Modified polyether polyol, preparation method thereof and polyurethane foam material
By reacting polyoxyalkylene polyether polyol with cyclic anhydride and carbonate, a modified polyether polyol with high primary hydroxyl content and low EO content was prepared, which solved the problem of performance degradation caused by the increase in primary hydroxyl content in the prior art. , realizes the excellent performance of polyurethane foam and the green and environmental protection of the process.
Patent Information
- Application Number
- CN202411182746.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The prior art is difficult to improve the primary hydroxyl content without reducing the hydrolysis resistance and humidity and heat aging properties of polyether polyols, and the catalyst is costly, toxic by-products and safety hazards.
By reacting polyoxyalkylene polyether polyol with cyclic acid anhydride and then reacting with cyclic carbonate, a modified polyether polyol with a primary hydroxyl content of more than 90% was prepared, with an EO content of less than 5%, and in a polyurethane foam material It is used in the process of using ethylene oxide and three waste emissions.
It realizes the preparation of low EO content of polyether polyols with high primary hydroxyl content, improves the elasticity, feel and mechanical properties of polyurethane foam, meets the lightweight, low odor and low VOC requirements of the automotive industry, and is safer and more environmentally friendly. .
Smart Images

Figure BDA0005012676320000031 
Figure BDA0005012676320000101 
Figure BDA0005012676320000111
Abstract
Description
Technical Field
[0001] The present invention relates to the synthesis of a modified polyether polyol and its application, and more specifically, the present invention relates to the synthesis of a modified polyether polyol with a high primary hydroxyl content and its application in polyurethane flexible foam. Background Art
[0002] Ordinary polyether polyols have a series of problems such as low molecular weight, high unsaturation and insufficient activity, which lead to poor product quality and application performance, limiting the application of PPG. When the relative molecular mass of PPG is high, the number of hydroxyl groups decreases, and the relative content of primary hydroxyl groups must be increased to improve the reactivity of the product. Polyether polyols with high primary hydroxyl content, i.e. highly active polyethers, can shorten the aging time during foaming, and the products made from them have high elasticity, energy absorption and high load-bearing capacity.
[0003] In the prior art, high-activity polyethers are generally prepared using alkaline compound catalysts. First, an initiator is reacted with PO. After the molecular weight is increased to a certain level, EO is added to cap the end. Alternatively, in the presence of a double metal cyanide catalyst (DMC bimetallic catalyst), an initiator is reacted with PO to prepare polyoxypropylene polyol, and then an alkali metal hydroxide is added to passivate the DMC bimetallic catalyst, and then EO is used to cap the end, such as JP1990294319A.
[0004] In the prior art, the primary hydroxyl content of polyether polyols is generally around 60-85%. If the primary hydroxyl content is to be further increased, the EO / PO ratio needs to be increased, resulting in an increase in the EO segments in the polyether polyols (as is known in the industry, the EO segments in the polyether molecules specifically refer to the polyethylene glycol segments, and the EO content in the polyether polyol molecules refers to the polyethylene glycol segment content, molar ratio or mass ratio), which reduces the hydrolysis resistance and wet heat aging performance of the polyether polyols and the polyurethane materials made therefrom. To solve this problem, CN102549043B discloses a method for preparing polyether polyols by ring-opening cyclic ethers or cyclic esters, cyclic anhydrides, and cyclic carbonates using a DMC catalyst, but does not mention the preparation of highly active polyether polyols; CN111087597B and CN102369232B disclose a process for preparing highly active polyether polyols using Lewis acids such as B(C6F5)3 and its derivatives, but the acidic catalyst will produce small molecular cycloalkane byproducts, reducing the yield, and the organic borane catalyst used is expensive, and there is no industrial report; US507 US Pat. No. 0125A and US Pat. No. 5,114,619A disclose processes for preparing polyethers with high primary hydroxyl content and low unsaturation, using barium hydroxide or strontium hydroxide as catalysts; CN106947074B and CN1061997C provide solutions using cesium hydroxide; CN110922580A discloses a solution using a phosphazene catalyst, but the above processes all have the problems of high catalyst cost, difficulty in industrialization or generation of toxic and hazardous solid wastes that are difficult to treat, and it is impossible to obtain high primary hydroxyl polyether polyols under the premise of a lower EO content (such as 5%).
[0005] US4487853A discloses a solution using cyclic anhydride to achieve a low EO content to prepare polyether polyols with a high primary hydroxyl content. However, as is known to all, the explosion limit of EO is 3-100%, which places high safety requirements on production and equipment. Summary of the invention
[0006] In view of this, the present invention provides a modified polyether polyol and a preparation method thereof, as well as a polyurethane foam material. The prepared polyether polyol has a low EO content and a high primary hydroxyl content, the primary hydroxyl content reaches more than 90%, and the EO content in the polyether polyol is less than 5%, has the characteristics of good compatibility with isocyanate and fast reaction speed, and gives the downstream foam products more excellent rebound and support performance, significantly improves the elasticity and hand comfort of the downstream foam products, and better meets the development trend of lightweight, comfort, low odor and low VOC in the automotive industry.
[0007] In order to achieve the purpose, the present invention adopts the following technical solutions:
[0008] A modified polyether polyol, the schematic structural formula of which is:
[0009]
[0010] Wherein, 4≥n≥2, X is a saturated alkylene group of 3 to 6 carbon atoms, Y is -CH2CH2-, and R is a polyethylene oxide or polypropylene oxide or polyethylene oxide propylene oxide polyether polyol residue.
[0011] The method for preparing the modified polyether polyol of the present invention comprises the following steps: polyoxyalkylene polyether polyol reacts with cyclic acid anhydride to prepare polyether half acid ester, and the polyether half acid ester further reacts with cyclic carbonate to prepare the modified polyether polyol.
[0012] The primary hydroxyl content of the present invention is the molar ratio of the primary hydroxyl group to all hydroxyl groups in the polyether polyol. The modified polyether polyol of the present invention has a primary hydroxyl content greater than 90%.
[0013] The EO content in the polyether polyol of the present invention refers to the mass fraction of the ethylene oxide chain segments in the relative number average molecular weight of the modified polyether polyol. The mass fraction of the ethylene oxide chain segments in the modified polyether polyol of the present invention is not more than 5%.
[0014] As a preferred solution, the method of the present invention comprises the following steps:
[0015] (1) reacting a polyoxyalkylene polyether polyol and a cyclic fatty acid anhydride at 80-120° C., and continuing the reaction for 0.5-5.5 hours after the reaction is completed to obtain a polyether half acid ester;
[0016] (2) Adding cyclic carbonate and a catalyst to a polyether half acid ester, reacting at 140 to 165° C. for 1.0 to 6.0 hours to obtain a modified polyether polyol.
[0017] Preferably, the above method is carried out under an inert gas atmosphere, preferably nitrogen atmosphere.
[0018] Preferably, the polyoxyalkylene polyether polyol in step (1) can be a polymerization product of any suitable alkylene oxide or a reaction product of alkylene oxide and polyol. Any suitable alkylene oxide can be used, such as one or more of ethylene oxide, propylene oxide, butylene oxide, and propylene oxide.
[0019] Preferably, the polyoxyalkylene polyether polyol is an alkylene oxide addition product of one or more of trimethylolpropane, glycerol, pentaerythritol, propylene glycol and ethylene glycol.
[0020] Further preferably, the polyoxyalkylene polyether polyol is a trimethylolpropane and / or glycerol-started polyoxypropylene triol having a molecular weight of 2000 to 10,000, preferably 3000-8000.
[0021] Preferably, step (1) may be performed without using a catalyst, or may use an inorganic base or an organic amine as a catalyst. Suitable inorganic bases may be one or more of potassium hydroxide, lithium hydroxide, and sodium hydroxide. The organic amine may be a trialkyl or triaryl amine or an alkylaryl tertiary amine, such as one or more of trimethylamine, triphenylamine, and dimethylphenylamine.
[0022] Preferably, the cyclic fatty acid anhydride in step (1) is one or more of succinic anhydride, malonic anhydride, glutaric anhydride and adipic anhydride.
[0023] Preferably, the molar ratio of the cyclic fatty acid anhydride to the hydroxyl group of the initiator is 0.8-1.2:1, preferably 1-1.1:1.
[0024] Preferably, the cyclic carbonate in step (2) is ethylene carbonate.
[0025] Preferably, step (2) can be carried out without or with a catalyst. It is preferably carried out in the presence of a catalyst, and a suitable catalyst is a catalyst that can catalyze the reaction of carbonate and carboxyl, such as a quaternary ammonium salt, a phosphonium salt, etc. Preferably, the quaternary ammonium salt catalyst is tetraethylammonium bromide, tetraethylammonium chloride, tetra-n-butylammonium chloride, tetra-n-butylammonium bromide, triethylbenzylammonium chloride or any combination thereof. Preferably, the phosphonium salt is triphenylphosphine, benzyltriphenylphosphine chloride, hexadecyltriphenylphosphine bromide, benzylsulfonated triphenylphosphine, hydroxyethylsulfonated triphenylphosphine, (1,2-dihydroxy)propylsulfonated triphenylphosphine, (1,2-dihydroxy)propylsulfonated triphenylphosphine, tetrabutylphosphonium bromide, tetrabutylphosphonium iodide, triethylbenzylammonium bromide or any combination thereof.
[0026] Preferably, the amount of catalyst used in step (2) accounts for 0.1‰-5‰ of the mass of the polyether half-acid ester, preferably 0.5-3‰.
[0027] Preferably, the mass ratio of the cyclic carbonate to the polyether half acid ester is 2%-15%, preferably 3-11%.
[0028] The modified polyether polyol of the present invention is particularly suitable for use in the preparation of polyurethane foam materials (such as flexible polyurethane foams). Therefore, the present invention also provides a polyurethane foam material obtained by foaming a composition comprising the modified polyether polyol of the present invention and polyisocyanate.
[0029] In the present invention, when preparing the polyurethane foam material, the polyisocyanate can use the known isocyanates allowed to be used in the field of polyurethane manufacturing (such as the isocyanates described in patent document US5011908A). From a practical point of view, one or more of aliphatic polyisocyanates, cycloaliphatic polyisocyanates and aromatic polyisocyanates are preferred. Aliphatic polyisocyanates include, but are not limited to, 1,6-hexamethylene diisocyanate, etc.; cycloaliphatic polyisocyanates include, but are not limited to, 1,6-cyclohexyl diisocyanate, 1-isocyanate-3,5,5-trimethyl-1,3-isocyanatomethylcyclohexane, 2,4- and 2,6-hexahydrotoluene-diisocyanate, 4,4'-, 2,2'- and 2,4'-isocyanatomethylcyclohexane. -dicyclohexyl-methane diisocyanate and their corresponding isomeric mixtures, etc.; aromatic polyisocyanates, for example, include but are not limited to 2,4- and 2,6-toluene diisocyanate (TDI) and corresponding isomeric mixtures, 4,4'-, 2,4'- and 2,2'-diphenylmethane diisocyanate (MDI) and corresponding isomeric mixtures, 4,4'-, 2,4'- and 2,2'-diphenylmethane diisocyanate and polyphenyl polymethylene polyisocyanate (PMDI) and one or more of the mixtures; and one or more of modified polyisocyanates containing carbamate, carbodiimide group, allophanate, urea group, biuret group or isocyanurate group derived from these polyisocyanates.
[0030] In the present invention, the equivalent ratio of the NCO groups in the polyisocyanate to the active hydrogen atoms in the polyol composition (the composition refers to a mixture of other raw material components except the polyisocyanate raw material) ((NCO group / active hydrogen atom)×100), also known as the NCO index, can be appropriately adjusted based on the mechanical properties of the polyurethane, for example, preferably 80 to 140, more preferably 85 to 120, and particularly preferably 95 to 115.
[0031] The specific preparation process of the polyurethane foam can adopt the corresponding process known in the art, and a polyurethane catalyst, a cross-linking agent, a foaming agent, a foam stabilizer, etc. are often added to the reaction system.
[0032] The polyurethane catalyst may be a corresponding catalyst commonly used in the art, for example, an organic metal compound, such as one or more of stannous octoate, stannous oleate, dibutyltin dilaurate, dibutyltin acetate and dibutyltin diacetate, etc.; an organic amine catalyst, such as one or more of di(2,2′-dimethylamino)ethyl ether, trimethylamine, triethylamine, triethylenediamine and dimethylethanolamine, etc. The amount of the polyurethane catalyst used is generally about 0.1-3.0 wt % based on the weight of the polyol composition (the composition refers to other raw material components except the polyisocyanate raw material).
[0033] In the preparation of polyurethane foam, the crosslinking agent can use the crosslinking agent commonly used in the art, for example, including but not limited to glycerol and / or diethanolamine. If a crosslinking agent is used, the amount of the crosslinking agent can be less than 3% (w / w), preferably 0.2-1.5% (w / w), based on the weight of the polyol composition.
[0034] Examples of suitable blowing agents include, but are not limited to, one or more of water, acetone, carbon dioxide, halogenated hydrocarbons, aliphatic alkanes, and cycloalkanes. As is well known in the art, water used as a blowing agent can generate carbon dioxide by reacting with isocyanates, which can be used as a blowing agent. Aliphatic alkanes and cycloalkanes are being developed as alternative blowing agents to CFC compounds. The blowing agent can be used alone or in a mixture of a plurality thereof. The amount of the blowing agent used is, for example, 0.1-20% (w / w) based on the weight of the polyol composition.
[0035] Suitable foam stabilizers are, for example, organopolysiloxane surfactants. The amount of foam stabilizer used may be 0.4-1% (w / w) based on the weight of the polyol package.
[0036] According to product requirements, 0.1-50% (w / w) of additives based on the weight of the polyol combination are often added, such as flame retardants, fillers, light stabilizers, antioxidants, etc., which are not described in detail here.
[0037] The present invention also provides a product, which contains the polyurethane foam material of the present invention.
[0038] The technical solution provided by the present invention has the following beneficial effects:
[0039] (1) The primary hydroxyl content of the modified polyether polyol product prepared by the present invention reaches more than 90%, and the EO ratio in the polyether molecule is less than or equal to 5%;
[0040] (2) Compared with the traditional high molecular weight and high activity polyether polyol synthesis process, the method of the present invention does not use ethylene oxide, does not discharge three wastes, can be produced on a large scale, and is more green, environmentally friendly, safe and reliable;
[0041] (3) The ester group in the modified polyether polyol prepared by the present invention is located at the end of the polyol molecule, and the polyether molecule does not contain an ester group, which has better compatibility with isocyanate, giving the polyurethane foam excellent uniform foaming performance, reducing the internal stress of the polyurethane foam, uniform pore opening, fine pores, and excellent hydrolysis resistance. DETAILED DESCRIPTION
[0042] In order to better understand the technical solution of the present invention, the content of the present invention is further described below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0043] The following describes some of the raw materials involved in the embodiments or comparative examples:
[0044] Polyoxyalkylene polyether polyol A: Polyether polyol prepared by reaction of glycerol with propylene oxide and ethylene oxide, molecular weight 3000, Wanhua Chemical Group Co., Ltd. F3156.
[0045] Polyoxyalkylene polyether polyol B: DMC-catalyzed, produced by the ring-opening reaction of glycerol and propylene oxide, with a molecular weight of 5,000.
[0046] Polyoxyalkylene polyether polyol C: DMC-catalyzed, produced by the ring-opening reaction of glycerol and propylene oxide, with a molecular weight of 8,000.
[0047] Polyether polyol D: A high primary hydroxyl polyether polyol prepared by reacting glycerol with propylene oxide and then end-capping with ethylene oxide, with a molecular weight of 5000 and a primary hydroxyl content of 80-85%, produced by Wanhua Chemical Group Co., Ltd. F3135.
[0048] Polymer polyol E: Polymer polyol containing styrene and acrylonitrile polymer, Wanhua Chemical Group Co., Ltd. POP2140.
[0049] A33: Polyurethane catalyst, a solution of 33% triethylenediamine and 67% dipropylene glycol, American Gas Chemical.
[0050] A1: Polyurethane catalyst, a solution of 70% bis(dimethylaminoethyl) ether in dipropylene glycol, 33% triethylenediamine and 67% dipropylene glycol, from American Gas Chemicals.
[0051] Cell opener: polyhydroxy compound (also called polyol) with a number average molecular weight of 2000-10000 and an average functionality of 2-4, Wanhua Chemical Group Co., Ltd. F5342.
[0052] 8001: Modified MDI (diphenylmethane diisocyanate), Wanhua Chemical Group Co., Ltd.
[0053] B-8715: Foam stabilizer, High Schmidt Chemical Co., Ltd.
[0054] Unless otherwise specified, other raw materials involved in the following examples were purchased from Aladdin Reagent.
[0055] The detection methods involved in the embodiments or comparative examples are described as follows:
[0056] Hydroxyl value: GB 12008.3-2009 Plastic polyether polyols Part 3: Determination of hydroxyl value;
[0057] Viscosity: GB 12008.7-2010 Plastic polyether polyols Part 7: Determination of viscosity;
[0058] Primary Hydroxyl Content: ASTM D4273-23 Standard Test Method for Polyurethane RawMaterials: Determination of Primary Hydroxyl Content of Polyether Polyols;
[0059] Determination of EO segment content in polyether: carbon 13 nuclear magnetic resonance spectroscopy (13C NMR) measurement, Bruker Ascend-400.
[0060] Examples 1-3 and Comparative Examples 1-3
[0061] Step (1) reacting a polyether polyol initiator and a cyclic fatty acid anhydride at 80-120° C., and continuing the reaction for 0.5-5.5 hours after the reaction is completed to obtain a polyether half acid ester;
[0062] Step (2) adding cyclic carbonate and catalyst to polyether half acid ester, reacting at 140-165° C. for 1.0-6.0 hours to obtain modified polyether polyol.
[0063] The specific preparation process parameters are shown in Table 1, and the product indicators are shown in Table 2.
[0064] Table 1 Preparation process parameters
[0065]
[0066] Table 2 Product indicators
[0067] Viscosity cp Acid value mgKOH / g Primary hydroxyl content / % EO segment / % Example 1 850 0.26 95% 4.50% Example 2 1200 0.24 96% 2.70% Example 3 4200 0.23 96% 1.70% Comparative Example 1 1610 0.24 95% 2.60% Comparative Example 2 4500 0.25 95% 3% Comparative Example 3 1310 1.07 <3% <1%
[0068] In order to illustrate the benefits of the present invention, the downstream application performance foaming evaluation of the polyether polyol was carried out. Since the molecular weight of the polyether affects the hydroxyl value and the corresponding isocyanate R value, it is necessary to select polyether polyols of the same type (such as molecular weight) for foaming testing, and then Example 2, Comparative Examples 1, 2, and 3 were selected for comparison with the commercially available product polyether polyol D.
[0069] Preparation of polyurethane foam:
[0070] Prepare the composite material according to the raw materials and weight parts shown in Table 3, keep the composite material and isocyanate raw material at constant temperature for 3 hours. Then take 100g of the composite material and mix it with 60g of isocyanate. 8001 components were stirred and mixed in a stirrer (rotation speed 3000 rpm) for 6 seconds. The stirred mixture was then quickly poured into an aluminum open mold (size: 300 mm long, 300 mm wide, 50 mm thick) preheated to 60°C to allow the mixture to foam. After 7 minutes, the foam was taken out to obtain polyurethane foam.
[0071] Table 3 Combination material formula
[0072]
[0073] The foaming properties of the prepared polyurethane foam are shown in Table 4 below:
[0074] Table 4 Polyurethane foaming properties
[0075]
[0076] From the foaming conditions of polyurethane foams in Example 4 and Comparative Examples 4 to 7, the foams prepared using the highly active polyether of the present invention and Comparative Example 1 are superior to the existing highly active polyethers in terms of foaming height, foaming rate, and fall back height, and are superior to the commercially available products and the polyethers prepared in Comparative Examples 2 to 3. However, the viscosity of the polyether prepared in Comparative Example 1 is higher than that of the highly active polyether in this case.
[0077] Those skilled in the art will appreciate that, based on the teachings of this specification, some modifications or adjustments may be made to the present invention, and these modifications or adjustments should also be within the scope defined by the claims of the present invention.
Claims
1. A modified polyether polyol, the schematic structural formula of which is: in, 4≥n≥2, X is a saturated alkylene group with 3 to 6 carbon atoms, Y is -CH2CH2-, and R is a polyethylene oxide or polypropylene oxide or polyethylene oxide propylene oxide polyether polyol residue.
2. The modified polyether polyol according to claim 1, characterized in that The primary hydroxyl content is greater than 90%, and the mass fraction of the ethylene oxide chain segments in the modified polyether polyol is not greater than 5%.
3. A method for preparing the modified polyether polyol according to claim 1 or 2, comprising the following steps: (1) reacting a polyoxyalkylene polyether polyol initiator and a cyclic fatty acid anhydride at 80-120° C., and continuing the reaction for 0.5-5.5 hours after the reaction is completed to obtain a polyether half acid ester; (2) Adding cyclic carbonate and a catalyst to a polyether half acid ester, reacting at 140 to 165° C. for 1.0 to 6.0 hours to obtain a modified polyether polyol.
4. The method according to claim 3, characterized in that The polyoxyalkylene polyether polyol in step (1) includes the polymerization product of alkylene oxide or the reaction product of alkylene oxide and polyol; the alkylene oxide includes one or more of ethylene oxide, propylene oxide, butylene oxide and propylene oxide; preferably, the polyoxyalkylene polyether polyol is the alkylene oxide addition product of one or more of trimethylolpropane, glycerol, pentaerythritol, propylene glycol and ethylene glycol.
5. The method according to claim 3 or 4, characterized in that: The polyoxyalkylene polyether polyol is a trimethylolpropane and / or glycerol-started polyoxypropylene triol having a molecular weight of 2000 to 10,000, preferably 3000-8000.
6. The method according to any one of claims 3 to 5, characterized in that: In the step (1), the cyclic fatty acid anhydride is one or more of succinic anhydride, malonic anhydride, glutaric anhydride and adipic anhydride.
7. The method according to any one of claims 3 to 6, characterized in that: The molar ratio of the cyclic fatty acid anhydride to the hydroxyl group of the initiator is 0.8-1.2:1, preferably 1-1.1:
1.
8. The method according to any one of claims 3 to 7, characterized in that: In the step (2), the cyclic carbonate is ethylene carbonate.
9. The method according to any one of claims 3 to 8, characterized in that: The mass ratio of the cyclic carbonate to the polyether half acid ester is 2%-15%, preferably 3-11%.
10. A polyurethane foam material, prepared by foaming a composition comprising the modified polyether polyol according to claim 1 or 2 or the modified polyether polyol prepared by the method according to any one of claims 3 to 9 and polyisocyanate.
Citation Information
Patent Citations
Modified polyether polyhydric alcohol and application thereof in polyurethane foam materials
CN109796588A
Polyurethane foams based on polyethercarbonate polyols
CN110709440A
Cyclic carbonate group-terminated polyurethane prepolymer and preparation method and application thereof
CN112011029A
Flexible polyurethane foams made from alkoxylated natural oil
US20120016048A1
Novel polyether polycarbonate block copolymers and polyurethanes prepared therefrom
US4634743A