as low toxicity, low volatility and high solubility. It is an organic solvent widely used in the fields of pesticides, coatings, adhesives, inks, etc. At the same time, cyclohexanone is a very important organic chemical raw material and intermediate, which can be used to produce fine chemicals such as caprolactam, adipic acid and nylon 66. In recent years, with the increasing demand for chemical fiber products such as nylon 6, nylon 66 and nylon, the demand for upstream raw material cyclohexanone has also increased. How to research and develop efficient and green cyclohexanone preparation methods has attracted much attention.

[0003] In the traditional production process, the preparation methods of cyclohexanone include phenol hydrogenation, cyclohexene hydration, cyclohexane oxidation and cyclohexanol dehydrogenation. These methods have the problems of harsh reaction conditions, low conversion rate of raw materials and product selectivity, long process route, high requirements for production equipment, high energy consumption and production cost, and serious environmental pollution. In order to solve some of the problems existing in the above traditional production processes, the simple and economical one-step oxidation process of cyclohexanol to directly prepare cyclohexanone has become a research hotspot for many scientific researchers in recent years.

[0004] In the traditional one-step oxidation process of cyclohexanol to directly prepare cyclohexanone, oxidants such as chromium trioxide, potassium dichromate, potassium permanganate, etc. are often used. Although these oxidants have strong oxidizing properties, they are easy to corrode equipment, causing serious environmental pollution, and the post-processing process of the product is also difficult. Therefore, it is very necessary to use environmentally friendly oxidants such as hydrogen peroxide and oxygen.

[0005] Zhao Yu et al. used H 2 O 2 As an oxidant, vanadium phosphate solid prepared with water and ionic liquid as solvent was used as a catalyst, and acetonitrile was used as a solvent. Under mild conditions of 70°C and 1atm for 12h, a cyclohexanol conversion rate of 69.6% and a cyclohexanone selectivity of 83.3% were achieved (Catalysis Letters, 2021, 151: 2366-2375). Xue Yingxue et al. used H 2 O 2As an oxidant, a dimer monoFe(III)-substituted Keggin-type phosphotungstate modified by an organic ammonium salt cation is used as a catalyst, and tert-butyl alcohol is used as a solvent. The reaction is carried out under mild conditions of 80°C and 1atm for 12 hours. The conversion rate of cyclohexanol can reach 92.0%, and the selectivity of cyclohexanone is as high as 99.0% (Molecular Catalysis, 2020, 492, 111010). However, the catalyst preparation steps of the above two methods are numerous and the conditions are harsh. It is not easy to use them in large quantities. In addition, a large amount of organic solvents are used, which will also cause environmental pollution.

[0006] Chinese patent CN107694610B discloses a solid-supported heteropolyacid phase transfer catalyst with H 2 O 2 As an oxidant, cyclohexanol is oxidized to cyclohexanone at 90°C and without solvent, and the conversion rate of cyclohexanol can reach 89.2%, and the selectivity of cyclohexanone can reach 95.4%, but the amount of substrate and product is small, which is not suitable for large-scale production. The Chinese patent application with publication number CN103071532A discloses a monovalent copper coordination polymer catalyst, the molecular formula of the coordination polymer is CuL, where L is 4,5-dicyanoimidazole, and air is used as an oxidant. The reaction is carried out at 80°C for 5h, and the complete conversion of cyclohexanol can be achieved, and the yield of cyclohexanone reaches 94.2%. However, the catalyst preparation process of this method is complicated, and it cannot be recycled, and the production cost is high.

[0007] In summary, from the perspective of industrial production practice, it is of great significance to develop a simple, efficient, economical and green production method for preparing cyclohexanone by selective oxidation of cyclohexanol with molecular oxygen. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art, especially to overcome the problems of weak catalyst activity and low catalytic efficiency, poor catalyst recyclability, high production cost, and serious pollution in the prior art, and to provide a method for preparing cyclohexanone by selective oxidation of cyclohexanol. The preparation method of the catalyst used is simple and convenient, the production cost is low, the catalytic activity is strong, the catalytic efficiency is high, the thermal stability is good, the recovery and recycling are convenient, and the catalyst is suitable for industrial production. The process of preparing cyclohexanone by selective oxidation of cyclohexanol does not add organic solvents and additives, the conversion rate of cyclohexanol is high, and the selectivity of cyclohexanone is high.

[0009] The technical solution adopted by the present invention to solve the technical problem is a method for preparing cyclohexanone by selective oxidation of cyclohexanol, which uses transition metal-modified graphite phase carbon nitride as a catalyst and oxygen or air as an oxidant to catalytically oxidize cyclohexanol to prepare cyclohexanone without adding any organic solvent or additive.

[0010] The preparation method of the transition metal-modified graphite phase carbon nitride catalyst comprises the following steps:

[0011] (1) Graphite phase carbon nitride (gC) was prepared by thermal polymerization 3 N 4 )Carrier:

[0012] Weigh a certain mass of graphite carbon nitride (gC 3 N 4 ) precursor, vacuum drying, grinding the precursor into a uniform powder (preferably using an agate mortar); heating the powdered precursor in a sealed, oxygen-free environment, calcining, cooling, and grinding to obtain graphite phase carbon nitride (gC 3 N 4 ) carrier;

[0013] (2) Prepare a transition metal solution with a certain molar concentration:

[0014] Weigh a certain mass of a soluble transition metal salt, add a solvent, and stir until the soluble transition metal salt is fully dissolved and the solution is evenly mixed to obtain a uniform transition metal mixed solution;

[0015] Furthermore, in step (2), the solvent is at least one of deionized water and anhydrous ethanol. The amount of the solvent used is sufficient to dissolve the soluble transition metal salt.

[0016] Furthermore, in step (2), the stirring speed is 500-800RPM.

[0017] Furthermore, in step (2), the stirring time is more than 4 hours, more preferably 8-10 hours.

[0018] (3) Preparation of transition metal modified graphite phase carbon nitride catalyst by impregnation method:

[0019] Add a certain mass of graphite phase carbon nitride (gC nitride) obtained in step (1) to the uniform transition metal mixed solution obtained in step (2). 3 N 4 ) carrier (the ratio of the two is determined by x), continue to stir evenly, then keep stirring and heating, evaporate the solvent during the stirring process to obtain a fully impregnated and uniform catalyst solid, then dry it, and grind the obtained solid to obtain a transition metal modified graphite phase carbon nitride (x% M / gC 3 N 4 , where x% is the mass fraction of the transition metal in the total mass of the catalyst, and M is the type of transition metal) catalyst.

[0020] Furthermore, in step (3), the stirring speed is 500-800RPM.

[0021] Further, the first stirring time in step (3) needs to ensure that the metal in the solution is fully in contact with the carrier, and the general stirring time is more than 4 hours (preferably 8-10 hours). The second stirring time during the stirring state and heating needs to ensure that the solvent (water and ethanol) in the solution is gradually evaporated, and generally requires stirring for 1-2 hours. No reaction occurs in these two stirrings, and the solution does not change significantly in the first stirring in step (3), which is generally a mixed color of the color of the metal solution plus the color of the carrier; the solvent in the solution gradually evaporates in the second stirring, and the color does not change or is slightly darker; if the stirring time of these two stirrings in step (3) is not enough, it will affect the catalytic effect of the catalyst.

[0022] Further, in the above-mentioned preparation method, in step (1), weigh gC 3 N 4 Precursor, vacuum drying is vacuum drying at 100-120°C for 8-10h.

[0023] Further, in the above-mentioned preparation method, in step (1), gC 3 N 4 The precursor may be at least one of melamine, dicyandiamide, urea, and thiourea. The heating rate may be 5-20° C. / min. The calcination temperature may be 400-700° C. The calcination time may be 3-7 hours.

[0024] Furthermore, in the above-mentioned preparation method, in step (1), the powdered precursor is heated in a sealed and oxygen-free environment, calcined, cooled, and then ground to obtain gC 3 N 4 The carrier can be operated as follows: put the powdered precursor into a crucible with a lid, and wrap the crucible tightly with tin foil to ensure that no oxygen enters the crucible during the thermal polymerization process; put the sealed crucible into a muffle furnace, heat it, calcine it, and grind it after cooling to obtain graphite phase carbon nitride (gC 3 N 4 ) carrier. In this step, the carrier must be fired in an oxygen-free environment because oxygen will 3 N 4 Support oxidation to CO 2 and NO X If oxygen enters the gas, all the carriers will be consumed.

[0025] Furthermore, in the above-mentioned preparation method, in step (2), the transition metal can be at least one of common transition metals such as vanadium, manganese, iron, cobalt, copper, zinc, nickel, etc.

[0026] Furthermore, in the above-mentioned preparation method, in step (3), the heating temperature for evaporating the solvent can be 100-200°C. The final prepared x%M / gC3 N 4 Catalyst, x% can be 0.1%-20% (x% is preferably 0.5-5%, more preferably 1%). Too large or too small x will result in insufficient catalytic performance of the catalyst, resulting in reduced raw material conversion rate and product selectivity.

[0027] Furthermore, in the above-mentioned preparation method, in step (3), the catalyst solid is dried at 100-120° C. for 4-8 hours.

[0028] The method for preparing cyclohexanone by selective oxidation of cyclohexanol of the present invention comprises the following steps:

[0029] Weigh a certain mass of catalyst and cyclohexanol, in an oxygen or air atmosphere, start stirring and heat to a certain temperature, then make the reactor reach a certain pressure to start the reaction; after a period of reaction, the reaction ends.

[0030] Collect product analysis: After the reaction is completed, cool to room temperature and exhaust the gas. Use anhydrous ethanol to collect and dilute the reaction solution. Then add internal standard chlorobenzene and perform quantitative analysis using the internal standard method in a gas chromatograph.

[0031] The x%M / gC of the present invention 3 N 4 Catalyst, preferably 1% V / gC 3 N 4 catalyst.

[0032] The amount of the catalyst used in the present invention is 1%-5% of the mass of the cyclohexanol raw material, preferably 3%. Too high or too low an amount of the catalyst will reduce the conversion rate and selectivity.

[0033] The reaction temperature of the present invention is 80-180° C., preferably 120° C. If the reaction temperature is too low, the conversion rate and selectivity will decrease; if the reaction temperature is too high, the conversion rate will increase and the selectivity will decrease.

[0034] The reaction pressure of the present invention is controlled at 0.1-2.0 MPa, preferably 0.7 MPa. If the reaction pressure is too low, the conversion rate and selectivity will be low; if the reaction pressure is too high, the conversion rate will increase and the selectivity will decrease.

[0035] The reaction time of the present invention is 2-16 hours, preferably 8 hours. If the reaction time is too short, the conversion rate and selectivity will be low; if the reaction pressure is too long, the conversion rate will increase and the selectivity will decrease.

[0036] Furthermore, after the reaction is completed, the catalyst can be recovered and reused after filtering, washing and drying. Furthermore, the catalyst is washed with anhydrous ethanol and deionized water.

[0037] Under the best reaction conditions, even with 1% V / gC 3 N 4 As a catalyst, the catalyst dosage is 3% of the raw material mass. The reaction is carried out at 120°C and 0.7MPa oxygen is continuously introduced for 8 hours. The conversion rate of cyclohexanol can reach up to 82.7%, and the selectivity of cyclohexanone can reach up to 93.7%. After the reaction, the catalyst can be recovered and reused by simple filtration, washing and drying. The catalyst can still maintain strong catalytic activity after being recycled for more than 8 times.

[0038] Compared with the prior art, the present invention has the following advantages:

[0039] (1) The preparation method of the catalyst of the present invention is simple and convenient, with low production cost and suitable for industrial production. 3 N 4 The catalyst has the advantages of strong catalytic activity, high catalytic efficiency, good thermal stability, convenient recycling and very stable catalytic performance after being recycled for 8 times;

[0040] (2) The present invention uses oxygen or air as an oxidant, avoiding the use of oxidants such as hydrogen peroxide, nitric acid, chromium trioxide and potassium permanganate, which are difficult to prepare, flammable and explosive, harmful to the environment and expensive to produce. In addition, no other solvents and additives need to be added during the reaction process. The entire reaction system is simple, green and efficient, and is an environmentally friendly catalytic oxidation method.

[0041] The present invention provides a new method for preparing cyclohexanone by selective oxidation of cyclohexanol in industry, which has broad market prospects and potential practical application value. The present invention provides a method for preparing cyclohexanone by selective oxidation of cyclohexanol, that is, using transition metal-modified graphite phase carbon nitride as a catalyst, oxygen or air as an oxidant, and efficiently catalytically oxidizing cyclohexanol to prepare cyclohexanone without adding any organic solvent and additive. It can solve the problems of harsh reaction conditions, low conversion rate of raw materials and selectivity of products, long process route, high requirements for production equipment, high energy consumption and production cost, serious environmental pollution, etc. in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 1% V / gC is used in Example 1 of the present invention 3 N 4 The gas chromatogram of the reaction liquid after cyclohexanol is catalytically oxidized when the catalyst is used; the conversion rate of the raw materials and the selectivity of the products in the reaction can be calculated from the peak area data in the gas chromatogram;

[0043] Figure 2 is gC in Example 1 3 N 4 SEM (scanning electron microscope) image of the carrier;

[0044] Figure 3 1% V / gC in Example 1 3 N 4 SEM images of the catalyst;

[0045] Figure 4 1% V / gC in Example 40 3 N 4 SEM image of the catalyst after being recycled 8 times. DETAILED DESCRIPTION

[0046] The present invention is further described and illustrated in detail below in conjunction with the accompanying drawings and specific embodiments, but it should be understood that the embodiments of the present invention are not limited thereto.

[0047] In this specification, unless otherwise specified, all percentages are by mass.

[0048] Embodiment 1:

[0049] The method for preparing the vanadium-modified graphite-phase carbon nitride catalyst of this embodiment comprises the following steps:

[0050] (1) Graphite phase carbon nitride (gC) was prepared by thermal polymerization 3 N 4 )Carrier:

[0051] Weigh 10.0g of melamine and dry it in vacuum at 100℃ for 8h. After drying, grind the precursor into a uniform powder with an agate mortar. Put the powdered precursor into a crucible with a lid and wrap the crucible tightly with tin foil to ensure that no oxygen enters the crucible during the thermal polymerization. Put the sealed crucible into a muffle furnace, heat it to 600℃ at a rate of 10℃ / min, calcine it for 5h, and grind it after cooling to obtain light yellow gC 3 N 4 -MCN carrier.

[0052] (2) Prepare a vanadium-containing solution with a certain molar concentration:

[0053] Weigh 0.065 g of vanadyl sulfate and put it into a clean crucible, measure 30 mL of deionized water and 30 mL of anhydrous ethanol respectively, add the mixed solution with a volume ratio of 1:1 into the crucible, and stir rapidly at a stirring speed of 500 RPM for 8 h until the solute is fully dissolved and the solution is mixed evenly to obtain a uniform transition metal mixed solution;

[0054] (3) Preparation of vanadium-modified graphite phase carbon nitride catalyst by impregnation method:

[0055] Add 2.0 g of gC obtained in step (1) to the uniform mixed solution obtained in step (2).3 N 4 -MCN carrier, continue to stir rapidly at a stirring speed of 500RPM for 8h, then turn on the stirring table heating, raise the temperature to 180°C, evaporate the solvent during the stirring process at a stirring speed of 500RPM (stirring for 2 hours), obtain a fully impregnated and uniform catalyst solid, and then put it into an oven at 100°C for 8h. After the solid is fully ground, a light green powder can be obtained, that is, 1% V / gC 3 N 4 -MCN catalyst.

[0056] The transition metal-modified graphite phase carbon nitride catalyst in Example 1 is used in the reaction of catalytic oxidation of cyclohexanol to prepare cyclohexanone.

[0057] The reaction conditions are as follows: in a stainless steel autoclave reactor with a volume of 100 mL and equipped with a polytetrafluoroethylene liner, the mass of cyclohexanol is 10.0 g, the mass of the catalyst is 0.3 g, the reaction temperature is 120° C., 0.7 MPa of oxygen is continuously introduced, and the reaction time is 8 h. After the reaction is completed, the reaction solution is cooled to room temperature, anhydrous ethanol is used to collect and dilute the reaction solution, and then internal standard chlorobenzene is added, and quantitative analysis is performed using the internal standard method in a gas chromatograph to calculate the conversion rate of cyclohexanone and the selectivity of cyclohexanone.

[0058] Figure 1 1% V / gC is used in Example 1 of the present invention 3 N 4 The gas chromatogram of the reaction liquid after cyclohexanol is catalytically oxidized when the catalyst is present; the conversion rate of the raw materials and the selectivity of the products in the reaction can be calculated from the peak area data in the gas chromatogram.

[0059] Embodiment 2:

[0060] The method for preparing a manganese-modified graphite phase carbon nitride catalyst in this embodiment is different from that in embodiment 1: in step (2), when preparing a transition metal solution with a certain molar concentration, 0.065 g of vanadyl sulfate is replaced with 0.082 g of manganese sulfate tetrahydrate, and other conditions are the same as those in embodiment 1. The catalyst finally prepared is 1% Mn / gC 3 N 4 -MCN.

[0061] Embodiment 3:

[0062] A method for preparing an iron-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution of a certain molar concentration, 0.065 g of vanadyl sulfate is replaced with 0.203 g of ferric sulfate nonahydrate, and other conditions are the same as in Example 1. The catalyst finally prepared is 1% Fe / gC 3 N4 -MCN.

[0063] Embodiment 4:

[0064] A method for preparing a cobalt-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution with a certain molar concentration, 0.065 g of vanadium sulfate is replaced with 0.096 g of cobalt sulfate heptahydrate, and other conditions are the same as in Example 1. The catalyst finally prepared is 1% Co / gC 3 N 4 -MCN.

[0065] Embodiment 5:

[0066] A method for preparing a nickel-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution of a certain molar concentration, 0.065 g of vanadium sulfate is replaced by 0.091 g of nickel sulfate, and other conditions are the same as in Example 1. The catalyst finally prepared is 1% Ni / gC 3 N 4 -MCN.

[0067] Embodiment 6:

[0068] A method for preparing a copper-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution of a certain molar concentration, 0.065 g of vanadium sulfate is replaced with 0.079 g of copper sulfate pentahydrate, and other conditions are the same as in Example 1. The catalyst finally prepared is 1% Cu / gC 3 N 4 -MCN.

[0069] Embodiment 7:

[0070] A method for preparing a zinc-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution of a certain molar concentration, 0.065 g of vanadyl sulfate is replaced by 0.088 g of zinc sulfate heptahydrate, and other conditions are the same as in Example 1. The catalyst finally prepared is 1% Zn / gC 3 N 4 -MCN.

[0071] The graphite phase carbon nitride catalysts modified with different transition metals in Examples 1 to 7 were used in the reaction of catalytic oxidation of cyclohexanol to prepare cyclohexanone.

[0072] The reaction conditions are as follows: in a stainless steel autoclave reactor with a volume of 100 mL and equipped with a polytetrafluoroethylene liner, the mass of cyclohexanol is 10.0 g, the mass of the catalyst is 0.3 g, the reaction temperature is 120° C., 0.7 MPa of oxygen is continuously introduced, and the reaction time is 8 h. After the reaction is completed, the reaction solution is cooled to room temperature, anhydrous ethanol is used to collect and dilute the reaction solution, and then internal standard chlorobenzene is added, and quantitative analysis is performed using the internal standard method in a gas chromatograph to calculate the conversion rate of cyclohexanone and the selectivity of cyclohexanone.

[0073] The experimental results of Examples 1 to 7 are shown in Table 1.

[0074] Table 1: Effects of different transition metal modified catalysts on the catalytic oxidation of cyclohexanol

[0075]

[0076] Embodiment 8:

[0077] A method for preparing a vanadium-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution of a certain molar concentration, the amount of vanadium oxysulfate is replaced from 0.065 g to 0.006 g, and the other conditions are the same as those in Example 1. The catalyst finally prepared is 0.1% V / gC 3 N 4 -MCN.

[0078] Embodiment 9:

[0079] A method for preparing a vanadium-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution of a certain molar concentration, the amount of vanadium oxysulfate is replaced from 0.065 g to 0.033 g, and the other conditions are the same as those in Example 1. The catalyst finally prepared is 0.5% V / gC 3 N 4 -MCN.

[0080] Embodiment 10:

[0081] A method for preparing a vanadium-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution of a certain molar concentration, the amount of vanadium oxysulfate is replaced from 0.065 g to 0.131 g, and the other conditions are the same as those in Example 1. The catalyst finally prepared is 2% V / gC 3 N 4 -MCN.

[0082] Embodiment 11:

[0083] A method for preparing a vanadium-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution of a certain molar concentration, the amount of vanadium oxysulfate is replaced from 0.065 g to 0.198 g, and the other conditions are the same as those in Example 1. The catalyst finally prepared is 3% V / gC 3 N 4 -MCN.

[0084] Embodiment 12:

[0085] A method for preparing a vanadium-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution of a certain molar concentration, the amount of vanadium oxysulfate is replaced from 0.065 g to 0.337 g, and the other conditions are the same as those in Example 1. The catalyst finally prepared is 5% V / gC 3 N 4 -MCN.

[0086] Embodiment 13:

[0087] A method for preparing a vanadium-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution with a certain molar concentration, the amount of vanadium oxysulfate is replaced from 0.065 g to 0.711 g, and the other conditions are the same as those in Example 1. The catalyst finally prepared is 10% V / gC 3 N 4 -MCN.

[0088] Embodiment 14:

[0089] A method for preparing a vanadium-modified graphite phase carbon nitride catalyst, which differs from Example 1 in that in step (2), when preparing a transition metal solution of a certain molar concentration, the amount of vanadium oxysulfate is replaced from 0.065 g to 1.601 g, and the other conditions are the same as those in Example 1. The catalyst finally prepared is 20% V / gC 3 N 4 -MCN.

[0090] The 0.1% V / gC in Examples 8 to 14 3 N 4 -MCN, 0.5% V / gC 3 N 4 -MCN, 2% V / gC 3 N 4 -MCN, 3% V / gC 3 N 4 -MCN, 5% V / gC 3 N 4 -MCN, 10% V / gC3 N 4 -MCN, 20% V / gC 3 N 4 -MCN catalyst is used in the catalytic oxidation reaction of cyclohexanol to prepare cyclohexanone, and the reaction conditions are the same as those in Example 1.

[0091] The experimental results of Examples 8 to 14 compared with Example 1 are shown in Table 2.

[0092] Table 2: Effect of vanadium loading on catalytic oxidation of cyclohexanol

[0093]

[0094] Embodiment 15:

[0095] The difference from Example 1 is that the gC 3 N 4 The precursor melamine of the carrier is replaced by dicyandiamide, and other conditions are the same as those in Example 1 to obtain gC 3 N 4 -DCN carrier, the final prepared catalyst is 1% V / gC 3 N 4 -DCN.

[0096] Embodiment 16:

[0097] The difference from Example 1 is that the gC 3 N 4 The precursor melamine of the carrier is replaced by urea, and other conditions are the same as those in Example 1 to obtain gC 3 N 4 -UCN carrier, the final prepared catalyst is 1% V / gC 3 N 4 -UCN.

[0098] Embodiment 17:

[0099] The difference from Example 1 is that the gC 3 N 4 The precursor melamine of the carrier is replaced by thiourea, and the other conditions are the same as those in Example 1 to obtain gC 3 N 4 -TCN carrier, the final prepared catalyst is 1% V / gC 3 N 4 -TCN.

[0100] The 1% V / gC in Examples 15 to 17 3 N 4-DCN, 1% V / gC 3 N 4 -UCN, 1% V / gC 3 N 4 -TCN catalyst is used in the catalytic oxidation reaction of cyclohexanol to prepare cyclohexanone, and the reaction conditions are the same as those in Example 1.

[0101] The experimental results of Examples 15 to 17 compared with Example 1 are shown in Table 3.

[0102] Table 3: Effects of different carrier precursors on the catalytic oxidation of cyclohexanol

[0103]

[0104] Embodiment 18:

[0105] The difference from Example 1 is that the 1% V / gC in Example 1 3 N 4 -MCN catalyst was calcined at 300℃ in an oxygen-free environment for 4h, and the final prepared catalyst was 1% V / gC 3 N 4 -MCN-300℃.

[0106] Embodiment 19:

[0107] The difference from Example 1 is that the 1% V / gC in Example 1 3 N 4 -MCN catalyst was calcined at 400℃ in an oxygen-free environment for 4h, and the final prepared catalyst was 1% V / gC 3 N 4 -MCN-400℃.

[0108] Embodiment 20:

[0109] The difference from Example 1 is that the 1% V / gC in Example 1 3 N 4 -MCN catalyst was calcined at 500℃ in an oxygen-free environment for 4h, and the final prepared catalyst was 1% V / gC 3 N 4 -MCN-500℃.

[0110] Embodiment 21:

[0111] The difference from Example 1 is that the 1% V / gC in Example 1 3 N 4 -MCN catalyst was calcined at 600℃ in an oxygen-free environment for 4h, and the final prepared catalyst was 1% V / gC 3 N 4-MCN-600℃.

[0112] The 1% V / gC in Examples 18 to 21 3 N 4 -MCN-300℃, 1% V / gC 3 N 4 -MCN-400℃, 1%V / gC 3 N 4 -MCN-500℃, 1% V / gC 3 N 4 -MCN-600°C, the catalyst is used in the catalytic oxidation reaction of cyclohexanol to prepare cyclohexanone, and the reaction conditions are the same as those in Example 1.

[0113] The experimental results of Examples 18 to 21 compared with Example 1 are shown in Table 4.

[0114] Table 4: Effect of catalyst calcination temperature on catalytic oxidation of cyclohexanol

[0115]

[0116]

[0117] Embodiment 22:

[0118] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst is used for the catalytic oxidation of cyclohexanol to prepare cyclohexanone, the oxidant is changed to air, and the other reaction conditions are the same as those in Example 1.

[0119] The experimental results of Example 22 compared with Example 1 are shown in Table 5.

[0120] Table 5: Effect of oxidants on catalytic oxidation of cyclohexanol

[0121]

[0122] Embodiment 23:

[0123] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst was used in the reaction of catalytic oxidation of cyclohexanol to prepare cyclohexanone. The amount of catalyst was changed to 0.1 g, and the other reaction conditions were the same as those in Example 1.

[0124] Embodiment 24:

[0125] Using the 1% V / gC in Example 1 3 N 4-MCN catalyst was used in the reaction of catalytic oxidation of cyclohexanol to prepare cyclohexanone. The amount of catalyst was changed to 0.2 g, and the other reaction conditions were the same as those in Example 1.

[0126] Embodiment 25:

[0127] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst was used in the reaction of catalytic oxidation of cyclohexanol to prepare cyclohexanone. The amount of catalyst was changed to 0.4 g, and the other reaction conditions were the same as those in Example 1.

[0128] Embodiment 26:

[0129] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst was used in the reaction of catalytic oxidation of cyclohexanol to prepare cyclohexanone. The amount of catalyst was changed to 0.5 g, and the other reaction conditions were the same as those in Example 1.

[0130] The experimental results of Examples 23 to 26 compared with Example 1 are shown in Table 6.

[0131] Table 6: Effect of catalyst dosage on catalytic oxidation of cyclohexanol

[0132]

[0133] Embodiment 27:

[0134] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst is used in the reaction of catalytic oxidation of cyclohexanol to prepare cyclohexanone, the reaction temperature is changed to 100°C, and the other reaction conditions are the same as those in Example 1.

[0135] Embodiment 28:

[0136] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst is used in the reaction of catalytic oxidation of cyclohexanol to prepare cyclohexanone, the reaction temperature is changed to 110°C, and the other reaction conditions are the same as those in Example 1.

[0137] Embodiment 29:

[0138] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst is used in the catalytic oxidation reaction of cyclohexanol to prepare cyclohexanone. The reaction temperature is changed to 130°C, and the other reaction conditions are the same as those in Example 1.

[0139] Embodiment 30:

[0140] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst is used in the catalytic oxidation reaction of cyclohexanol to prepare cyclohexanone. The reaction temperature is changed to 140°C, and the other reaction conditions are the same as those in Example 1.

[0141] The experimental results of Examples 27 to 30 compared with Example 1 are shown in Table 7.

[0142] Table 7: Effect of reaction temperature on catalytic oxidation of cyclohexanol

[0143]

[0144] Embodiment 31:

[0145] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst is used for the catalytic oxidation of cyclohexanol to prepare cyclohexanone. The reaction pressure is controlled at 0.3 MPa. Other reaction conditions are the same as those in Example 1.

[0146] Embodiment 32:

[0147] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst is used for the catalytic oxidation of cyclohexanol to prepare cyclohexanone. The reaction pressure is controlled at 0.5 MPa. Other reaction conditions are the same as those in Example 1.

[0148] Embodiment 33:

[0149] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst is used for the catalytic oxidation of cyclohexanol to prepare cyclohexanone. The reaction pressure is controlled at 0.9 MPa. Other reaction conditions are the same as those in Example 1.

[0150] Embodiment 34:

[0151] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst is used for catalytic oxidation of cyclohexanol to prepare cyclohexanone. The reaction pressure is controlled at 1.1 MPa. Other reaction conditions are the same as those in Example 1.

[0152] The experimental results of Examples 31 to 34 compared with Example 1 are shown in Table 8.

[0153] Table 8: Effect of reaction pressure on catalytic oxidation of cyclohexanol

[0154]

[0155] Embodiment 35:

[0156] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst was used for the catalytic oxidation of cyclohexanol to prepare cyclohexanone. The reaction time was changed to 2 h. Other reaction conditions were the same as those in Example 1.

[0157] Embodiment 36:

[0158] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst was used for the catalytic oxidation of cyclohexanol to prepare cyclohexanone. The reaction time was changed to 4 h. Other reaction conditions were the same as those in Example 1.

[0159] Embodiment 37:

[0160] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst was used for the catalytic oxidation of cyclohexanol to prepare cyclohexanone. The reaction time was changed to 6 h. Other reaction conditions were the same as those in Example 1.

[0161] Embodiment 38:

[0162] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst was used for the catalytic oxidation of cyclohexanol to prepare cyclohexanone. The reaction time was changed to 10 h. Other reaction conditions were the same as those in Example 1.

[0163] Embodiment 39:

[0164] Using the 1% V / gC in Example 1 3 N 4 -MCN catalyst was used for the catalytic oxidation of cyclohexanol to prepare cyclohexanone. The reaction time was changed to 12 h. Other reaction conditions were the same as those in Example 1.

[0165] The experimental results of Examples 35 to 39 compared with Example 1 are shown in Table 9.

[0166] Table 9: Effect of reaction time on catalytic oxidation of cyclohexanol

[0167]

[0168]

[0169] Embodiment 40:

[0170] 1% V / gC after the reaction in Example 1 is recycled 3 N 4 -MCN catalyst steps are as follows: first, the catalyst in the reaction solution can be recovered by filtering, and then the catalyst is washed more than 3 times with anhydrous ethanol and deionized water respectively, and finally after vacuum drying at 100 ° C and 8 hours, the catalyst for recycling can be obtained, and the recovery rate of each cycle can reach about 90%.

[0171] The catalyst recycled 1 to 8 times was used to catalyze the oxidation of cyclohexanone to prepare cyclohexanone. The reaction conditions were the same as those in Example 1. The experimental results are shown in Table 10.

[0172] Table 10: 1% V / gC 3 N 4 -The recycling effect of MCN catalyst

[0173]

[0174] From Table 10, we can see that 1% V / gC 3 N 4 -MCN catalyst can still maintain strong catalytic activity after being recycled 8 times, and its catalytic performance is very stable.

[0175] Scanning electron microscope (SEM) is a large precision instrument used for high-resolution morphological analysis. It is widely used to observe the morphology and composition of the surface ultrastructure of various solid substances.

[0176] Figure 2 is a SEM image of the g-C3N4 carrier in Example 1, Figure 3 is a SEM image of the 1% V / g-C3N4 catalyst in Example 1; Figure 4 This is the SEM image of the 1% V / g-C3N4 catalyst in Example 40 after being recycled 8 times.

[0177] from Figure 2-4 It can be seen that the external morphology of these three solids is Tremella nanosheets; Figure 2 It can be seen that the g-C3N4 carrier fired by thermal polymerization in Example 1 conforms to its two-dimensional layered structure similar to graphite, which is the same as described in the literature, indicating that the preparation method of the catalyst is feasible; Figure 3 It can be seen that the external morphology of the catalyst modified by metal V is not much different from that of the pure g-C3N4 carrier, indicating that metal modification will not affect the porous structure of the catalyst; Figure 4 It can be seen that the external morphology of the catalyst did not change significantly after being recycled 8 times, indicating that the catalytic performance and physical structure of the catalyst are very stable.

[0178] The applicant declares that the above descriptions are only some specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any improvement and transformation that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention is within the protection scope of the present invention.

Claims

1. A method for preparing cyclohexanone by selective oxidation of cyclohexanol, characterized in that: Graphite phase carbon nitride modified by transition metal is used as catalyst and oxygen or air is used as oxidant to catalytically oxidize cyclohexanol to prepare cyclohexanone.

2. The method for preparing cyclohexanone by selective oxidation of cyclohexanol according to claim 1, characterized in that: The preparation method of the transition metal modified graphite phase carbon nitride catalyst comprises the following steps: (1) Firing of graphite phase carbon nitride carrier by thermal polymerization: Weigh a certain mass of graphite phase carbon nitride precursor, vacuum dry it, and grind the precursor into uniform powder after drying; heat the powdered precursor in a sealed and oxygen-free environment, calcine it, and grind it after cooling to obtain a graphite phase carbon nitride carrier; (2) Prepare a transition metal solution with a certain molar concentration: Weigh a certain mass of a soluble transition metal salt, add a solvent, and stir until the soluble transition metal salt is fully dissolved and the solution is evenly mixed to obtain a uniform transition metal mixed solution; (3) Preparation of transition metal modified graphite phase carbon nitride catalyst by impregnation method: A certain mass of the graphite phase carbon nitride carrier obtained in step (1) is added to the uniform transition metal mixed solution obtained in step (2), and the mixture is stirred evenly. The mixture is then heated while being stirred. During the stirring process, the solvent is evaporated to obtain a fully impregnated and uniform catalyst solid. The solid is then dried and fully ground to obtain a transition metal-modified graphite phase carbon nitride catalyst.

3. The method for preparing cyclohexanone by selective oxidation of cyclohexanol according to claim 2, characterized in that: In the preparation method of the transition metal modified graphite phase carbon nitride catalyst, in step (1), a g-C3N4 precursor is weighed and vacuum dried at 100-120°C for 8-10 h; and / or, in step (1), the g-C3N4 precursor is at least one of melamine, dicyandiamide, urea, and thiourea; and / or in step (1), the heating rate is 5-20°C / min; and / or in step (1), the calcination temperature is 400-700°C; and / or in step (1), the calcination time is 3-7 h.

4. The method for preparing cyclohexanone by selective oxidation of cyclohexanol according to claim 2 or 3, characterized in that: In the preparation method of the transition metal-modified graphite phase carbon nitride catalyst, in step (2), the transition metal is at least one of vanadium, manganese, iron, cobalt, copper, zinc, and nickel; and / or in step (2), the solvent is at least one of deionized water and anhydrous ethanol; and / or in step (2), the stirring speed is 500-800 RPM; and / or in step (2), the stirring time is more than 4 hours.

5. The method for preparing cyclohexanone by selective oxidation of cyclohexanol according to claim 2 or 3, characterized in that: In the preparation method of the transition metal modified graphite phase carbon nitride catalyst, in step (3), the heating temperature for evaporating the solvent is 100-200°C; and / or in step (3), the stirring speed is 500-800 RPM; and / or in step (3), the first stirring time is more than 4 hours; and / or the second stirring time during the stirring state and heating is 1-2 hours; and / or in step (3), the catalyst solid is dried at 100-120°C for 4-8 hours.

6. The method for preparing cyclohexanone by selective oxidation of cyclohexanol according to claim 2 or 3, characterized in that: In the preparation method of the transition metal modified graphite phase carbon nitride catalyst, the x% M / g-C3N4 catalyst is finally prepared, wherein x% is the mass fraction of the transition metal in the total mass of the catalyst, M is the type of transition metal, and x% is 0.1%-20%.

7. The method for preparing cyclohexanone by selective oxidation of cyclohexanol according to any one of claims 1 to 6, characterized in that: The following steps are involved: Weigh a certain mass of catalyst and cyclohexanol, in an oxygen or air atmosphere, start stirring and heat to a certain temperature, then make the reactor reach a certain pressure to start the reaction; after a period of reaction, the reaction ends.

8. The method for preparing cyclohexanone by selective oxidation of cyclohexanol according to any one of claims 1 to 7, characterized in that: The amount of catalyst used is 1%-5% of the mass of cyclohexanol raw material.

9. The method for preparing cyclohexanone by selective oxidation of cyclohexanol according to any one of claims 1 to 8, characterized in that: The reaction temperature is 80-180°C; and / or the reaction pressure is controlled at 0.1-2.0 MPa; and / or the reaction time is 2-16 h.

10. The method for preparing cyclohexanone by selective oxidation of cyclohexanol according to any one of claims 1 to 9, characterized in that: After the reaction is completed, the catalyst can be recovered and reused after filtering, washing and drying.