Degradable polyester for preparing non-woven fabric as well as preparation method and application of degradable polyester

By adding specific components and processes to the degradable polyester material, the problem of insufficient spinning performance and flexibility was solved, and polyester suitable for non-woven fabrics with high flexibility and high biodecomposition rate was prepared, achieving no Application of textile fabrics in the field of personal hygiene care.

CN118994542AInactive Publication Date: 2024-11-22SHANDONG DAWN DEGRADABLE MATERIAL CO LTD

Patent Information

Application Number
CN202411487174.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing biodegradable polyester materials have shortcomings in spinning performance and flexibility, and it is difficult to meet the preparation needs of non-woven fabrics, especially in the application of personal hygiene care, and the preparation method is complex and the popularity is poor.

Method used

The components such as dibasic acid, dihydric alcohol, triol, internal lubricant, nucleating agent, chain extender and titanium catalyst are prepared with good flexibility and spinning properties through esterification and polycondensation reaction. Degrade polyester and produce non-woven fabrics with high softness and high biodecomposition rate through specific process parameters and textile processes.

Benefits of technology

Degradable polyester with higher molecular weight, more uniform molecular weight distribution and better fluidity were obtained, which solved the problems of poor spinning properties and thick fiber diameters, and achieved high biodecomposition rate and excellent non-woven fabrics under composting conditions. Spinning effect, suitable for personal hygiene care.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994542A_ABST
    Figure CN118994542A_ABST
Patent Text Reader

Abstract

The invention relates to the field of degradable polyester, in particular to degradable polyester for non-woven fabric preparation and a preparation method and application thereof. Dibasic acid with different chain lengths, dihydric alcohol with different chain lengths and long-chain trihydric alcohol are used as raw materials, an internal lubricant, a nucleating agent, a chain extender and a stabilizer are added at the same time, and esterification and condensation polymerization are carried out under the action of a hydrolysis-resistant titanium catalyst to prepare the high-temperature-resistant polyester resin. Compared with polyester simply prepared from dihydric alcohol and dibasic acid in the prior art, the polyester prepared by the invention not only has good flexibility and excellent spinning performance, but also can be completely degraded after being used without causing any pollution to the environment, and the polyester prepared by the preparation method has the advantages of good flexibility and good spinning performance after the spinning process. The non-woven fabric with fine fiber diameter and high softness is obtained, the biological decomposition rate of the non-woven fabric in 180 days under the composting condition is larger than 97%, and the non-woven fabric can be applied to the field of personal hygiene care.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of degradable polyester, and in particular to a degradable polyester used for preparing non-woven fabrics, and a preparation method and application thereof. Background Art

[0002] With the improvement of environmental awareness, the pollution problem caused by traditional non-degradable non-woven fabrics to the environment is becoming increasingly serious. Therefore, the development of a degradable and environmentally friendly non-woven material has become the focus of industry research. As a new type of environmentally friendly material, degradable polyester has attracted much attention because it can be decomposed by microorganisms in the natural environment. However, the degradable polyester materials that can be used for spinning on the market are mainly polylactic acid (PLA), poly (butylene succinate-co-butylene adipate) (PBAT), polybutylene succinate (PBS), polyhydroxyalkanoate (PHA), etc., but most of the degradable polyester materials have poor spinnability and need to be modified to meet the spinning requirements. At present, PLA has relatively good spinning performance, but PLA is severely brittle and has low elongation, resulting in poor softness of the spunbond nonwoven fabric prepared from it, and cannot be applied to the field of personal hygiene care.

[0003] CN103788346B discloses a biodegradable polyester and a preparation method thereof, wherein a branched aliphatic aromatic copolyester is mixed and contacted with an organic tin catalyst, and then the mixture obtained after the moderate contact is contacted and reacted with lactide. However, it is not known whether the polyester can be used in the preparation of non-woven fabrics. In addition, the preparation method is complicated, and at least three different catalysts must be selected, and different raw materials and catalysts must be added at different reaction nodes, which makes it difficult to popularize the reaction process.

[0004] CN114409910B discloses an antibacterial fully biodegradable plastic and a preparation method thereof, the preparation method is divided into three steps: (1) aliphatic diol and aliphatic dibasic acid in excess molar ratio are subjected to esterification reaction under the catalysis of a catalyst to obtain oligomers; (2) the oligomers are subjected to ester exchange reaction under reduced pressure conditions to obtain polyester precursors; (3) the polyester precursors are reacted with chitin, chitosan and / or their derivatives to obtain antibacterial fully biodegradable plastics. The catalyst is at least one of the chlorides or acetates of metal elements contained in the human body, such as calcium, magnesium, zinc, tin, iron, copper, chromium, cobalt, manganese, and molybdenum. The technical solution proposes that polyols should not be added during the preparation process, because aliphatic polyols and aliphatic polyols will form a macromolecular chain of a body structure, which will directly solidify and ultimately lead to the problem that they cannot be applied to the preparation of non-woven fabrics.

[0005] Based on the above-mentioned prior art, there are limitations in the selection of raw materials for preparing degradable polyester in the prior art, and whether the prepared degradable polyester can be successfully used in the preparation of non-woven fabrics has become a technical problem that needs to be solved urgently. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a degradable polyester for preparing non-woven fabrics, wherein a dibasic acid, a diol, a triol, an internal lubricant, a nucleating agent, a chain extender, a titanium catalyst, and a stabilizer are simultaneously added into a reaction system, and the degradable polyester is obtained by esterification and polycondensation; In terms of weight, the components and contents are as follows: Dibasic acid: 40-50 parts by weight; Diol: 40-60 parts by weight; Triol: 2-20 parts by weight; Internal lubricant: 0.1-2.0 parts by weight; Nucleating agent: 0.2-1.0 parts by weight; Chain extender: 0.1-1.0 parts by weight; Titanium catalyst: 0.02-1.0 parts by weight; Stabilizer: 0.02-0.8 parts by weight; The degradable polyester has a melt index of 24.2-25.8 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, a weight average molecular weight of 70,000-90,000 Daltons, a molecular weight distribution of 1.30-1.50, a tensile strength of 22-23 MPa, and an elongation at break of 701-723%.

[0007] Furthermore, the biodegradable polyester used for preparing the non-woven fabric has a 90-day biodegradability rate greater than 90% under composting conditions.

[0008] Furthermore, the melt index is tested using a melt index meter in accordance with ASTM D1238 standard; The weight average molecular weight and molecular weight distribution are tested by gel permeation chromatography (e2695HPLC), wherein tetrahydrofuran is used as solvent, room temperature, and the flow rate is 1 mL / min. The tensile strength and elongation at break are tested using a tensile testing machine in accordance with ISO527 standards; Furthermore, the dibasic acid is one or more of succinic acid, adipic acid, suberic acid, and sebacic acid.

[0009] Furthermore, the diol is one or more of ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, octanediol, and dodecanediol.

[0010] Furthermore, the triol is one or more of trimethylolpropane octanedecanoic acid ester and trihydroxy long-chain amide.

[0011] Furthermore, the internal lubricant is one or more of glyceryl stearate, N,N-ethylenebisstearamide, butyl stearate, and oxidized polyethylene wax.

[0012] Furthermore, the nucleating agent is one or more of sodium succinate, sodium glutarate, sodium caproate, 4-methyl sodium valerate, and di(p-methylbenzylidene) sorbitol.

[0013] Furthermore, the chain extender is one or more of N,N'-di(2,6-diisopropylphenyl)carbodiimide, isophorone diisocyanate, and hexamethylene diisocyanate.

[0014] Furthermore, the titanium-based catalyst is a hydrolysis-resistant titanium-based catalyst.

[0015] Furthermore, the titanium-based catalyst is tetrabutyl titanate, and its product name is Tyzor AC446.

[0016] Furthermore, the stabilizer is one or more of triethyl phosphate, thiobisphenol, and 2,6-di-tert-butyl-4-methylphenol.

[0017] The present invention also provides a method for preparing the above-mentioned degradable polyester for preparing non-woven fabrics, comprising the following steps: Step 1, adding dibasic acid, diol, triol, internal lubricant, nucleating agent, chain extender, titanium catalyst and stabilizer into a reaction kettle at the same time, heating to esterification temperature, and completing esterification; Step 2: evacuate the reactor and raise the temperature to the polycondensation temperature. After the polycondensation reaction is completed, the degradable polyester is obtained.

[0018] Furthermore, in step 1, the esterification temperature is 200° C. and the esterification time is 3 h.

[0019] Furthermore, the vacuum degree of the vacuum extraction in step 2 is 150 Pa or less, the polycondensation temperature is 230° C., and the polycondensation time is 4 hours.

[0020] The present invention also provides a non-woven fabric, which is prepared by using the above-mentioned degradable polyester for preparing non-woven fabric; The nonwoven fabric has a softness of 17.5-18.7 mN and a fiber diameter of 18.1-18.2 μm.

[0021] Furthermore, the biodegradability of the nonwoven fabric under composting conditions within 180 days is greater than 97%.

[0022] Furthermore, the softness is measured according to GB / T 2986-2016; the fiber diameter is measured by scanning electron microscopy.

[0023] The present invention also provides a method for preparing the non-woven fabric, wherein the degradable polyester used for preparing the non-woven fabric is added into a spunbond non-woven fabric production device, and the non-woven fabric is obtained by drawing and stretching.

[0024] Furthermore, the spunbond nonwoven fabric production equipment includes a single-screw extruder, and the degradable polyester enters the single-screw extruder through a main feeding system connected to a first zone of the single-screw extruder.

[0025] Further, the single screw extruder comprises six temperature zones, and the temperatures of the zones are respectively set to 180-190°C for zone 1, 190-200°C for zone 2, 190-200°C for zone 3, 200-210°C for zone 4, 200-210°C for zone 5, and 200-210°C for zone 6; At the same time, the die temperature is set to 190-200°C, the feed metering pump operates at a frequency of 15-30Hz, the non-woven fabric laying frequency is set to 45-60Hz, and the drafting air frequency is 35-55Hz.

[0026] The present invention also provides a non-woven fabric product, which is prepared from the non-woven fabric.

[0027] Furthermore, the non-woven fabric products include baby diapers, feminine hygiene products, face towels, facial masks, and wet wipes.

[0028] The beneficial effects of the present invention are: 1. The present invention provides a degradable polyester for the preparation of non-woven fabrics. The polyester is prepared by esterification and polycondensation reaction under the action of a hydrolysis-resistant titanium catalyst, using dibasic acids of different chain lengths, diols of different chain lengths, and long-chain triols as raw materials, and adding internal lubricants, nucleating agents, chain extenders, and stabilizers. Compared with the polyester simply prepared from diols and dibasic acids in the prior art, the polyester obtained by the present invention not only has good flexibility and excellent spinning performance, but also can be completely degraded after use, and will not cause any pollution to the environment; 2. The present invention adjusts the formula and process parameters for preparing the degradable polyester, uses long-chain triols, increases the branch length of the polyester, overcomes the technical bias of polyols that cannot be used in the prior art, and obtains a degradable polyester with better performance than that in the prior art; 3. The internal lubricant used in the present invention has good compatibility with the degradable polyester and can be evenly dispersed between the molecular chains, thereby reducing the internal friction between the molecular chains of the degradable polyester and reducing the viscosity of the degradable polyester, thereby improving the fluidity of the degradable polyester; The nucleating agent used in the present invention can increase the crystallization rate of the degradable polyester and provide the required crystal nuclei in the molten state, thereby accelerating the crystallization speed, refining the grain structure, shortening the molding cycle of the degradable polyester, and maintaining the stable performance of the degradable polyester; The chain extender used in the present invention can increase the degree of polymerization of the degradable polyester, increase the molecular weight and melt strength, thereby enhancing the mechanical properties and processing properties of the polyester. The chain extender reacts with the functional groups on the polyester chain to increase the molecular weight of the polyester, while improving its mechanical properties and stability; The titanium catalyst used in the present invention is a hydrolysis-resistant titanium catalyst. The water generated by the esterification reaction will cause the ordinary titanium catalyst to hydrolyze and decompose into titanium dioxide, thereby affecting the reaction process. The present invention uses a specific type of hydrolysis-resistant titanium catalyst, which can effectively prevent the occurrence of the above problem. The stabilizer used in the present invention can improve the thermal stability of the degradable polyester; By combining the internal lubricant, nucleating agent, chain extender, stabilizer, and titanium catalyst, and by selecting the types and proportions of raw materials, the long-chain triol is smoothly added to the formula of the present invention, thereby obtaining a biodegradable polyester with a higher weight average molecular weight, a more uniform molecular weight distribution, and better fluidity. 4. By adjusting the formula and process for preparing biodegradable polyester and finally cooperating with a specific non-woven fabric weaving process, the non-woven fabric has better spinning effect and softness than the non-woven fabric in the prior art. The technical problems of poor spinning performance, easy fiber breakage and coarse fiber diameter in the process of preparing non-woven fabric in the prior art are overcome; After the spinning process, the polyester prepared by the present invention obtains a non-woven fabric with fine fiber diameter and high softness, and the biodegradability of the non-woven fabric under composting conditions is greater than 97% within 180 days, and can be applied to the field of personal hygiene care. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a scanning electron microscope image of the diameter of the non-woven fabric fiber of Example 8 of the present invention; Figure 2 This is the spinning process of Example 8 of the present invention; Figure 3 The nonwoven fabric sample prepared in Example 8 of the present invention; Figure 4 This is a scanning electron microscope image of the diameter of the non-woven fabric fiber of Comparative Example 3 of the present invention; Figure 5 This is the spinning process of Comparative Example 3 of the present invention; Figure 6 The nonwoven fabric sample prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0030] Examples 1-7 are degradable polyesters for use in the preparation of nonwoven fabrics and methods for preparing the same; Wherein, the melt index is tested using a melt index meter according to ASTM D1238 standard; The weight average molecular weight and molecular weight distribution are tested by gel permeation chromatography (e2695HPLC), wherein tetrahydrofuran is used as solvent, room temperature, and the flow rate is 1 mL / min. The tensile strength and elongation at break are tested using a tensile testing machine in accordance with ISO527 standards; Examples 8-9 are non-woven fabrics made from the degradable polyester prepared in Examples 1-2; Wherein, the softness is measured according to GB / T 2986-2016; The fiber diameter was measured by scanning electron microscopy.

[0031] Example 1 This embodiment provides a degradable polyester for preparing a non-woven fabric, wherein succinic acid, hexanediol, trihydroxy long-chain amide, internal lubricant butyl stearate, nucleating agent sodium caproate, chain extender hexamethylene diisocyanate, tetrabutyl titanate Tyzor AC446, and stabilizer triethyl phosphate are simultaneously added into a reaction system, and the degradable polyester is obtained by esterification and polycondensation; In terms of weight, the components and contents are as follows: Succinic acid: 50 parts by weight; Hexylene glycol: 40 parts by weight; Trihydroxy long chain amide: 10 parts by weight; Internal lubricant butyl stearate: 0.2 parts by weight; Nucleating agent sodium caproate: 0.2 parts by weight; Chain extender hexamethylene diisocyanate: 0.1 parts by weight; Tetrabutyl titanate Tyzor AC446: 0.08 parts by weight; Stabilizer triethyl phosphate: 0.1 parts by weight; The degradable polyester has a melt index of 25.8 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, a weight average molecular weight of 78811 Daltons, a molecular weight distribution of 1.33, a tensile strength of 22.0 MPa, and an elongation at break of 701%. The biodegradability of the degradable polyester used for the preparation of non-woven fabrics is 93% under composting conditions within 90 days.

[0032] This embodiment also provides a method for preparing the above-mentioned degradable polyester for preparing non-woven fabrics, comprising the following steps: Step 1, adding succinic acid, hexanediol, trihydroxy long-chain amide, internal lubricant butyl stearate, nucleating agent sodium caproate, chain extender hexamethylene diisocyanate, tetrabutyl titanate Tyzor AC446, and stabilizer triethyl phosphate into a reaction kettle at the same time, heating to an esterification temperature of 200° C., the esterification time is 3 hours, and the esterification is completed; Step 2: evacuate the reactor to 150 Pa and raise the temperature to the polycondensation temperature of 230° C. for 4 hours. After the polycondensation reaction is completed, the degradable polyester is obtained.

[0033] Example 2 This embodiment provides a degradable polyester for preparing non-woven fabrics, wherein succinic acid, butanediol, trihydroxy long-chain amide, internal lubricant oxidized polyethylene wax, nucleating agent sodium glutarate, chain extender isophorone diisocyanate, tetrabutyl titanate Tyzor AC446, and stabilizer thiobisphenol are added to a reaction system at the same time, and the degradable polyester is obtained by esterification and polycondensation; In terms of weight, the components and contents are as follows: Succinic acid: 50 parts by weight; Butanediol: 40 parts by weight; Trihydroxy long chain amide: 10 parts by weight; Internal lubricant oxidized polyethylene wax: 0.1 parts by weight; Nucleating agent sodium glutarate: 0.2 parts by weight; Chain extender isophorone diisocyanate: 0.2 parts by weight; Tetrabutyl titanate Tyzor AC446: 0.08 parts by weight; Stabilizer thiobisphenol: 0.1 parts by weight; The degradable polyester has a melt index of 24.2 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, a weight average molecular weight of 73610 Daltons, a molecular weight distribution of 1.36, a tensile strength of 23.0 MPa, and an elongation at break of 723%. The biodegradability of the degradable polyester used for the preparation of non-woven fabrics is 97% under composting conditions within 90 days.

[0034] This embodiment also provides a method for preparing the above-mentioned degradable polyester for preparing non-woven fabrics, comprising the following steps: Step 1, adding succinic acid, hexanediol, trihydroxy long-chain amide, internal lubricant oxidized polyethylene wax, nucleating agent sodium glutarate, chain extender isophorone diisocyanate, tetrabutyl titanate Tyzor AC446, and stabilizer thiobisphenol into a reaction kettle at the same time, heating to an esterification temperature of 200° C., the esterification time is 3 hours, and the esterification is completed; Step 2: evacuate the reactor to 150 Pa and raise the temperature to the polycondensation temperature of 230° C. for 4 hours. After the polycondensation reaction is completed, the degradable polyester is obtained.

[0035] Example 3 This embodiment provides a degradable polyester for preparing non-woven fabrics, wherein adipic acid, octanediol, trimethylolpropane octanedioate, internal lubricant glyceryl stearate, nucleating agent sodium succinate, chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide, tetrabutyl titanate Tyzor AC446, and stabilizer 2,6-di-tert-butyl-4-methylphenol are simultaneously added to a reaction system, and the degradable polyester is obtained by esterification and polycondensation. In terms of weight, the components and contents are as follows: Adipic acid: 40 parts by weight; Octanediol: 60 parts by weight; Trimethylolpropane octanedionate: 2 parts by weight; Internal lubricant glyceryl stearate: 1.0 parts by weight; Nucleating agent sodium succinate: 1.0 parts by weight; Chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide: 0.6 parts by weight; Tetrabutyl titanate Tyzor AC446: 0.02 parts by weight; Stabilizer 2,6-di-tert-butyl-4-methylphenol: 0.8 parts by weight; The degradable polyester has a melt index of 24.4 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, a weight average molecular weight of 84710 Daltons, a molecular weight distribution of 1.40, a tensile strength of 22.7 MPa, and an elongation at break of 721%. The biodegradable polyester used for the preparation of non-woven fabrics has a 90-day biodegradability of 95% under composting conditions.

[0036] This embodiment also provides a method for preparing the above-mentioned degradable polyester for preparing non-woven fabrics, comprising the following steps: Step 1, adding adipic acid, octanediol, trimethylolpropane octanedioate, internal lubricant glyceryl stearate, nucleating agent sodium succinate, chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide, tetrabutyl titanate Tyzor AC446, and stabilizer 2,6-di-tert-butyl-4-methylphenol into a reaction kettle at the same time, heating to an esterification temperature of 200°C, and the esterification time is 3 hours to complete the esterification; Step 2: evacuate the reactor to 150 Pa and raise the temperature to the polycondensation temperature of 230° C. for 4 hours. After the polycondensation reaction is completed, the degradable polyester is obtained.

[0037] Example 4 This embodiment provides a degradable polyester for preparing non-woven fabrics, wherein suberic acid, ethylene glycol, trimethylolpropane octanoate, internal lubricant N,N-ethylenebisstearamide, nucleating agent sodium 4-methylvalerate, chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide, tetrabutyl titanate Tyzor AC446, and stabilizer 2,6-di-tert-butyl-4-methylphenol are added to a reaction system at the same time, and the degradable polyester is obtained by esterification and polycondensation. In terms of weight, the components and contents are as follows: Suberic acid: 44 parts by weight; Ethylene glycol: 50 parts by weight; Trimethylolpropane octanedecanoate: 20 parts by weight; Internal lubricant N,N-ethylenebisstearamide: 2.0 parts by weight; Nucleating agent 4-methyl sodium valerate: 0.7 parts by weight; Chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide: 1.0 parts by weight; Tetrabutyl titanate Tyzor AC446: 1.0 parts by weight; Stabilizer 2,6-di-tert-butyl-4-methylphenol: 0.02 parts by weight; The degradable polyester has a melt index of 25.3 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, a weight average molecular weight of 87180 Daltons, a molecular weight distribution of 1.43, a tensile strength of 22.1 MPa, and an elongation at break of 715%. The biodegradability of the degradable polyester used for the preparation of non-woven fabrics is 98% under composting conditions within 90 days.

[0038] This embodiment also provides a method for preparing the above-mentioned degradable polyester for preparing non-woven fabrics, comprising the following steps: Step 1, add suberic acid, ethylene glycol, trimethylolpropane octanoate, internal lubricant N,N-ethylenebisstearamide, nucleating agent sodium 4-methylvalerate, chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide, tetrabutyl titanate Tyzor AC446, stabilizer 2,6-di-tert-butyl-4-methylphenol into a reaction kettle at the same time, heat to esterification temperature 200°C, esterification time 3h, and complete esterification; Step 2: evacuate the reactor to 150 Pa and raise the temperature to the polycondensation temperature of 230° C. for 4 hours. After the polycondensation reaction is completed, the degradable polyester is obtained.

[0039] Example 5 This embodiment provides a degradable polyester for preparing non-woven fabrics, wherein succinic acid, sebacic acid, propylene glycol, octanediol, trimethylolpropane octanedioate, trihydroxy long-chain amide, internal lubricant oxidized polyethylene wax, nucleating agent di(p-methylbenzylidene) sorbitol, chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide, tetrabutyl titanate Tyzor AC446, and stabilizer 2,6-di-tert-butyl-4-methylphenol are added to a reaction system at the same time, and the degradable polyester is obtained by esterification and polycondensation. In terms of weight, the components and contents are as follows: Succinic acid: 22 parts by weight; Sebacic acid: 22 parts by weight; Propylene glycol: 30 parts by weight; Octanediol: 30 parts by weight; Trimethylolpropane octanedecanoate: 8 parts by weight; Trihydroxy long chain amide: 8 parts by weight; Internal lubricant oxidized polyethylene wax: 1.4 parts by weight; Nucleating agent di(p-methylbenzylidene)sorbitol: 0.3 parts by weight; Chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide: 1.0 parts by weight; Tetrabutyl titanate Tyzor AC446: 0.04 parts by weight; Stabilizer 2,6-di-tert-butyl-4-methylphenol: 0.6 parts by weight; The degradable polyester has a melt index of 24.9 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, a weight average molecular weight of 82590 Daltons, a molecular weight distribution of 1.48, a tensile strength of 22.2 MPa, and an elongation at break of 716%. The biodegradability of the degradable polyester used for the preparation of non-woven fabrics is 95% under composting conditions within 90 days.

[0040] This embodiment also provides a method for preparing the above-mentioned degradable polyester for preparing non-woven fabrics, comprising the following steps: Step 1, adding succinic acid, sebacic acid, propylene glycol, octanediol, trimethylolpropane octanedioate, trihydroxy long-chain amide, internal lubricant oxidized polyethylene wax, nucleating agent di(p-methylbenzylidene) sorbitol, chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide, tetrabutyl titanate Tyzor AC446, stabilizer 2,6-di-tert-butyl-4-methylphenol into a reaction kettle at the same time, heating to an esterification temperature of 200°C, esterification time of 3h, and completing esterification; Step 2: evacuate the reactor to 150 Pa and raise the temperature to the polycondensation temperature of 230° C. for 4 hours. After the polycondensation reaction is completed, the degradable polyester is obtained.

[0041] Example 6 This embodiment provides a degradable polyester for preparing non-woven fabrics. Sebacic acid, dodecyl glycol, trihydroxy long-chain amide, internal lubricant butyl stearate, internal lubricant oxidized polyethylene wax, nucleating agent sodium succinate, nucleating agent di(p-methylbenzylidene) sorbitol, chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide, chain extender isophorone diisocyanate, tetrabutyl titanate Tyzor AC446, and stabilizer 2,6-di-tert-butyl-4-methylphenol are added to a reaction system at the same time, and the degradable polyester is obtained by esterification and polycondensation. In terms of weight, the components and contents are as follows: Sebacic acid: 47 parts by weight; Dodecyl glycol: 52 parts by weight; Trihydroxy long chain amide: 13 parts by weight; Internal lubricant butyl stearate: 0.6 parts by weight; Internal lubricant oxidized polyethylene wax: 1.0 parts by weight; Nucleating agent sodium succinate: 0.4 parts by weight; Nucleating agent di(p-methylbenzylidene)sorbitol: 0.5 parts by weight; Chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide: 0.5 parts by weight; Chain extender isophorone diisocyanate: 0.5 parts by weight; Tetrabutyl titanate Tyzor AC446: 0.07 parts by weight; Stabilizer 2,6-di-tert-butyl-4-methylphenol: 0.47 parts by weight; The degradable polyester has a melt index of 24.6 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, a weight average molecular weight of 76,830 Daltons, a molecular weight distribution of 1.32, a tensile strength of 22.7 MPa, and an elongation at break of 709%. The biodegradability of the degradable polyester used for the preparation of non-woven fabrics is 94% under composting conditions within 90 days.

[0042] This embodiment also provides a method for preparing the above-mentioned degradable polyester for preparing non-woven fabrics, comprising the following steps: Step 1, add sebacic acid, dodecyl glycol, trihydroxy long-chain amide, internal lubricant butyl stearate, internal lubricant oxidized polyethylene wax, nucleating agent di(p-methylbenzylidene) sorbitol, chain extender N,N'-bis(2,6-diisopropylphenyl)carbodiimide, chain extender isophorone diisocyanate, tetrabutyl titanate Tyzor AC446, stabilizer 2,6-di-tert-butyl-4-methylphenol into a reaction kettle at the same time, heat to esterification temperature 200°C, esterification time 3h, and complete esterification; Step 2: evacuate the reactor to 150 Pa and raise the temperature to the polycondensation temperature of 230° C. for 4 hours. After the polycondensation reaction is completed, the degradable polyester is obtained.

[0043] Example 7 This embodiment provides a degradable polyester for preparing non-woven fabrics, wherein succinic acid, hexanediol, trihydroxy long-chain amide, internal lubricant oxidized polyethylene wax, nucleating agent sodium glutarate, chain extender isophorone diisocyanate, tetrabutyl titanate Tyzor AC446, stabilizer triethyl phosphate, and stabilizer thiobisphenol are added to a reaction system at the same time, and the degradable polyester is obtained by esterification and polycondensation; In terms of weight, the components and contents are as follows: Succinic acid: 50 parts by weight; Hexylene glycol: 60 parts by weight; Trihydroxy long chain amide: 10 parts by weight; Internal lubricant oxidized polyethylene wax: 0.1 parts by weight; Nucleating agent sodium glutarate: 0.2 parts by weight; Chain extender isophorone diisocyanate: 0.2 parts by weight; Tetrabutyl titanate Tyzor AC446: 1.0 parts by weight; Stabilizer triethyl phosphate: 0.05 parts by weight; Stabilizer thiobisphenol: 0.05 parts by weight; The degradable polyester has a melt index of 24.2 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, a weight average molecular weight of 71050 Daltons, a molecular weight distribution of 1.39, a tensile strength of 22.5 MPa, and an elongation at break of 719%. The biodegradability of the degradable polyester used for the preparation of non-woven fabrics is 99% under composting conditions within 90 days.

[0044] This embodiment also provides a method for preparing the above-mentioned degradable polyester for preparing non-woven fabrics, comprising the following steps: Step 1, adding succinic acid, hexanediol, trihydroxy long-chain amide, internal lubricant oxidized polyethylene wax, nucleating agent sodium glutarate, chain extender isophorone diisocyanate, tetrabutyl titanate Tyzor AC446, stabilizer triethyl phosphate, stabilizer thiobisphenol into a reaction kettle at the same time, heating to an esterification temperature of 200° C., the esterification time is 3 hours, and the esterification is completed; Step 2: evacuate the reactor to 150 Pa and raise the temperature to the polycondensation temperature of 230° C. for 4 hours. After the polycondensation reaction is completed, the degradable polyester is obtained.

[0045] Example 8 This embodiment provides a non-woven fabric, which is prepared by using the degradable polyester used for preparing the non-woven fabric in Embodiment 1; The nonwoven fabric has a softness of 17.5 mN, an average fiber diameter of 18.2 μm, and a biodegradability of 98% within 180 days under composting conditions. Figure 1 As shown, the fiber diameter was measured by scanning electron microscopy.

[0046] This embodiment also provides a method for preparing the non-woven fabric. The degradable polyester used for preparing the non-woven fabric in Embodiment 1 is added into a spunbond non-woven fabric production device, and the non-woven fabric is obtained by drawing and stretching.

[0047] The spunbond nonwoven fabric production equipment comprises a single-screw extruder, and the degradable polyester enters the single-screw extruder through a main feeding system connected to a first zone of the single-screw extruder.

[0048] The single screw extruder comprises six temperature zones, and the temperatures of the zones are respectively set to 180°C for zone 1, 190°C for zone 2, 190°C for zone 3, 200°C for zone 4, 200°C for zone 5, and 200°C for zone 6; At the same time, the die temperature was set to 200°C, the feed metering pump operating frequency was 15 Hz, the nonwoven fabric laying frequency was set to 45 Hz, and the drafting air frequency was 35 Hz.

[0049] like Figure 2 The spinning process of this embodiment is shown.

[0050] like Figure 3 Shown is the nonwoven fabric sample prepared in this embodiment.

[0051] Example 9 This embodiment provides a non-woven fabric, which is prepared by using the degradable polyester used for preparing the non-woven fabric in Embodiment 2; The nonwoven fabric has a softness of 18.7 mN, an average fiber diameter of 18.1 μm, and a 180-day biodegradability rate of 99% under composting conditions.

[0052] This embodiment also provides a method for preparing the above non-woven fabric, wherein the degradable polyester used for preparing the non-woven fabric in Example 2 is added into a spunbond non-woven fabric production device, and the non-woven fabric is obtained by drawing and stretching.

[0053] The spunbond nonwoven fabric production equipment comprises a single-screw extruder, and the degradable polyester enters the single-screw extruder through a main feeding system connected to a first zone of the single-screw extruder.

[0054] The single screw extruder includes six temperature zones, and the temperatures of the zones are set to 190°C for zone 1, 200°C for zone 2, 200°C for zone 3, 210°C for zone 4, 210°C for zone 5, and 210°C for zone 6; At the same time, the die temperature was set to 190°C, the feed metering pump operated at 30 Hz, the nonwoven fabric laying frequency was set to 60 Hz, and the drafting air frequency was 55 Hz.

[0055] Comparative Example 1 This comparative example provides a polyester used for preparing non-woven fabrics in the prior art, wherein succinic acid, butanediol, and ordinary tetrabutyl titanate without anti-hydrolysis function are added to a reaction system, and the polyester is obtained after reaction; In terms of weight, the components and contents are as follows: Succinic acid: 50 parts by weight; Butanediol: 50 parts by weight; Tetrabutyl titanate: 0.03 parts by weight; The polyester has a melt index of 4.8 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, a weight average molecular weight of 69590 Daltons, a molecular weight distribution of 1.86, a tensile strength of 17 MPa, an elongation at break of 659%, and a 90-day biodegradability of 90% under composting conditions.

[0056] This comparative example also provides a method for preparing the above polyester, comprising the following steps: Step 1, adding succinic acid, butanediol and tetrabutyl titanate into a reaction kettle at the same time, heating to an esterification temperature of 200°C, and the esterification time is 3 hours to complete the esterification; Step 2: After the temperature is raised to 240° C., the reactor is evacuated to 150 Pa, and the polycondensation time is 4 hours. After the polycondensation reaction is completed, the polyester is obtained.

[0057] Comparative Example 2 This comparative example provides a polyester obtained by adding a triol, wherein succinic acid, butanediol, trihydroxy long-chain amide, and tetrabutyl titanate Tyzor AC446 are added to a reaction system, and the polyester is obtained after reaction; In terms of weight, the components and contents are as follows: Succinic acid: 50 parts by weight; Butanediol: 50 parts by weight; Trihydroxy long chain amide: 10 parts by weight; Tetrabutyl titanate Tyzor AC446: 0.03 parts by weight; The polyester has a melt index of 14.2 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, a weight average molecular weight of 47,380 Daltons, a molecular weight distribution of 2.19, a tensile strength of 8 MPa, an elongation at break of 365%, and a 90-day biodegradability of 76% under composting conditions.

[0058] This comparative example also provides a method for preparing the above polyester, comprising the following steps: Step 1, adding succinic acid, butanediol, trihydroxy long-chain amide, and tetrabutyl titanate Tyzor AC446 into a reaction kettle at the same time, heating to an esterification temperature of 200° C., and the esterification time is 3 hours to complete the esterification; Step 2: After the temperature is raised to 240°C, the reactor is evacuated to 150 Pa, and the polycondensation time is 4 hours. After the polycondensation reaction is completed, the polyester is obtained, and the polyester is a solidified product. It is impossible to spin and prepare non-woven fabrics under the same conditions.

[0059] Comparative Example 3 This comparative example provides a nonwoven fabric, which is prepared by using the polyester in comparative example 1; The nonwoven fabric has a softness of 10.4 mN, an average fiber diameter of 24.0 μm, and a biodegradability of 91% within 180 days under composting conditions. Figure 4 As shown, the fiber diameter was measured by scanning electron microscopy.

[0060] This comparative example also provides a method for preparing the nonwoven fabric. The polyester in comparative example 1 is added into a spunbond nonwoven fabric production device, and the nonwoven fabric is obtained by drawing and stretching.

[0061] The spunbond nonwoven fabric production equipment comprises a single-screw extruder, and the degradable polyester enters the single-screw extruder through a main feeding system connected to a first zone of the single-screw extruder.

[0062] The single screw extruder includes six temperature zones, and the temperatures of the zones are set to 190°C for zone 1, 200°C for zone 2, 200°C for zone 3, 210°C for zone 4, 210°C for zone 5, and 210°C for zone 6; At the same time, the die temperature was set to 190°C, the feed metering pump operated at 30 Hz, the nonwoven fabric laying frequency was set to 60 Hz, and the drafting air frequency was 55 Hz.

[0063] like Figure 5 Shown is the spinning process of this comparative example.

[0064] like Figure 6 Shown is a nonwoven fabric sample prepared in this comparative example.

[0065] The properties of the polyesters prepared in Examples 1-6 and Comparative Examples 1-2 are compared, and the results are shown in Table 1: Table 1 Comparison of properties of polyesters prepared in Examples and Comparative Examples

[0066] The properties of the nonwoven fabrics prepared in Examples 7-8 and Comparative Example 3 are compared, and the comparison results are shown in Table 2: Table 2 Comparison of properties of nonwoven fabrics prepared in Examples and Comparative Examples

[0067] Through the above-mentioned performance comparison of polyester and non-woven fabric, it can be intuitively seen that the degradable polyester prepared by the present invention has a higher melt index, a more uniform molecular weight distribution, better tensile strength and elongation at break, and a degradation rate of nearly 100% in 90 days compared with the polyester in the prior art. At the same time, it can be intuitively seen from the spinning process of the non-woven fabric prepared by the comparative example and the comparative example, and the comparison chart of the processed non-woven fabric finished product that the non-woven fabric prepared by the present invention has better spinning effect and softness than the non-woven fabric in the prior art. However, the polyester in the comparative example is prone to poor spinning, easy broken wires, and thick fiber diameter during the preparation of the non-woven fabric.

[0068] It should be understood that the present invention is not limited to what has been described above and shown in the accompanying drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present invention is limited only by the appended claims.

Claims

1. A degradable polyester for preparing nonwoven fabrics, It is characterized in that Adding dibasic acid, diol, triol, internal lubricant, nucleating agent, chain extender, titanium catalyst and stabilizer into the reaction system at the same time, and obtaining the degradable polyester through esterification and polycondensation; In terms of weight, the components and contents are as follows: Dibasic acid: 40-50 parts by weight; Diol: 40-60 parts by weight; Triol: 2-20 parts by weight; Internal lubricant: 0.1-2.0 parts by weight; Nucleating agent: 0.2-1.0 parts by weight; Chain extender: 0.1-1.0 parts by weight; Titanium catalyst: 0.02-1.0 parts by weight; Stabilizer: 0.02-0.8 parts by weight; The degradable polyester has a melt index of 24.2-25.8 g / 10min at a temperature of 190°C and a load of 2.16 kg, a weight average molecular weight of 70,000-90,000 Daltons, a molecular weight distribution of 1.30-1.50, a tensile strength of 22-23 MPa, and an elongation at break of 701-723%.

2. The degradable polyester for preparing nonwoven fabrics according to claim 1, It is characterized in that The dibasic acid is one or more of succinic acid, adipic acid, suberic acid and sebacic acid.

3. The degradable polyester for preparing nonwoven fabric according to claim 1, It is characterized in that The diol is one or more of ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, octanediol and dodecanediol.

4. The degradable polyester for preparing nonwoven fabric according to claim 1, It is characterized in that The triol is one or more of trimethylolpropane octanedecanoic acid ester and trihydroxy long-chain amide.

5. The degradable polyester for preparing nonwoven fabric according to claim 1, It is characterized in that The internal lubricant is one or more of stearic acid glyceryl ester, N, N-ethylene bis stearic acid amide, butyl stearate, and oxidized polyethylene wax; The nucleating agent is one or more of sodium succinate, sodium glutarate, sodium caproate, sodium 4-methylvalerate, and di(p-methylbenzylidene)sorbitol; The chain extender is one or more of N,N'-di(2,6-diisopropylphenyl)carbodiimide, isophorone diisocyanate, and hexamethylene diisocyanate; The titanium catalyst is tetrabutyl titanate; The stabilizer is one or more of triethyl phosphate, thiobisphenol, and 2,6-di-tert-butyl-4-methylphenol.

6. A method for preparing the degradable polyester for non-woven fabric according to any one of claims 1 to 5, It is characterized in that The steps include: Step 1, adding dibasic acid, diol, triol, internal lubricant, nucleating agent, chain extender, titanium catalyst and stabilizer into a reaction kettle at the same time, heating to esterification temperature, and completing esterification; Step 2: evacuate the reactor and raise the temperature to the polycondensation temperature. After the polycondensation reaction is completed, the degradable polyester is obtained.

7. The method for preparing the degradable polyester for non-woven fabric according to claim 6, It is characterized in that In step 1, the esterification temperature is 200°C and the esterification time is 3h; The vacuum degree of the vacuum pumping in step 2 is 150Pa or less, the polycondensation temperature is 230°C, and the polycondensation time is 4h.

8. A nonwoven fabric, It is characterized in that The nonwoven fabric is prepared by using the degradable polyester for preparing nonwoven fabric according to any one of claims 1 to 5; The nonwoven fabric has a softness of 17.5-18.7 mN and a fiber diameter of 18.1-18.2 μm.

9. A method for preparing the nonwoven fabric according to claim 8, It is characterized in that The above-mentioned degradable polyester for preparing non-woven fabric is added into the spunbond non-woven fabric production equipment, and the non-woven fabric is obtained by drawing and stretching.

10. A non-woven fabric product, It is characterized in that The nonwoven fabric product is made from the nonwoven fabric of claim 8; The non-woven fabric products include baby diapers, feminine hygiene products, face towels, facial masks, and wet wipes.

Citation Information

Patent Citations

  • Preparation method for high-strength biodegradable polyester fiber

    WO2024164576A1

Cited By

  • Degradable polyester fiber and preparation process therefor

    WO2026124576A1