Seawater degradable injection molding material and preparation method thereof

By designing new seawater degradation resins and functional modifiers, the problem of poor degradation performance of existing degradable plastics in the marine environment is solved, rapid degradation and excellent mechanical properties in seawater are achieved, and the feasibility of the injection molding process is improved. .

CN118994545APending Publication Date: 2024-11-22DANYANG HENGLV NEW MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411307624.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing biodegradable plastics have poor degradation performance in marine environments, especially in low temperature environments, which are difficult to decompose quickly, and their processing and mechanical properties are insufficient, which cannot meet the application needs in seawater.

Method used

By designing a new seawater degradation resin and functional modifier, it uses raw materials such as 1,4-butanediol, dimethyl carbonate, lactic acid, glycolic acid, terephthalic acid, oxalic acid and low molecular weight polyethylene glycol. Transesterification and silanization coupling reaction prepare injection molding with excellent flexibility, seawater degradability and mechanical properties, and seawater degradation injection molding is prepared through mixing and granulation processes.

Benefits of technology

It achieves rapid degradation and excellent mechanical properties in seawater, improves the feasibility of the injection molding process and the comprehensive performance of the materials, and solves the problem of slow degradation of existing materials in the marine environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PKAPZLRSDGPDGGTUXQYR1BGRB4IRQGATC8C1Y8H6
    Figure PKAPZLRSDGPDGGTUXQYR1BGRB4IRQGATC8C1Y8H6
Patent Text Reader

Abstract

The invention belongs to the field of high polymer materials. The invention relates to a seawater degradable injection molding material and a preparation method thereof. The material comprises the following raw materials in parts by weight: 80-90 parts of seawater degradable resin; 10 to 20 parts of a polylactic acid-glycollic acid copolymer; 3.0 to 5.0 parts of a functional modifier; 0.5 to 1.0 part of a UV absorbent; 0.2 to 0.5 part of an antioxidant; 0.3 to 0.8 part of an anti-hydrolysis agent; 0.5 to 1.0 part of a plasticizer; 1.5 to 2.5 parts of a heat stabilizer; 0.2 to 0.5 part of a lubricant; wherein the total mass of the seawater degradable resin and the polylactic acid-glycollic acid copolymer is 100 parts; the raw materials are blended and granulated to prepare the degradable material, so that the defect of slow seawater degradation of the degradable material which is easily subjected to injection molding in the prior art can be effectively overcome, and the degradable material has relatively great application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a seawater degradable injection molding material and a preparation method thereof, and belongs to the field of degradable polymer materials. Background Art

[0002] About 10 million tons of plastic enter the ocean every year. UN Secretary-General Guterres pointed out that if humans do not change their current plastic usage habits, by 2050, the total weight of plastic waste in the ocean may exceed that of fish. A large amount of microplastics enters sea salt or is eaten by marine life. Microplastics in sea salt are directly ingested by humans, and microplastics in marine life will eventually enter the human body through the food chain. According to statistics, there are 550-681 pieces of microplastics in each kilogram of sea salt. Based on the calculation that each person eats 5 grams of salt per day, a person will eat about 2,000 pieces of microplastics per year.

[0003] In view of the above situation, the research and development of fully biodegradable plastics has entered people's field of vision as a cutting-edge scientific work. However, general fully biodegradable plastics such as polylactic acid (PLA), polybutylene terephthalate adipate copolyester (PBAT), polybutylene succinate (PBS), polycaprolactone (PCL), etc. often have unsatisfactory degradation performance in the ocean due to their high glass transition temperature, good hydrophobicity or excellent crystallization performance.

[0004] PLA has good biodegradability, especially in industrial composting, PLA can be degraded within 3 months. It has excellent injection molding properties, but in the low temperature environment of the ocean, PLA cannot be degraded for several years. PCL is also a recognized fully biodegradable plastic, and it has very excellent mechanical strength and low-temperature processing properties (PCL melting point is around 60°C), but PCL's biodegradability in the ocean is also extremely limited; and it has low hardness, low bending strength and modulus; poor injection molding properties, especially thick-walled products require a longer molding cycle.

[0005] Different from PLA, PBAT, PBS and PCL is another biodegradable material, polyglycolic acid (PGA). PGA is an excellent biodegradable material. Its glycolic acid structural unit is an easily hydrolyzed structural unit. Compared with PLA, the main chain unit has one less methyl group, so it is more hydrophilic and has a faster hydrolysis rate than PLA. However, it is also expensive, and the processing temperature is too high and the toughness is insufficient, which affects its promotion and use.

[0006] In view of the above reasons, taking into account the seawater degradability and processability of the materials, it is necessary to modify existing materials and develop new materials in order to meet the requirements. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a seawater-degradable injection molding material in view of the defect that the degradable materials that are easy to be injection molded in the prior art are slowly degraded by seawater. The method is based on molecular structure design to prepare a seawater-degradable resin and a functional modifier; and through formula design optimization; and through mixing and granulation processes to prepare injection molding pellets. The technical solution adopted by the present invention to solve its technical problems is: The present invention provides a method for preparing a seawater-degradable resin, comprising the following steps: S11, subjecting 1,4-butanediol and dimethyl carbonate to an ester exchange reaction to obtain an intermediate product IA and an intermediate product IB; S12, mixing the intermediate product IB, lactic acid and glycolic acid for pre-polycondensation reaction to obtain an intermediate product II; S13, performing a pre-polycondensation reaction on terephthalic acid, oxalic acid, polyethylene glycol, and 1,4-butanediol to obtain an intermediate product III; S14, subjecting the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate to an ester exchange reaction to obtain a target product, namely, a seawater degradable resin.

[0008] Furthermore, the molar ratio of 1,4-butanediol to dimethyl carbonate is 1.5-2.5:1.

[0009] Furthermore, the molar ratio of the intermediate product IB, lactic acid and glycolic acid is 1:0.4-0.6:1.4-1.8.

[0010] Furthermore, the molar ratio of terephthalic acid, oxalic acid, polyethylene glycol, and 1,4-butanediol is 0.3-0.5: 0.5-0.7: 1.5-2.0: 0.5-1.0; and The amount of polyethylene glycol is 200-600.

[0011] Furthermore, the molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 1.0-1.2:0.2-0.3:0.1-0.2:1.0.

[0012] The present invention also provides a seawater-degradable resin, which is prepared by the above-mentioned seawater-degradable resin preparation method.

[0013] Another object of the present invention is to provide a method for preparing a functional modifier, comprising the following steps: S21, adding zeolite into a salt solution to carry out an ion exchange reaction to obtain a modified zeolite I; S22, performing coordination reaction on the modified zeolite I and the organic ligand to obtain modified zeolite II; S23, performing a silylation coupling reaction on the modified zeolite II and the epoxy silane coupling agent to obtain a functional modifier.

[0014] Furthermore, the usage ratio of the zeolite and the salt solution is 10 g: 100-200 mL; and The mesh number of the zeolite is 250-2500 mesh; The salt solution is iron salt and has a concentration of 1.0-3.0 mol / L.

[0015] Furthermore, the usage ratio of the modified zeolite I and the organic ligand solution is 10 g: 100-300 mL; and The organic ligand concentration is 1.0-3.0 mol / L; The organic ligand is glycolic acid and / or other carboxylic acids.

[0016] Furthermore, the usage ratio of the modified zeolite II and the epoxy silane coupling agent is 1g:3.0-5.0g.

[0017] The present invention also provides a functional modifier, which is prepared by the preparation method of the functional modifier.

[0018] Another object of the present invention is to provide a seawater-degradable injection molding material, comprising the following raw materials in parts by weight: 80-90 parts of seawater degradable resin; 10-20 parts of polylactic acid-glycolic acid copolymer; Functional modifier 3.0-5.0 parts; UV absorber 0.5-1.0 part; Antioxidant 0.2-0.5 parts; Anti-hydrolysis agent 0.3-0.8 parts; Plasticizer 0.5-1.0 part; Heat stabilizer 1.5-2.5 parts; Lubricant 0.2-0.5 parts; The total weight of the seawater degradable resin and the polylactic acid-glycolic acid copolymer is 100 parts.

[0019] Furthermore, the plasticizer is glycolate.

[0020] Another object of the present invention is to provide a method for preparing a seawater-degradable injection molding material, comprising the following steps: S31, mixing, i.e. Place all raw materials in a mixer according to the formula and mix them evenly; S32, granulation, i.e. The material is put into a granulating unit, extruded and pelletized at 120-140° C. to obtain the seawater-degradable injection molding material.

[0021] Beneficial effects of the present invention: (1) The present invention provides a seawater degradable injection molding material, the formula of which contains a self-made seawater degradable resin, and is a novel random block polyester resin prepared with 1,4-butanediol, dimethyl carbonate, lactic acid, glycolic acid, terephthalic acid, oxalic acid, and low molecular weight polyethylene glycol as raw materials. First, the polyester molecular chain with 1,4-butanediol and dimethyl carbonate as the main structure has excellent flexibility and excellent fluidity, and can be used in the injection molding process; second, the lactate ester and glycolate ester structures are easily hydrolyzed structural units, which can effectively improve the degradability of the material in seawater; in addition, the density of the ester group can be increased, and the thermal and mechanical properties of the material can be improved; third, the terephthalate ester structure can absorb UV light on the one hand and promote the photodegradation of the material; on the other hand, as a hard segment, it can improve the thermal and mechanical properties of the material; fourth, the oxalate ester structure has non-enzymatic degradation characteristics on the one hand, which is conducive to seawater degradation; on the other hand, it can increase the ester group density and improve the mechanical properties; fifth, the low molecular weight polyethylene glycol is water-soluble, which promotes the water solubility of the material and thus promotes the water degradation characteristics.

[0022] (2) The present invention provides a seawater-degradable injection molding material, the formula of which contains a self-made functional modifier, which is an additive with zeolite as a carrier and carboxylic acid iron and epoxy silane structures on the surface. First, zeolite is a porous structure that can effectively adsorb free carboxylic acid structures, which helps to improve the stability of the material and extend its service life; and during the degradation process, the release of free carboxylic acids will promote the degradation of the material, which has a certain degree of controllability; second, the porous structure of zeolite can effectively improve the water vapor and oxygen barrier properties of the material; third, the carboxylic acid iron structure has a photosensitizing effect, which can induce the polymer chain to form more secondary alkyl free radical structures, accelerating the oxidative degradation process; and it synergistically acts with the main resin to further promote the degradation of the material; fourth, the epoxy-modified zeolite structure has a large number of epoxy groups grafted on the surface, which has the effects of increasing capacity and extending the chain, and can improve the mechanical properties of the material.

[0023] (3) The present invention provides a seawater-degradable injection molding compound, which is rationally formulated by compounding a self-made seawater-degradable resin with a polylactic acid-glycolic acid copolymer. On the one hand, the processing window of the injection molding compound is improved; on the other hand, the initial degradation performance of the material can be promoted; in addition, other resins can be added to the injection molding compound for physical blending, which has the characteristics of flexibility in use.

[0024] (4) The present invention provides a method for preparing a seawater-degradable injection molding material, which is prepared using a conventional granulation process, is simple to operate, and is suitable for large-scale promotion and use. DETAILED DESCRIPTION

[0025] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.

[0026] The purpose of the present invention is to develop a seawater-degradable injection molding material to solve the defect of slow degradation in seawater of the degradable materials that are easy to be injection molded in the prior art. The design idea is: first, considering the excellent injection moldability of common polyester materials such as PBT and the excellent seawater degradation of polyglycolic acid structure; design a new polyester structure containing glycolate structure, that is, seawater-degradable resin; second, design a functional modifier with the functions of capacity expansion, chain extension and degradation promotion. The solution for the new polyester is: first, using 1,4-butanediol and dimethyl carbonate as the main raw materials; supplemented by terephthalic acid, oxalic acid, lactic acid, glycolic acid, polyethylene glycol and other raw materials, a polyester material with excellent degradation performance is synthesized. The solution for the functional modifier is: based on zeolite, iron ion modification and coordination with carboxylic acid, and modification and preparation with silane coupling agent. The theoretical basis for the realization is: first, for the seawater degradable resin, a multi-step esterification reaction is carried out to prepare hydroxyl-terminated intermediate products respectively; and an ester exchange reaction is carried out with dimethyl carbonate to obtain the target product; for the functional modifier, ion exchange is used to obtain a zeolite containing iron ions; and a modified zeolite containing hydroxyl groups is prepared by coordination with hydroxycarboxylic acid; and then a functional modifier containing an epoxy structure is prepared with an epoxy silane coupling agent. The above-mentioned self-made ingredients are added to the formula system for mixing and granulation processes, and the components work synergistically with each other, and the seawater degradation performance and mechanical properties of the effective material are improved. The embodiments of the present invention are as follows: The embodiment of the present invention provides a method for preparing a seawater-degradable resin, comprising the following steps: S11, under nitrogen protection, mix 1,4-butanediol and dimethyl carbonate, add catalyst A, stir, heat to 160-180°C, react for 1-3h, obtain intermediate product I, and divide it into two parts, namely intermediate product IA and intermediate product IB; set aside.

[0027] The molar ratio of 1,4-butanediol to dimethyl carbonate is 1.5-2.5:1.

[0028] The amount of the catalyst A is 0.05-0.2wt% of the total mass of the reactants; The catalyst A may be titanium glycolate, tetrabutyl titanate, tetraisopropyl titanate, etc., and tetrabutyl titanate is preferred.

[0029] S12, under nitrogen protection, after the intermediate product IB and the catalyst B are uniformly mixed, lactic acid and glycolic acid are mixed and then added dropwise, stirred, and the temperature is raised to 180-200°C for reaction. The reaction endpoint is determined by the disappearance of the carboxyl peak monitored by infrared, to obtain the intermediate product II.

[0030] The molar ratio of the intermediate product IB, lactic acid and glycolic acid is 1:0.4-0.6:1.4-1.8.

[0031] The amount of the catalyst B is 0.1-0.4wt% of the total mass of the reactants; The catalyst B may be antimony glycolate, antimony trioxide, antimony acetate, tetrabutyl titanate, titanium glycolate, n-butyl titanate or tetraisopropyl titanate; and preferably tetrabutyl titanate.

[0032] S13, under nitrogen protection, terephthalic acid, oxalic acid, polyethylene glycol, 1,4-butanediol, catalyst C and auxiliary agents are mixed, stirred, and heated to 180-200° C. for reaction for 3-5 hours to obtain intermediate product III.

[0033] The molar ratio of terephthalic acid, oxalic acid, polyethylene glycol and 1,4-butanediol is 0.3-0.5: 0.5-0.7: 1.5-2.0: 0.5-1.0; The amount of polyethylene glycol is 200-600.

[0034] The amount of the catalyst C is 0.1-0.4wt% of the total mass of the reactants; The catalyst C may be antimony glycolate, antimony trioxide, antimony acetate, tetrabutyl titanate, titanium glycolate, n-butyl titanate or tetraisopropyl titanate; and antimony trioxide is preferred.

[0035] The dosage of the auxiliary agent is 0.1-0.2wt%; The auxiliary agent may be phosphoric acid, phosphorous acid, trimethyl phosphate, triphenyl phosphate, triphenyl phosphite or trialkyl phosphite; and preferably triphenyl phosphate.

[0036] S14, under nitrogen protection, the intermediate product IA, the intermediate product II, the intermediate product III, dimethyl carbonate and the catalyst D are mixed, stirred, and heated to 200°C for reaction until no fraction is released; the temperature is raised to 220-250°C, the vacuum degree is 0.1 MPa, and the reaction is performed for 3-5 hours to obtain the target product, i.e., the seawater degradable resin.

[0037] The molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 1.0-1.2:0.2-0.3:0.1-0.2:1.0.

[0038] The amount of the catalyst D is 0.2-0.5wt% of the total mass of the reactants; The catalyst D may be antimony glycolate, antimony trioxide, antimony acetate, tetrabutyl titanate, titanium glycolate, n-butyl titanate or tetraisopropyl titanate; and preferably tetrabutyl titanate.

[0039] The seawater degradable resin in the present invention is made of 1,4-butanediol and dimethyl carbonate as main raw materials, supplemented with terephthalic acid, oxalic acid, lactic acid, glycolic acid, polyethylene glycol and other raw materials. In the synthesis process, by controlling the reaction ratio and the structure of the polymer, there are functional structural unit blocks such as glycolic acid (easy to hydrolyze), lactic acid (hydrolyzable), oxalic acid (non-enzymatic degradation), terephthalic acid (photolyzable) or polyethylene glycol (water-soluble and degradable) in the molecular chain structure, which can effectively ensure that the seawater degradable resin is absorbed by the marine environment. At the same time, functional structural units such as glycolic acid, lactic acid, oxalic acid, and terephthalic acid can effectively improve mechanical strength, melting point and other properties; polyethylene glycol can improve properties such as elongation at break.

[0040] The present invention also provides a method for preparing a functional modifier, comprising the following steps: S21, adding zeolite to a salt solution, reacting at 70-90° C. for 3-5 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking out insoluble matter, washing with deionized water A for 3 times, and drying at 90-100° C. for 2-4 hours to obtain modified zeolite I; The dosage ratio of the zeolite, salt solution and deionized water A is 10g:100-200mL:500mL; The salt solution is iron salt and has a concentration of 1.0-3.0 mol / L.

[0041] The iron salt is ferric chloride, ferric sulfate, ferric nitrate, etc.; and ferric chloride is preferred.

[0042] The mesh number of the zeolite is 250-2500 mesh; it can be 250 mesh, 270 mesh, 325 mesh, 425 mesh, 500 mesh, 625 mesh, 800 mesh, 1250 mesh, 2500 mesh, or a range value consisting of any two values.

[0043] The zeolite may be X-type zeolite, Y-type zeolite, chabazite, mordenite, L-type zeolite, P-type zeolite, etc.; and the zeolite described in the following embodiments of the present invention is Y-type zeolite.

[0044] S22, adding modified zeolite I to the organic ligand solution, stirring and shaking at 20-30° C. for 4-6 hours, filtering and taking out insoluble matter; washing with deionized water B for 3 times, and drying at 60° C. for 8 hours to obtain modified zeolite II; The usage ratio of the modified zeolite I, the organic ligand solution, and the deionized water B is 10 g: 100-300 mL: 500 mL; The concentration of the organic ligand solution is 1.0-3.0 mol / L.

[0045] The organic ligand is glycolic acid and / or other carboxylic acids; and the molar ratio of glycolic acid to other carboxylic acids is 0.6-1.0:0.4-0; The other carboxylic acids may be lactic acid, oxalic acid, terephthalic acid, benzoic acid, trimellitic acid, stearic acid, and the like.

[0046] S23, place the modified zeolite II in ethyl acetate A, ultrasonically disperse for 1 hour, add epoxy silane coupling agent and deionized water C, slowly heat to 60-80°C, heat and stir for 6-14 hours, after the reaction is completed, cool to room temperature, filter, wash with ethyl acetate B, and vacuum dry at 40°C to constant weight to obtain a functional modifier.

[0047] The usage ratio of the modified zeolite II, ethyl acetate A, epoxy silane coupling agent, deionized water C, and ethyl acetate B is: 1.00 g: 50 mL: 3.0-5.0 g: 0.6 g: 200 mL.

[0048] The epoxy silane coupling agent may be silane coupling agent KH560, silane coupling agent KH561, silane coupling agent KH577, silane coupling agent KH578, etc., and preferably silane coupling agent KH560.

[0049] Unless otherwise specified, the solvent of the organic ligand solution in the preparation method of the functional modifier described in the following examples of the present invention is water.

[0050] The functional modifier in the present invention carries a large amount of iron ions, which have high photosensitivity after being coordinated with carboxylic acid, and have an excellent accelerated oxidative degradation process after receiving UV light outdoors. The zeolite structure is a porous structure with a large specific surface area, which can amplify the efficacy of the iron ion complex and further promote degradation. In addition, carboxylic acid structures such as glycolic acid structures have the effect of promoting degradation, and epoxy structures have the effect of increasing capacity and extending chains, which can effectively improve physical properties such as tensile strength and melting point.

[0051] The embodiment of the present invention further provides a seawater-degradable injection molding material, comprising the following raw materials in parts by weight: 80-90 parts of seawater degradable resin; 10-20 parts of polylactic acid-glycolic acid copolymer; Functional modifier 3.0-5.0 parts; UV absorber 0.5-1.0 part; Antioxidant 0.2-0.5 parts; Anti-hydrolysis agent 0.3-0.8 parts; Plasticizer 0.5-1.0 part; Heat stabilizer 1.5-2.5 parts; Lubricant 0.2-0.5 parts; The total weight of the seawater degradable resin and the polylactic acid-glycolic acid copolymer is 100 parts.

[0052] The melting point of the polylactic acid-glycolic acid copolymer is 135-144°C, 196-202°C; and the preparation method of the polylactic acid-glycolic acid copolymer described in the following embodiments of the present invention is prepared according to the reference (He Feng, et al. Synthesis of polylactic acid-polyglycolic acid copolymer and study on its structure and properties, Synthetic Fiber Industry [J], 2016, 39(4): 42-44). m1 is 140.74℃; T m2 It is 199.83℃.

[0053] The polylactic acid-glycolic acid copolymer described in the present invention has two melting points due to random block copolymerization, and the molecular weight distribution is relatively wide. It is compounded with seawater degradable resin for use. During the injection molding process, due to the shearing effect of the screw in the injection molding machine, the polylactic acid part in the polylactic acid-glycolic acid copolymer is first melted, and then the seawater degradable resin is promoted to melt. Finally, in the process of macromolecular chain entanglement, the entire resin melts and flows, and a composite material with a certain melting range is selected, which is conducive to a larger injection molding window, reduces processing difficulty, and improves the yield rate of products. In addition, the polylactic acid-glycolic acid copolymer has excellent initial seawater degradation characteristics.

[0054] The UV absorber is a benzotriazole, specifically UV-326, UV-327, UV-328 or UV-329, etc. Moreover, in the following embodiments of the present invention, the UV absorber is UV-329.

[0055] The antioxidant is a hindered phenol; it can be antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant 2246, etc.; and the antioxidant described in the following embodiments of the present invention is antioxidant 1010.

[0056] The anti-hydrolysis agent is a monomeric anti-hydrolysis agent bis(2,6-diisopropylbenzene) carbodiimide, model number HyMax1010, purchased from Shanghai Langyi Functional Materials Co., Ltd.

[0057] The plasticizer is a glycolate, specifically methyl glycolate, ethyl glycolate, propyl glycolate or butyl glycolate, etc., and preferably ethyl glycolate.

[0058] The heat stabilizer is a calcium zinc stabilizer, specifically calcium stearate, zinc stearate, and hydrotalcite mixed in a mass ratio of 2:2:1.

[0059] The lubricant is EBS, stearamide, oleamide or erucamide, and the lubricant in the following embodiments of the present invention is EBS.

[0060] The embodiment of the present invention also provides a method for preparing a seawater-degradable injection molding material, comprising the following steps: S31, mixing, i.e. Place all raw materials in a mixer according to the formula and mix them evenly; S32, granulation, i.e. The material is put into a granulating unit, extruded and pelletized at 120-140° C. to obtain the seawater-degradable injection molding material.

[0061] In order to further understand the present invention, a seawater-degradable injection molding material provided by the present invention is described in detail below in conjunction with specific embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0062] A method for preparing a seawater-degradable resin comprises the following steps: S11, under nitrogen protection, mix 1,4-butanediol and dimethyl carbonate, add tetrabutyl titanate, stir, heat to 170°C, react for 2h, obtain intermediate product I, and divide it into two parts, namely intermediate product IA and intermediate product IB; set aside.

[0063] The molar ratio of 1,4-butanediol to dimethyl carbonate is 2.0:1.

[0064] The amount of tetrabutyl titanate used is 0.1wt% of the total mass of the reactants.

[0065] Its infrared data are as follows: 3384 cm -1 :-OH exists and weakens; 1732cm -1 :-C=O exists; 1255 cm -1 、1110cm -1 :-COC- exists.

[0066] Its NMR data are as follows ( 1 H NMR, CDCl 3 as solvent, TMS as internal standard, δppm): 4.20 (-CH 2 -, 4H); 3.72 (-CH 2 -, 4H); 1.85 (-CH 2 -, 4H); 1.22 (-OH, 2H).

[0067] S12, under nitrogen protection, the intermediate product IB and tetrabutyl titanate are uniformly mixed, lactic acid and glycolic acid are mixed and then added dropwise, stirred, and the temperature is raised to 190°C for reaction. The reaction endpoint is determined by the disappearance of the carboxyl peak monitored by infrared, to obtain the intermediate product II.

[0068] The molar ratio of the intermediate product IB, lactic acid and glycolic acid is 1:0.5:1.6.

[0069] The amount of tetrabutyl titanate used is 0.2 wt % of the total mass of the reactants.

[0070] Its infrared data are as follows: 3384 cm -1 :-OH exists; 1732cm -1 :-C=O (ester group) exists; 1255 cm -1 、1110cm -1 :-COC- exists; 1760 cm -1 、1710cm -1 :-C=O (carboxyl) does not exist.

[0071] S13, under nitrogen protection, terephthalic acid, oxalic acid, polyethylene glycol, 1,4-butanediol, antimony trioxide and triphenyl phosphate were mixed, stirred, and heated to 190° C. for 4 h to obtain an intermediate product III.

[0072] The molar ratio of terephthalic acid, oxalic acid, polyethylene glycol and 1,4-butanediol is 0.4:0.6:1.7:0.8; The weight of the polyethylene glycol is 400.

[0073] The amount of antimony trioxide used is 0.2wt% of the total mass of the reactants.

[0074] The amount of triphenyl phosphate used is 0.15wt%.

[0075] Its infrared data are as follows: 3379 cm -1 :-OH exists; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists; 1255 cm -1 、1110cm -1 :-COC- exists; 1760 cm -1 、1710cm -1 :-C=O (carboxyl) does not exist.

[0076] S14, under nitrogen protection, the intermediate product IA, the intermediate product II, the intermediate product III, dimethyl carbonate and tetrabutyl titanate were mixed, stirred, and heated to 200°C to react until no fraction was removed; the temperature was raised to 240°C, the vacuum degree was 0.1 MPa, and the reaction was carried out for 3.5 hours to obtain the target product, namely, seawater degradable resin ( ).

[0077] The molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 1.1:0.25:0.15:1.0.

[0078] The amount of tetrabutyl titanate used is 0.4wt% of the total mass of the reactants.

[0079] Its infrared data are as follows: 3379 cm -1 :-OH does not exist; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1255 cm -1 、1110cm -1 :-COC- exists.

[0080] A method for preparing a functional modifier comprises the following steps: S21, adding zeolite to ferric chloride solution, reacting at 80°C for 3.5 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking insoluble matter, washing with deionized water A for 3 times, and drying at 95°C for 3 hours to obtain modified zeolite I; The usage ratio of the zeolite, ferric chloride solution and deionized water A is 10 g: 150 mL: 500 mL; The concentration of the ferric chloride solution is 2.0 mol / L.

[0081] The mesh number of the zeolite is 1250 mesh.

[0082] Its infrared data is as follows: 3441cm -1 : -OH broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 604 cm -1 :Fe-O exists.

[0083] S22, adding modified zeolite I to the organic ligand solution, stirring and shaking at 25°C for 5 hours, filtering and taking insoluble matter; washing with deionized water B for 3 times, and drying at 60°C for 8 hours to obtain modified zeolite II; The usage ratio of the modified zeolite I, the organic ligand solution, and the deionized water B is 10 g: 200 mL: 500 mL; The concentration of the organic ligand solution is 2.0 mol / L.

[0084] The organic ligand is glycolic acid and lactic acid added in a molar ratio of 0.8:0.2.

[0085] Its infrared data are as follows: 3400-3500cm -1 : -OH broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 604 cm -1 :Fe-O exists; 1674 cm -1 :-C=O (coordinated with iron ions) exists.

[0086] S23, place the modified zeolite II in ethyl acetate A, ultrasonically disperse for 1 hour, add silane coupling agent KH560 and deionized water C, slowly heat to 70°C, heat and stir for 9 hours, after the reaction is completed, cool to room temperature, filter, wash with ethyl acetate B, and vacuum dry at 40°C to constant weight to obtain a functional modifier.

[0087] The usage ratio of the modified zeolite II, ethyl acetate A, silane coupling agent KH560, deionized water C, and ethyl acetate B is: 1.00 g: 50 mL: 4.0 g: 0.6 g: 200 mL.

[0088] Its infrared data are as follows: 3440cm -1 : -OH broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 604 cm -1 :Fe-O exists; 1674 cm -1 :-C=O (coordinated with iron ion) exists; 1265cm -1 、938cm -1 、825cm -1 : Epoxy group exists.

[0089] A seawater-degradable injection molding material comprises the following raw materials in parts by weight: 85 parts of seawater degradable resin; 15 parts of polylactic acid-glycolic acid copolymer; Functional modifier 4.0 parts; 0.8 parts of UV absorber; 0.3 parts of antioxidant; 0.5 part of anti-hydrolysis agent; Ethyl glycolate 0.7 parts; 2.0 parts of heat stabilizer; 0.3 parts of lubricant.

[0090] A method for preparing a seawater-degradable injection molding material comprises the following steps: S31, mixing, i.e. Place all raw materials in a high-speed mixer according to the formula, stir at 200 rpm for 25 min, and mix evenly.

[0091] S32, granulation, i.e. The mixture was put into a granulating unit, and the temperatures of zone 1, zone 2, zone 3 and die head were set at 120°C, 130°C, 140°C, extrusion, water cooling, pelletizing and drying at 50°C were performed to obtain the seawater-degradable injection molding material.

[0092] The twin-screw extruder in the granulator unit is a universal screw with a length-to-diameter ratio of 36:1, a screw speed of 200 rpm, and a pelletizer speed of 250 rpm.

[0093] The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin comprises the following steps: S11, under nitrogen protection, mix 1,4-butanediol and dimethyl carbonate, add tetrabutyl titanate, stir, heat to 160°C, react for 3h, obtain intermediate product I, and divide it into two parts, namely intermediate product IA and intermediate product IB; set aside.

[0094] The molar ratio of 1,4-butanediol to dimethyl carbonate is 2.5:1.

[0095] The amount of tetrabutyl titanate used is 0.2 wt % of the total mass of the reactants.

[0096] Its infrared data are as follows: 3384 cm -1 :-OH exists and weakens; 1732cm -1 :-C=O exists; 1255 cm -1 、1110cm -1 :-COC- exists.

[0097] Its NMR data are as follows ( 1 H NMR, CDCl 3 as solvent, TMS as internal standard, δppm): 4.20 (-CH 2 -, 8H); 3.72 (-CH 2 -, 12H); 1.85 (-CH 2 -, 4H); 1.74 (-CH 2 -, 16H); 1.31 (-OH, 2H); 2.03 (-OH, 4H).

[0098] S12, under nitrogen protection, the intermediate product IB and tetrabutyl titanate are uniformly mixed, lactic acid and glycolic acid are mixed and then added dropwise, stirred, and the temperature is raised to 180°C for reaction. The reaction endpoint is determined by the disappearance of the carboxyl peak monitored by infrared, to obtain the intermediate product II.

[0099] The molar ratio of the intermediate product IB, lactic acid and glycolic acid is 1:0.5:1.6.

[0100] The amount of tetrabutyl titanate used is 0.4wt% of the total mass of the reactants.

[0101] Its infrared data are as follows: 3384 cm -1 :-OH exists; 1732cm -1 :-C=O (ester group) exists; 1255 cm -1 、1110cm -1 :-COC- exists; 1760 cm -1 、1710cm -1 :-C=O (carboxyl) does not exist.

[0102] S13, under nitrogen protection, terephthalic acid, oxalic acid, polyethylene glycol, 1,4-butanediol, antimony trioxide and triphenyl phosphate are mixed, stirred, and heated to 180° C. for reaction for 5 h to obtain an intermediate product III.

[0103] The molar ratio of terephthalic acid, oxalic acid, polyethylene glycol and 1,4-butanediol is 0.4:0.6:1.7:0.8; The weight of the polyethylene glycol is 400.

[0104] The amount of antimony trioxide used is 0.4wt% of the total mass of the reactants.

[0105] The amount of triphenyl phosphate used is 0.2wt%.

[0106] Its infrared data are as follows: 3379 cm -1 :-OH exists; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists; 1255 cm -1 、1110cm -1 :-COC- exists; 1760 cm -1 、1710cm -1 :-C=O (carboxyl) does not exist.

[0107] S14, under nitrogen protection, the intermediate product IA, the intermediate product II, the intermediate product III, dimethyl carbonate and tetrabutyl titanate were mixed, stirred, and heated to 200°C to react until no fraction was removed; the temperature was raised to 220°C, the vacuum degree was 0.1 MPa, and the reaction was performed for 5 hours to obtain the target product, i.e., seawater degradable resin ( ).

[0108] The molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 1.1:0.25:0.15:1.0.

[0109] The amount of tetrabutyl titanate used is 0.5wt% of the total mass of the reactants.

[0110] Its infrared data are as follows: 3379 cm -1 :-OH does not exist; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1255 cm -1 、1110cm -1 :-COC- exists.

[0111] The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin comprises the following steps: S11, under nitrogen protection, mix 1,4-butanediol and dimethyl carbonate, add tetrabutyl titanate, stir, heat to 180°C, react for 1 hour, obtain intermediate product I, and divide it into two parts, namely intermediate product IA and intermediate product IB; set aside.

[0112] The molar ratio of 1,4-butanediol to dimethyl carbonate is 1.5:1.

[0113] The amount of tetrabutyl titanate used is 0.05wt% of the total mass of the reactants.

[0114] Its infrared data are as follows: 3384 cm -1 :-OH exists and weakens; 1732cm -1 :-C=O exists; 1255 cm -1 、1110cm -1 :-COC- exists.

[0115] Its NMR data are as follows ( 1 H NMR, CDCl 3 as solvent, TMS as internal standard, δppm): 4.20 (-CH 2-, 8H); 3.72 (-CH 2 -, 4H); 1.85 (-CH 2 -, 4H); 1.74 (-CH 2 -, 8H); 1.31 (-OH, 2H).

[0116] S12, under nitrogen protection, the intermediate product IB and tetrabutyl titanate are uniformly mixed, lactic acid and glycolic acid are mixed and then added dropwise, stirred, and the temperature is raised to 200°C for reaction. The reaction endpoint is determined by the disappearance of the carboxyl peak monitored by infrared, to obtain the intermediate product II.

[0117] The molar ratio of the intermediate product IB, lactic acid and glycolic acid is 1:0.5:1.6.

[0118] The amount of tetrabutyl titanate used is 0.1wt% of the total mass of the reactants.

[0119] Its infrared data are as follows: 3384 cm -1 :-OH exists; 1732cm -1 :-C=O (ester group) exists; 1255 cm -1 、1110cm -1 :-COC- exists; 1760 cm -1 、1710cm -1 :-C=O (carboxyl) does not exist.

[0120] S13, under nitrogen protection, terephthalic acid, oxalic acid, polyethylene glycol, 1,4-butanediol, antimony trioxide and triphenyl phosphate are mixed, stirred, and heated to 200° C. for reaction for 3 h to obtain an intermediate product III.

[0121] The molar ratio of terephthalic acid, oxalic acid, polyethylene glycol and 1,4-butanediol is 0.4:0.6:1.7:0.8; The weight of the polyethylene glycol is 400.

[0122] The amount of antimony trioxide used is 0.1wt% of the total mass of the reactants.

[0123] The amount of triphenyl phosphate used is 0.1 wt %.

[0124] Its infrared data are as follows: 3379 cm -1 :-OH exists; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists; 1255 cm -1 、1110cm -1:-COC- exists; 1760 cm -1 、1710cm -1 :-C=O (carboxyl) does not exist.

[0125] S14, under nitrogen protection, the intermediate product IA, the intermediate product II, the intermediate product III, dimethyl carbonate and tetrabutyl titanate were mixed, stirred, and heated to 200°C to react until no fraction was removed; the temperature was raised to 250°C, the vacuum degree was 0.1 MPa, and the reaction was carried out for 3 hours to obtain the target product, i.e., seawater degradable resin ( ).

[0126] The molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 1.1:0.25:0.15:1.0.

[0127] The amount of tetrabutyl titanate used is 0.2 wt % of the total mass of the reactants.

[0128] Its infrared data are as follows: 3379 cm -1 :-OH does not exist; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1255 cm -1 、1110cm -1 :-COC- exists.

[0129] The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S12, The molar ratio of the intermediate product IB, lactic acid and glycolic acid is 1:0.6:1.4.

[0130] The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S12, The molar ratio of the intermediate product IB, lactic acid and glycolic acid is 1:0.4:1.8.

[0131] The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S13, The molar ratio of terephthalic acid, oxalic acid, polyethylene glycol and 1,4-butanediol is 0.3:0.7:2.0:0.5; and The weight of the polyethylene glycol is 200.

[0132] The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S13, The molar ratio of terephthalic acid, oxalic acid, polyethylene glycol and 1,4-butanediol is 0.5:0.5:1.5:1.0; and The weight of the polyethylene glycol is 600.

[0133] The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S14, The molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 1.0:0.3:0.2:1.0.

[0134] The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S14, The molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 1.2:0.2:0.1:1.0.

[0135] The rest is the same as in Example 1, except that: A method for preparing a functional modifier comprises the following steps: S21, adding zeolite to ferric chloride solution, reacting at 70°C for 5 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking insoluble matter, washing with deionized water A for 3 times, and drying at 90°C for 4 hours to obtain modified zeolite I; The usage ratio of the zeolite, ferric chloride solution and deionized water A is 10 g: 100 mL: 500 mL; The concentration of the ferric chloride solution is 3.0 mol / L.

[0136] The mesh number of the zeolite is 2500 mesh.

[0137] Its infrared data is as follows: 3441cm -1 : -OH broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 604 cm -1 :Fe-O exists.

[0138] S22, adding modified zeolite I to the organic ligand solution, stirring and shaking at 20°C for 6 hours, filtering and taking insoluble matter; washing with deionized water B for 3 times, and drying at 60°C for 8 hours to obtain modified zeolite II; The usage ratio of the modified zeolite I, the organic ligand solution, and the deionized water B is 10 g: 200 mL: 500 mL; The concentration of the organic ligand solution is 2.0 mol / L.

[0139] The organic ligand is glycolic acid and lactic acid added in a molar ratio of 0.8:0.2.

[0140] Its infrared data are as follows: 3400-3500cm -1 : -OH broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 604 cm -1 :Fe-O exists; 1674 cm -1 :-C=O (coordinated with iron ions) exists.

[0141] S23, place the modified zeolite II in ethyl acetate A, ultrasonically disperse for 1 hour, add silane coupling agent KH560 and deionized water C, slowly heat to 60°C, heat and stir for 14 hours, after the reaction is completed, cool to room temperature, filter, wash with ethyl acetate B, and vacuum dry at 40°C to constant weight to obtain a functional modifier.

[0142] The usage ratio of the modified zeolite II, ethyl acetate A, silane coupling agent KH560, deionized water C, and ethyl acetate B is: 1.00 g: 50 mL: 5.0 g: 0.6 g: 200 mL.

[0143] Its infrared data are as follows: 3440cm -1 : -OH broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 604 cm -1 :Fe-O exists; 1674 cm -1 :-C=O (coordinated with iron ion) exists; 1265cm -1 、938cm -1 、825cm -1 : Epoxy group exists.

[0144] The rest is the same as in Example 1, except that: A method for preparing a functional modifier comprises the following steps: S21, adding zeolite to ferric chloride solution, reacting at 90°C for 3 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking insoluble matter, washing with deionized water A for 3 times, and drying at 100°C for 2 hours to obtain modified zeolite I; The usage ratio of the zeolite, ferric chloride solution and deionized water A is 10 g: 200 mL: 500 mL; The concentration of the ferric chloride solution is 1.0 mol / L.

[0145] The mesh number of the zeolite is 1250 mesh.

[0146] Its infrared data is as follows: 3441cm -1 : -OH broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 604 cm -1 :Fe-O exists.

[0147] S22, adding modified zeolite I to the organic ligand solution, stirring and shaking at 30°C for 4 hours, filtering and taking insoluble matter; washing with deionized water B for 3 times, and drying at 60°C for 8 hours to obtain modified zeolite II; The usage ratio of the modified zeolite I, the organic ligand solution, and the deionized water B is 10 g: 200 mL: 500 mL; The concentration of the organic ligand solution is 2.0 mol / L.

[0148] The organic ligand is glycolic acid and lactic acid added in a molar ratio of 0.8:0.2.

[0149] Its infrared data are as follows: 3400-3500cm -1 : -OH broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 604 cm -1 :Fe-O exists; 1674 cm -1 :-C=O (coordinated with iron ions) exists.

[0150] S23, place the modified zeolite II in ethyl acetate A, ultrasonically disperse for 1 hour, add silane coupling agent KH560 and deionized water C, slowly heat to 80°C, heat and stir for 6 hours, after the reaction is completed, cool to room temperature, filter, wash with ethyl acetate B, and vacuum dry at 40°C to constant weight to obtain a functional modifier.

[0151] The usage ratio of the modified zeolite II, ethyl acetate A, silane coupling agent KH560, deionized water C, and ethyl acetate B is: 1.00 g: 50 mL: 3.0 g: 0.6 g: 200 mL.

[0152] Its infrared data are as follows: 3440cm -1 : -OH broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 604 cm -1 :Fe-O exists; 1674 cm -1 :-C=O (coordinated with iron ion) exists; 1265cm -1 、938cm -1 、825cm -1 : Epoxy group exists.

[0153] The rest is the same as in Example 1, except that: A method for preparing a functional modifier, wherein in S22, The usage ratio of the modified zeolite I, the organic ligand solution, and the deionized water B is 10 g: 100 mL: 500 mL; The concentration of the organic ligand solution is 3.0 mol / L.

[0154] The organic ligand is glycolic acid and lactic acid added in a molar ratio of 1.0:0, that is, no lactic acid is added.

[0155] The rest is the same as in Example 1, except that: A method for preparing a functional modifier, wherein in S22, The usage ratio of the modified zeolite I, the organic ligand solution, and the deionized water B is 10 g: 300 mL: 500 mL; The concentration of the organic ligand solution is 1.0 mol / L.

[0156] The organic ligand is glycolic acid and lactic acid added in a molar ratio of 0.6:0.4.

[0157] The rest is the same as in Example 1, except that: A method for preparing a functional modifier, wherein in S22, The organic ligand is glycolic acid and oxalic acid added in a molar ratio of 0.8:0.2.

[0158] The rest is the same as in Example 1, except that: A method for preparing a functional modifier, wherein in S22, The organic ligand is glycolic acid and benzoic acid added in a molar ratio of 0.8:0.2.

[0159] The rest is the same as in Example 1, except that: A seawater-degradable injection molding material comprises the following raw materials in parts by weight: 80 parts of seawater degradable resin; 20 parts of polylactic acid-glycolic acid copolymer; Functional modifier 5.0 parts; 0.5 parts of UV absorber; 0.5 parts of antioxidant; 0.3 parts of anti-hydrolysis agent; 1.0 part of ethyl glycolate; 1.5 parts of heat stabilizer; 0.5 parts of lubricant.

[0160] A method for preparing a seawater-degradable injection molding material comprises the following steps: S31, mixing, i.e. Place all raw materials in a high-speed mixer according to the formula, stir at 200 rpm for 25 min, and mix evenly.

[0161] S32, granulation, i.e. The mixture was put into a granulating machine, and the temperatures of zone 1, zone 2, zone 3 and zone 3 were set at 125°C, 132°C, 140°C and the die head were set at 140°C. The mixture was extruded, water-cooled, pelletized and dried at 50°C to obtain the seawater-degradable injection molding material.

[0162] The twin-screw extruder in the granulator unit is a universal screw with a length-to-diameter ratio of 36:1, a screw speed of 220 rpm, and a pelletizer speed of 280 rpm.

[0163] The rest is the same as in Example 1, except that: A seawater-degradable injection molding material comprises the following raw materials in parts by weight: 90 parts of seawater degradable resin; 10 parts of polylactic acid-glycolic acid copolymer; 3.0 parts of functional modifier; 1.0 part of UV absorber; 0.2 parts of antioxidant; 0.8 part of anti-hydrolysis agent; 0.5 parts of ethyl glycolate; 2.5 parts of heat stabilizer; 0.2 parts of lubricant.

[0164] A method for preparing a seawater-degradable injection molding material comprises the following steps: S31, mixing, i.e. Place all raw materials in a high-speed mixer according to the formula, stir at 200 rpm for 25 min, and mix evenly.

[0165] S32, granulation, i.e. The mixture was put into a granulating unit, and the temperatures of zone 1, zone 2, zone 3 and die head were set at 120°C, 128°C, 135°C, and extrusion, water cooling, pelletizing, and drying at 50°C were performed to obtain the seawater-degradable injection molding material.

[0166] The twin-screw extruder in the granulator unit is a universal screw with a length-to-diameter ratio of 36:1, a screw speed of 175 rpm, and a pelletizer speed of 210 rpm.

[0167] The following comparative examples are compared with specific embodiment 1: Comparative Example 1 The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S14, The molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 0:0.75:0.45:1.0; that is, the intermediate product IA is not added.

[0168] Comparative Example 2 The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S14, The molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 1.35:0:0.15:1.0; that is, the intermediate product II is not added.

[0169] Comparative Example 3 The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S12, The molar ratio of the intermediate product IB, lactic acid and glycolic acid is 1:2.1:0; that is, no glycolic acid is added.

[0170] Comparative Example 4 The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S14, The molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 1.25:0.25:0:1.0; that is, the intermediate product III is not added.

[0171] Comparative Example 5 The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S13, The molar ratio of terephthalic acid, oxalic acid, polyethylene glycol and 1,4-butanediol is 1.0:0:1.7:0.8; that is, no oxalic acid is added.

[0172] Comparative Example 6 The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S13, The molar ratio of terephthalic acid, oxalic acid, polyethylene glycol and 1,4-butanediol is 0:1.0:1.7:0.8, that is, no terephthalic acid is added.

[0173] Comparative Example 7 The rest is the same as in Example 1, except that: A method for preparing a seawater-degradable resin, wherein in S13, The molar ratio of terephthalic acid, oxalic acid, polyethylene glycol and 1,4-butanediol is 0.4:0.6:0:2.5; that is, polyethylene glycol is not added.

[0174] Comparative Example 8 The rest is the same as in Example 1, except that: A seawater-degradable injection molding compound is formulated without adding a functional modifier.

[0175] Comparative Example 9 The rest is the same as in Example 1, except that: A method for preparing a functional modifier, wherein in S21, The ferric chloride solution was replaced with calcium chloride solution.

[0176] Comparative Example 10 The rest is the same as in Example 1, except that: The preparation method of a functional modifier is the same as that of modified zeolite I.

[0177] Comparative Example 11 The rest is the same as in Example 1, except that: A method for preparing a functional modifier, wherein in S22, The organic ligand is glycolic acid and lactic acid added in a molar ratio of 0:1.0; that is, glycolic acid is not added.

[0178] Comparative Example 12 The rest is the same as in Example 1, except that: The preparation method of a functional modifier is the same as that of modified zeolite II.

[0179] Comparative Example 13 The rest is the same as in Example 1, except that: A seawater-degradable injection molding compound is formulated without adding polylactic acid-glycolic acid copolymer.

[0180] Comparative Example 14 The rest is the same as in Example 1, except that: A seawater-degradable injection molding compound is formulated without the addition of ethyl glycolate.

[0181] The injection molding materials prepared in the above embodiments and comparative examples were subjected to injection molding at injection temperatures of 120° C., 130° C., 136° C., 143° C., and 148° C.; the mold temperature was 40° C., the injection time was 10 s, the injection pressure was 800 Pa, and the holding time was 15 s.

[0182] The results of measuring the physical properties of the seawater-degradable injection molding materials in the embodiments of the present invention and the comparative examples are shown in Table 1.

[0183] Table 1 Physical properties test of each embodiment Firstly, it can be concluded from Examples 1-17 in Table 1 that the seawater-degradable injection molding material of the present invention has excellent mechanical properties and seawater degradation ability.

[0184] Second, it can be observed from Example 1 and Comparative Examples 1-7 that the seawater degradable injection molding material of the present invention uses a self-made seawater degradable resin as the main raw material, the polymer of dimethyl carbonate and butanediol has excellent flexibility; lactic acid ester and glycolic acid ester have excellent seawater degradability; terephthalic acid, oxalic acid, polyethylene glycol, etc. all have a promoting effect on seawater degradability; and the chemical structures act synergistically with each other, so that the main resin has excellent mechanical properties and excellent seawater degradability; It can be observed from Example 1 and Comparative Examples 8-12 that the self-made functional modifier in the seawater degradable injection molding material of the present invention has the effects of promoting degradation, increasing capacity and extending the chain, and has a promoting effect on improving mechanical properties and seawater degradability; It can be observed from Example 1 and Comparative Examples 13-14 that in the seawater-degradable injection molding compound of the present invention, the polylactic acid-glycolic acid copolymer has significantly improved initial seawater degradability and also has excellent mechanical properties.

[0185] In summary, the seawater-degradable injection molding compound provided by the present invention, on the one hand, is a self-made seawater-degradable resin and a functional modifier through molecular design; and the seawater-degradable resin and the functional modifier act synergistically on mechanical properties and seawater degradation properties; on the other hand, the comprehensive performance of the injection molding compound is significantly improved through formula design.

[0186] The test method is as follows: (1) Appearance: Visually inspect the molded parts to see if there is color difference, deformation, water marks, or weld marks; whether the surface is smooth and has burrs. If there are no such defects, it is marked as "OK".

[0187] (2) T m : DSC was used for testing, with a heating rate of 20°C / min and a nitrogen atmosphere.

[0188] (3) Vicat softening temperature: tested using the A120 method as described in GB / T 1633-2000.

[0189] (4) Mechanical properties: Tested according to the method described in GB / T 1040.3-2006.

[0190] (5) Weight loss rate of seawater degradation: The prepared samples were cut into 2×2×0.2 cm 3 The slices were labeled and weighed, then placed in 3.5% simulated seawater and degraded under light for a period of time; samples were collected regularly, the sample surface was cleaned with deionized water, and then dried to constant weight in a vacuum oven at 48±2℃, taken out, dried, weighed, and the residual weight ratio was calculated.

[0191] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a seawater-degradable resin, characterized in that: The following steps are involved: S11, subjecting 1,4-butanediol and dimethyl carbonate to an ester exchange reaction to obtain an intermediate product IA and an intermediate product IB; S12, mixing the intermediate product IB, lactic acid and glycolic acid for pre-polycondensation reaction to obtain an intermediate product II; S13, performing a pre-polycondensation reaction on terephthalic acid, oxalic acid, polyethylene glycol, and 1,4-butanediol to obtain an intermediate product III; S14, subjecting the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate to an ester exchange reaction to obtain a target product, namely, a seawater degradable resin.

2. The preparation method according to claim 1, characterized in that: The molar ratio of 1,4-butanediol to dimethyl carbonate is 1.5-2.5:1; The molar ratio of the intermediate product IB, lactic acid and glycolic acid is 1:0.4-0.6:1.4-1.8; The molar ratio of terephthalic acid, oxalic acid, polyethylene glycol and 1,4-butanediol is 0.3-0.5:0.5-0.7:1.5-2.0:0.5-1.0; and The amount of polyethylene glycol is 200-600.

3. The preparation method according to claim 1, characterized in that: The molar ratio of the intermediate product IA, the intermediate product II, the intermediate product III and dimethyl carbonate is 1.0-1.2:0.2-0.3:0.1-0.2:1.

0.

4. A seawater degradable resin, characterized in that: Prepared by the preparation method according to any one of claims 1 to 3.

5. A method for preparing a functional modifier, characterized in that: The following steps are involved: S21, adding zeolite into a salt solution to carry out an ion exchange reaction to obtain a modified zeolite I; S22, performing coordination reaction on the modified zeolite I and the organic ligand to obtain modified zeolite II; S23, performing a silylation coupling reaction on the modified zeolite II and the epoxy silane coupling agent to obtain a functional modifier.

6. The preparation method according to claim 5, characterized in that: The dosage ratio of the zeolite and the salt solution is 10 g: 100-200 mL; and The mesh number of the zeolite is 250-2500 mesh; The salt solution is iron salt and has a concentration of 1.0-3.0 mol / L; The modified zeolite I and the organic ligand solution are used in a ratio of 10 g: 100-300 mL; and The organic ligand concentration is 1.0-3.0 mol / L; The organic ligand is glycolic acid and / or other carboxylic acids; The usage ratio of the modified zeolite II and the epoxy silane coupling agent is 1g:3.0-5.0g.

7. A functional modifier, characterized in that: Prepared by the preparation method according to any one of claims 7 to 10.

8. A seawater-degradable injection molding material, characterized in that: The invention comprises the following raw materials in parts by weight: 80-90 parts of seawater degradable resin; 10-20 parts of polylactic acid-glycolic acid copolymer; Functional modifier 3.0-5.0 parts; UV absorber 0.5-1.0 part; Antioxidant 0.2-0.5 parts; Anti-hydrolysis agent 0.3-0.8 parts; Plasticizer 0.5-1.0 part; Heat stabilizer 1.5-2.5 parts; Lubricant 0.2-0.5 parts; The total weight of the seawater degradable resin and the polylactic acid-glycolic acid copolymer is 100 parts.

9. The seawater-degradable injection molding material according to claim 11, characterized in that: The plasticizer is glycolate.

10. A method for preparing a seawater-degradable injection molding material, characterized in that: The steps include: S31, mixing, i.e. Place all raw materials in a mixer according to the formula and mix them evenly; S32, granulation, i.e. The material is put into a granulating unit, extruded and pelletized at 120-140° C. to obtain the seawater-degradable injection molding material.

Citation Information

Patent Citations

  • Seawater degradation composite material and preparation method thereof

    CN112625414A

  • Preparation method of high-molecular-weight poly(hexanediol oxalate)

    CN113527644A

  • Hydrolyzable copolyester, preparation method therefor, and application thereof

    WO2020156346A1