Novel conjugated microporous polymer as well as preparation method and application thereof

The conjugated microporous polymer synthesized through Schiff base condensation reaction uses high specific surface area and porous structure to improve the electrochemical performance of the negative electrode material of lithium-ion battery, solving the limitations of traditional materials in energy density and cycle stability, and achieving the goal of achieving High specific capacity and good rate performance.

CN118994512AActive Publication Date: 2024-11-22HUNAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411327650.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-22
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

Traditional lithium-ion battery negative electrode materials have limitations in terms of energy density and charge and discharge speed. Small molecule organic electrode materials and linear conjugated polymers have unstable cycle life due to high solubility and π-π stacking, and low electron conductivity, which is limited. Its rate performance is achieved.

Method used

Benzo[1,2-b:3,4-b':5,6-b']trithiophene-2,5,8-trialdehyde and dithiooxalamide were used to convert Schiff base Synthesize a new conjugated microporous polymer for raw materials with high specific surface area and porous structure. As the negative electrode material of lithium-ion batteries, it is optimized by constructing a conjugated thiophene bridge and introducing thiazole[5,4-d]thiazole ring structure. Electronic structure and pore structure.

Benefits of technology

It significantly improves electrochemical performance, provides high specific capacity, good rate performance and excellent cycle stability, extends the structural integrity and cycle life of the electrode material, and avoids capacity attenuation problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994512A_ABST
    Figure CN118994512A_ABST
Patent Text Reader

Abstract

The invention discloses a novel conjugated microporous polymer as well as a preparation method and application thereof. According to the invention, benzo [1, 2-b: 3, 4-b ': 5, 6-b'] trithiophene-2, 5, 8-trialdehyde and dithio oxamide are used as raw materials, and a reversible Schiff base condensation reaction is adopted to synthesize the novel conjugated microporous polymer. The invention also provides an application of the novel conjugated microporous polymer in a lithium ion battery negative electrode material. The prepared novel conjugated microporous polymer has a high specific surface area and a porous structure, is beneficial to electron transfer and ion transmission as a lithium ion battery negative electrode material, shows excellent electrochemical performance, and has a relatively good application prospect in the field of lithium ion battery negative electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of negative electrode materials for lithium ion batteries, and in particular to a novel conjugated microporous polymer and a preparation method and application thereof. Background Art

[0002] With the rapid development of portable electronic devices and electric vehicles, electrochemical energy storage devices have become one of the hottest research areas. Among them, lithium-ion batteries (LIBs) have attracted much attention due to their significant advantages such as high energy density, high power density, long cycle life and low self-discharge rate. However, with the continuous growth of market demand and the continuous advancement of technology, the requirements for the performance of lithium-ion batteries are also increasing. Although traditional lithium-ion battery anode materials such as graphite have stable performance and relatively low cost, they have great limitations in energy density and charge and discharge speed. Therefore, the development of a new high-performance anode material has become a hot topic in lithium-ion battery research.

[0003] Organic electrode materials have attracted extensive attention due to their structural tunability, resource sustainability, environmental friendliness and renewability. However, small molecule organic electrode materials and linear polymers have high solubility in organic electrolytes, which may lead to rapid capacity decay, and the occurrence of side reactions will lead to low coulombic efficiency and poor cycle life. Traditional linear conjugated polymers have dense molecular chains due to π-π stacking, which limits the contact with the electrolyte, thus affecting the redox activity. In addition, during long-term cycles, the electrode materials may undergo structural degradation, which in turn affects the cycle stability. In addition, the electronic conductivity of organic electrode materials is low, which limits their rate performance. Conjugated microporous polymers (CMPs), as a new type of organic porous material, show significant advantages in lithium-ion battery negative electrode materials due to their high specific surface area, porous structure and excellent physicochemical stability. The high specific surface area helps to expose more redox reaction active sites, thereby improving the specific capacity; the porous structure helps the penetration of the electrolyte, shortens the lithium ion transmission path, thereby improving the reaction kinetics; and the excellent stability ensures the performance stability during the cycle.

[0004] Therefore, the development of conjugated microporous polymers that are easy to synthesize and have high specific capacity, high rate performance and excellent cycle stability has become a new research direction for organic negative electrode materials for lithium-ion batteries. Summary of the invention

[0005] In order to solve the technical problems existing in the above-mentioned prior art, the present invention provides a novel conjugated microporous polymer and its preparation method and application. The present invention uses benzo[1,2-b:3,4-b':5,6-b']trithiophene-2,5,8-trialdehyde and dithiooxamide as raw materials, and adopts a reversible Schiff base condensation reaction to synthesize the novel conjugated microporous polymer. The novel conjugated microporous polymer prepared by the present invention has a high specific surface area and a porous structure. As a negative electrode material for lithium-ion batteries, it is conducive to electron transfer and ion transport, exhibits excellent electrochemical properties, and has good application prospects in the field of negative electrode materials for lithium-ion batteries.

[0006] To achieve the above object, the present invention provides a novel conjugated microporous polymer having a structural formula as shown in formula (I):

[0007] The present invention also provides a method for preparing the novel conjugated microporous polymer, comprising the following steps:

[0008] (1) Under the protection of inert gas, benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and dithiooxamide are added to an organic solvent, and heated and stirred for reaction;

[0009] (2) After the reaction is completed, washing, filtering and drying are performed to obtain the novel conjugated microporous polymer.

[0010] Furthermore, in step (1), the molar ratio of the benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde to dithiooxamide is 1:1-5.

[0011] Furthermore, the organic solvent is N,N-dimethylformamide or N-methylpyrrolidone.

[0012] Furthermore, the heating reaction is carried out under stirring at 100-200° C. for 24-120 hours.

[0013] Furthermore, the inert gas is nitrogen or argon.

[0014] Furthermore, after the reaction is completed, the reaction solution is poured into deionized water and stirred and slurried, and then the mixed solution is filtered, and the filter residue is washed with dichloromethane, ethanol and water respectively, and vacuum dried at 80-150° C. to obtain the novel conjugated microporous polymer.

[0015] The present invention also provides application of the novel conjugated microporous polymer in negative electrode materials of lithium ion batteries.

[0016] Furthermore, the above-mentioned new type of conjugated microporous polymer is used as an active material, mixed evenly with a conductive agent and a binder in a solvent to form a slurry, and the slurry is evenly coated on a copper foil. After vacuum drying, it is cut into electrodes to be used with a cutting machine; the electrode is assembled into a button battery in an argon-protected glove box with a lithium sheet as a negative electrode, a diaphragm, and an electrolyte.

[0017] Furthermore, the conductive agent is at least one of acetylene black, Ketjen black, conductive carbon black and carbon nanotubes, the binder is at least one of polyvinylidene fluoride, styrene-butadiene rubber, sodium alginate, carboxymethyl cellulose, polyvinyl alcohol, polyacrylic acid and polyacrylonitrile, and the solvent is at least one of N-methylpyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide, diethyl ether, ethyl acetate, N-butylpyrrolidone and deionized water.

[0018] Specifically, the preparation of the pole piece includes the following steps: First, the pre-prepared BTSZ is used as the active material, the conductive carbon black is used as the conductive agent, and the polyvinylidene fluoride is used as the binder. The active material, the conductive agent, and the binder are mixed in a mass ratio of 6:3:1, and an appropriate amount of N-methylpyrrolidone is added and ground to form a uniform slurry. Use a scraper to evenly apply the slurry on the surface of the copper foil and vacuum dry it at 80°C for 12 hours. After drying, use a mold to punch it into a disc with a diameter of 10 mm to obtain the pole piece.

[0019] The assembly of the battery includes the following steps: using the prepared electrode as the positive electrode, the metal lithium sheet as the negative electrode, 1MLiClO4 ethylene carbonate (EC): diethyl carbonate (DEC) = 1:1 (v / v) solution as the electrolyte solution, and a polypropylene microporous membrane (Celgard 2500) as the separator to assemble into a CR2032 button battery.

[0020] The present invention has the following beneficial effects:

[0021] (1) The present invention constructs a conjugated microporous polymer material (BTSZ) with large specific surface area, good chemical stability and excellent thermal stability through reasonable molecular structure design. Specifically, a new type of conjugated microporous polymer is synthesized by reversible Schiff base condensation reaction using benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and dithiooxamide as raw materials. The conjugated microporous polymer material is in the form of spherical particles with a specific surface area of ​​279.4 m 2 g -1The average pore size distribution is about 0.79nm. As a negative electrode material for lithium-ion batteries, its high specific surface area helps to fully infiltrate the electrolyte, thereby exposing more active sites for more effective redox reactions; and the structural characteristics of the high specific surface area and porous structure of the new conjugated microporous polymer are conducive to electron transfer and ion transport, making it exhibit excellent electrochemical properties, and has good application prospects in the field of negative electrode materials for lithium-ion batteries.

[0022] (2) The present invention uses benzo[1,2-b:3,4-b':5,6-b']trithiophene-2,5,8-trialdehyde and dithiooxamide as raw materials and adopts a reversible Schiff base condensation reaction to synthesize a new type of conjugated microporous polymer. The conjugated microporous polymer material extends the conjugated structure of thiophene and constructs a conjugated thiophene bridge, in which three thiophene units are fused at the boundary of the benzene ring, resulting in a dihedral angle between adjacent thiophenes that is almost zero, which helps to achieve superior π electron delocalization and thus improve conductivity. The present invention introduces a thiazolyl[5,4-d]thiazole ring structure, which can be used as an electron acceptor unit. Combined with the conjugated thiophene bridge structure as an electron donor, an effective electron donor-acceptor system can be formed, which can significantly improve its conductivity. At the same time, the thiazolyl[5,4-d]thiazole ring structure can optimize the pore structure of the conjugated microporous polymer and promote ion transport. The present invention optimizes the electronic structure of the conjugated microporous polymer by introducing heteroatoms such as N and S, thereby improving its conductivity, and at the same time, the C=N double bond in the molecular structure enhances the molecular stability. The conjugated microporous polymer material of the present invention improves the intrinsic conductivity and structural stability of the material by extending the thiophene conjugated structure to construct a conjugated thiophene bridge and introducing a thiazolyl[5,4-d]thiazole ring structure, thereby showing excellent electrochemical properties and having good application prospects in the field of negative electrode materials for lithium ion batteries.

[0023] (3) The present invention synthesizes conjugated microporous polymers with high specific surface area and abundant active sites through molecular design, which can enhance the structural integrity and cycle life of electrode materials. At the same time, by designing conjugated microporous polymers with cross-linked porous skeletons, their chemical stability in electrolytes can be significantly enhanced, avoiding the problem of rapid capacity decay caused by the high solubility of organic small molecules and linear polymers in organic electrolytes. The new conjugated microporous polymer BTSZ prepared by the present invention is used as a negative electrode material for lithium-ion batteries, which has high specific capacity, good rate performance and excellent cycle stability. When the current density is increased from 0.1Ag -1 Increase to 2Ag -1 When BTSZ has a peak value of 1016, 742, 533, 409 and 302 mAh g -1 High reversible specific capacity; when the current density is restored to 0.1A -1 When the BTSZ electrode is used, it can recover to 982 mAh g -1The reversible specific capacity has excellent rate performance; at 0.2Ag -1 After 1000 cycles at a current density of 1.34 Å, BTSZ can still maintain 820 mAh g -1 It has high reversible specific capacity and excellent electrochemical cycle stability.

[0024] In addition to the above objects, features and advantages, the present invention has other objects, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0026] Figure 1 The structural formula and synthetic route of the conjugated microporous polymer BTSZ are shown below;

[0027] Figure 2 is a Fourier transform infrared spectrum of the conjugated microporous polymer BTSZ prepared in Example 2;

[0028] Figure 3 The conjugated microporous polymer BTSZ prepared in Example 2 13 C solid NMR spectrum;

[0029] Figure 4 is a thermogravimetric curve of the conjugated microporous polymer BTSZ prepared in Example 2 under a nitrogen atmosphere;

[0030] Figure 5 is a scanning electron microscope image of the conjugated microporous polymer BTSZ prepared in Example 2;

[0031] Figure 6 is the nitrogen adsorption-desorption curve of the conjugated microporous polymer BTSZ prepared in Example 2;

[0032] Figure 7 is the pore size distribution diagram of the conjugated microporous polymer BTSZ prepared in Example 2;

[0033] Figure 8 This is a rate performance diagram of the conjugated microporous polymer BTSZ used as a negative electrode material for lithium-ion batteries in the application example;

[0034] Fig. 9 The charge and discharge curves of the conjugated microporous polymer BTSZ used as the negative electrode material of the lithium ion battery in the application example;

[0035] Fig.10This is a graph showing the cycling performance of the conjugated microporous polymer BTSZ as a negative electrode material for lithium-ion batteries in an application example. DETAILED DESCRIPTION

[0036] Below in conjunction with the accompanying drawings in the embodiments of the present invention, the technical scheme in the embodiments of the present invention is clearly and completely described. Obviously, the described embodiments are only partial embodiments of the present invention, rather than all embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the scope of protection of the present invention. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0037] Example 1

[0038] The preparation method of the conjugated microporous polymer BTSZ comprises the following specific steps:

[0039] (1) Under argon atmosphere, 165 mg (0.50 mmol) of benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 60 mg (0.50 mmol) of dithiooxamide were added to 30 mL of N,N-dimethylformamide, and the mixture was stirred at 200° C. for 24 h.

[0040] (2) After the reaction is completed, the reaction solution is poured into deionized water and stirred, and then the mixed solution is filtered, and the filter residue is washed with dichloromethane, ethanol, and water respectively, and vacuum dried at 80° C. to finally obtain a reddish brown BTSZ powder.

[0041] Example 2

[0042] The preparation method of the conjugated microporous polymer BTSZ comprises the following specific steps:

[0043] (1) Under argon atmosphere, 250 mg (0.76 mmol) of benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 137 mg (1.14 mmol) of dithiooxamide were added to 40 mL of N,N-dimethylformamide, and the mixture was stirred at 160° C. for 72 h.

[0044] (2) After the reaction is completed, the reaction solution is poured into deionized water and stirred, and then the mixed solution is filtered, and the filter residue is washed with dichloromethane, ethanol, and water respectively, and vacuum dried at 100° C. to finally obtain a reddish-brown BTSZ powder.

[0045] Example 3

[0046] The preparation method of the conjugated microporous polymer BTSZ comprises the following specific steps:

[0047] (1) Under argon atmosphere, 165 mg (0.50 mmol) of benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 300 mg (2.50 mmol) of dithiooxamide were added to 50 mL of N,N-dimethylformamide, and the mixture was stirred at 100° C. for 120 h.

[0048] (2) After the reaction is completed, the reaction solution is poured into deionized water and stirred, and then the mixed solution is filtered, and the filter residue is washed with dichloromethane, ethanol, and water respectively, and vacuum dried at 150° C. to finally obtain a reddish-brown BTSZ powder.

[0049] Figure 1 The structural formula and synthetic route of the conjugated microporous polymer BTSZ are presented. The heterocyclic polymer is synthesized via a reversible Schiff base condensation reaction.

[0050] Figure 2 is the Fourier transform infrared spectrum of the conjugated microporous polymer BTSZ prepared in Example 2. Figure 2 It can be seen that BTSZ is at 1600cm -1 The characteristic absorption peak of C=N double bond is shown at , while this absorption peak is not observed in the infrared spectrum of benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde (BTT), proving the success of the condensation reaction.

[0051] Figure 3 The conjugated microporous polymer BTSZ prepared in Example 2 13 C solid NMR spectrum. Figure 3 It can be seen that the peaks at 130.9ppm and 137.4ppm correspond to the aggregated aromatic carbons in the BTT framework, and the peaks at 142.6ppm and 184.1ppm correspond to the C=C double bond and C=N double bond of the thiazolo[5,4-d]thiazole ring in the BTSZ structure, respectively, proving the success of the condensation reaction.

[0052] Figure 4 The thermogravimetric curve of the conjugated microporous polymer BTSZ prepared in Example 2 under a nitrogen atmosphere. Figure 4 It can be seen that at 322°C, the weight of BTSZ only loses 10%, indicating that it has good thermal stability, ensuring its cycle stability and safety as a negative electrode material for lithium-ion batteries during the cycle process.

[0053] Figure 5 is a scanning electron microscope image of the conjugated microporous polymer BTSZ prepared in Example 2. Figure 5 It can be seen that BTSZ is composed of spherical nanoparticles, and this micromorphology can provide high specific surface area and porous structure.

[0054] Figure 6 is the nitrogen adsorption-desorption curve of the conjugated microporous polymer BTSZ prepared in Example 2. Figure 6 It can be seen that the specific surface area of ​​BTSZ is 279.4m 2 g -1 , whose high specific surface area provides more active sites for redox reactions, thus providing high specific capacity.

[0055] Figure 7 is the pore size distribution diagram of the conjugated microporous polymer BTSZ prepared in Example 2. Figure 7 According to the calculation of the non-local density functional theory model, the pore size of BTSZ is mainly distributed around 0.79 nm, showing significant microporous characteristics. Its porous structure helps the full penetration of the electrolyte and shortens the transmission path of lithium ions, thereby improving the reaction kinetics and rate performance. The conjugated microporous polymers prepared in Examples 1 and 3 have similar physical and chemical properties to the conjugated microporous polymer prepared in Example 2, which will not be repeated here.

[0056] Application Examples

[0057] The BTSZ prepared in Example 2 was used as the negative electrode material of a lithium ion battery to prepare a lithium ion battery and its electrochemical performance was tested.

[0058] (1) Preparation of pole piece: First, use the pre-prepared BTSZ as the active material, conductive carbon black as the conductive agent, and polyvinylidene fluoride as the binder. Mix the active material, conductive agent, and binder in a mass ratio of 6:3:1, add an appropriate amount of N-methylpyrrolidone, and grind to form a uniform slurry. Use a scraper to evenly apply the slurry on the surface of the copper foil and vacuum dry it at 80°C for 12 hours. After drying, use a mold to punch it into a disc with a diameter of 10 mm to obtain the pole piece.

[0059] (2) Assembly of lithium-ion batteries: CR2032 button cells were assembled in an argon-filled glove box (O2≤0.01ppm, H2O≤0.01ppm) using the prepared electrode as the positive electrode, the metal lithium sheet as the negative electrode, 1M LiClO4 in ethylene carbonate (EC): diethyl carbonate (DEC) = 1:1 (v / v) solution as the electrolyte solution, and a polypropylene microporous membrane (Celgard 2500) as the separator.

[0060] (3) Electrochemical performance test of lithium-ion batteries: The prepared lithium-ion batteries were subjected to electrochemical tests.

[0061] Figure 8The conjugated microporous polymer BTSZ is used as the rate performance of the negative electrode material of lithium ion batteries. Figure 8 It can be seen that when the current density increases from 0.1Ag -1 Increase to 2Ag -1 When BTSZ has a peak value of 1016, 742, 533, 409 and 302 mAh g -1 When the current density is restored to 0.1A -1 When the BTSZ electrode is used, it can recover to 982 mAh g -1 The reversible specific capacity shows that it has excellent rate performance.

[0062] Fig. 9 The charge-discharge curves of the conjugated microporous polymer BTSZ as the negative electrode material of lithium-ion batteries under different current densities are shown in the application example. Although the overpotential increases with the increase of current density, the shapes of the charge-discharge curves under different current densities are basically similar.

[0063] Fig.10 The cycling performance of the conjugated microporous polymer BTSZ as a negative electrode material for lithium-ion batteries is shown in the following application examples. Fig.10 It can be seen that at 0.2Ag -1 After 1000 cycles at a current density of 1.34 Å, BTSZ can still maintain 820 mAh g -1 The high reversible specific capacity indicates that it has excellent electrochemical cycle stability. The electrochemical performance of lithium-ion batteries prepared with BTSZ prepared in Examples 1 and 3 as the negative electrode material of lithium-ion batteries is similar to that of lithium-ion batteries prepared with BTSZ prepared in Example 2 as the negative electrode material of lithium-ion batteries, which will not be described in detail here.

[0064] In summary, the present invention uses benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and dithiooxamide as raw materials, and synthesizes the conjugated microporous organic polymer BTSZ in one step through a reversible Schiff base condensation reaction. The material consists of spherical nanoparticles. From a microscopic perspective, this structure not only expands the specific surface area and increases the redox active sites, thereby providing a high specific capacity, but also its porous structure promotes the full penetration of the electrolyte and shortens the transmission path of lithium ions, thereby improving the reaction kinetics and rate performance.

[0065] In addition, the present invention uses benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and dithiooxamide as raw materials, and adopts a reversible Schiff base condensation reaction to synthesize a new type of conjugated microporous polymer. The conjugated microporous polymer material extends the conjugated structure of thiophene and constructs a conjugated thiophene bridge, in which three thiophene units are fused at the boundary of the benzene ring, resulting in a dihedral angle between adjacent thiophenes that is almost zero, which helps to achieve superior π electron delocalization and thus improve conductivity. The present invention introduces a thiazolyl[5,4-d]thiazole ring structure, which can be used as an electron acceptor unit. Combined with the conjugated thiophene bridge structure as an electron donor, an effective electron donor-acceptor system can be formed, which can significantly improve its conductivity. At the same time, the thiazolyl[5,4-d]thiazole ring structure can optimize the pore structure of the conjugated microporous polymer and promote ion transport. The present invention optimizes the electronic structure of the conjugated microporous polymer by introducing heteroatoms such as N and S, thereby improving its conductivity, and at the same time, the C=N double bond in the molecular structure enhances the molecular stability. The conjugated microporous polymer material of the present invention improves the intrinsic conductivity and structural stability of the material by extending the thiophene conjugated structure to construct a conjugated thiophene bridge and introducing a thiazolyl[5,4-d]thiazole ring structure, thereby showing excellent electrochemical properties and having good application prospects in the field of negative electrode materials for lithium ion batteries.

[0066] The present invention synthesizes conjugated microporous polymers with high specific surface area and abundant active sites through molecular design, which can enhance the structural integrity and cycle life of electrode materials. At the same time, by designing conjugated microporous polymers with cross-linked porous skeletons, it can significantly enhance its chemical stability in electrolytes, avoiding the problem that small organic molecules and linear polymers have high solubility in organic electrolytes, which may lead to rapid capacity decay. The new conjugated microporous polymer BTSZ prepared by the present invention is used as a negative electrode material for lithium-ion batteries, which has high specific capacity, good rate performance and excellent cycle stability, and has good application prospects in the field of negative electrode materials for lithium-ion batteries.

[0067] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A novel conjugated microporous polymer, characterized in that: It has the structural formula shown in formula (I):

2. A method for preparing a novel conjugated microporous polymer as claimed in claim 1, characterized in that: The following steps are involved: (1) Under the protection of inert gas, benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and dithiooxamide are added to an organic solvent, and heated and stirred for reaction; (2) After the reaction is completed, washing, filtering and drying are performed to obtain the novel conjugated microporous polymer.

3. The method for preparing a novel conjugated microporous polymer according to claim 2, characterized in that: In step (1), the molar ratio of the benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde to dithiooxamide is 1:1-5.

4. The method for preparing a novel conjugated microporous polymer according to claim 2, characterized in that: In step (1), the organic solvent is N,N-dimethylformamide or N-methylpyrrolidone.

5. The method for preparing a novel conjugated microporous polymer according to claim 2, characterized in that: In step (1), the heating reaction is carried out under stirring at 100-200° C. for 24-120 hours.

6. The method for preparing a novel conjugated microporous polymer according to claim 2, characterized in that: In step (1), the inert gas is nitrogen or argon.

7. The method for preparing a novel conjugated microporous polymer according to claim 2, characterized in that: In step (2), after the reaction is completed, the reaction solution is poured into deionized water and stirred and slurried, and then the mixed solution is filtered, and the filter residue is washed with dichloromethane, ethanol and water respectively, and vacuum dried at 80-150° C. to obtain the novel conjugated microporous polymer.

8. Use of the novel conjugated microporous polymer as claimed in claim 1 in negative electrode materials for lithium-ion batteries.

9. The use according to claim 8, characterized in that The novel conjugated microporous polymer described in claim 1 or the novel conjugated microporous polymer prepared by the preparation method described in any one of claims 2 to 7 is used as an active material, and is evenly mixed with a conductive agent and a binder in a solvent to form a slurry. The slurry is evenly coated on a copper foil, and after vacuum drying, it is cut into electrodes to be used with a cutting machine; the electrode is assembled into a button battery in an argon-protected glove box with a lithium sheet as a negative electrode, a diaphragm, and an electrolyte.

10. The use according to claim 9, characterized in that The conductive agent is at least one of acetylene black, Ketjen black, conductive carbon black and carbon nanotubes; the binder is at least one of polyvinylidene fluoride, styrene-butadiene rubber, sodium alginate, carboxymethyl cellulose, polyvinyl alcohol, polyacrylic acid and polyacrylonitrile; and the solvent is at least one of N-methylpyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide, diethyl ether, ethyl acetate, N-butylpyrrolidone and deionized water.

Citation Information

Patent Citations

  • Polymer containing thiazolo [5, 4-D] thiazole structural unit as well as preparation method and application thereof

    CN116574257A

  • Conjugated porous polymer photocatalytic material as well as preparation method and application thereof

    CN117720728A

  • D-A type covalent organic framework material based on thiazolo [5, 4-d] thiazole bridging as well as preparation method and application of D-A type covalent organic framework material

    CN118290737A

  • Thiazolothiazole composite materials and methods employing the same

    WO2024059798A1