Phenyl high-molecular polysiloxane resistant to low-temperature irradiation

Through the bicatalytic system synthesis method, the problem of insufficient radiation resistance of phenyl polysiloxane at low temperature was solved, and phenyl polymer polysiloxane with stable low temperature resistance, radiation resistance and burn resistance was prepared. Suitable for high-end industrial applications.

CN118994584AInactive Publication Date: 2024-11-22BENGBU AIYOU NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411051334.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing phenyl polysiloxane has poor radiation resistance at low temperatures, which affects its application in the field of low temperatures.

Method used

The octamethylcyclotetrasiloxane was opened by a tetramethylammonium hydroxide alkali glue catalyst by a bicatalyst synthesis method, and then the bismethylbisphenylcyclosiloxane was connected by a vinyl-nBuLi alkali glue catalyst. and tetramethyldivinyldisiloxane, and finally the polymerization chain was terminated with hexamethyldisiloxane to prepare a phenyl polymer polysiloxane with stable low temperature irradiation resistance.

Benefits of technology

Improve the low temperature resistance, radiation resistance and burn resistance of phenyl polymer polysiloxane, avoiding the hysteresis problem during the ring-opening polymerization process, and the prepared materials have good stability and controllability, which are suitable for High-end fields such as aerospace industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994584A_ABST
    Figure CN118994584A_ABST
Patent Text Reader

Abstract

The invention discloses phenyl high-molecular polysiloxane resistant to low-temperature irradiation, and belongs to the technical field of high-molecular materials. The preparation method comprises the following steps of: performing ring opening on octamethylcyclotetrasiloxane by using a tetramethylammonium hydroxide alkali gel catalyst with relatively high activity to form an active center, and connecting dimethyl diphenylcyclosiloxane and tetramethyldivinyldisiloxane to a ring opening chain by using a vinyl-nBuL i alkali gel catalyst with relatively low activity; and finally, enabling an end-capping reagent hexamethyldisiloxane to react with the active center to promote chain termination, so as to obtain the raw silicone rubber methyl phenyl vinyl high-molecular polysiloxane. The light-emitting diode is transparent or has milky white light, no mechanical impurities exist, the content of phenyl is 5-25 mol%, the content of vinyl is 0.1-0.35 mol%, and the molecular weight is 3 * 10 < 5 >-10 * 10 < 5 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a phenyl polymer polysiloxane resistant to low-temperature radiation. Background Art

[0002] Polysiloxane (such as silicone oil, silicone rubber, silicone resin, etc.) plays an important role in industrial production and daily life due to its good thermal stability and radiation stability, high air permeability, low dielectric constant, low temperature flexibility, electrical insulation, damping and excellent biocompatibility. Especially in high-end technical fields such as aerospace, electronics and electrical, weapons and equipment, polysiloxane has been widely used. It has become one of the indispensable polymer materials in daily life and national comprehensive strength.

[0003] Linear polysiloxane is a polymer with repeated SiO bonds as the main chain and organic groups as the side chains. It is also the most common type of siloxane polymer in the field of polysiloxane research, among which polydimethylsiloxane (PDMS) is the most common. However, the transition temperature (Tg) of PDMS is around -123℃ and the crystallization temperature is around -50℃, which limits its application at low temperatures. The problem of low-temperature crystallization can be further improved by introducing Japanese siloxane units. The introduction of phenyl siloxane can effectively destroy the regularity of the molecular structure of polysiloxane, reduce the crystallization temperature of the polymer, and make the polymer maintain good elasticity at lower temperatures, thereby effectively improving the low-temperature resistance and broadening its application in the low-temperature field without significantly changing the glass transition temperature. However, due to the large difference in the ring-opening reaction activity between phenylcyclosiloxane monomers and methylcyclosiloxane monomers, and the large steric hindrance of phenylcyclosiloxane monomers leads to a large hysteresis in the ring-opening polymerization process, thereby affecting the performance of phenyl polysiloxane. Therefore, there is an urgent need for a phenyl high-molecular polysiloxane with stable low-temperature radiation resistance to solve the above problems. Summary of the invention

[0004] The object of the present invention is to provide a phenyl high molecular weight polysiloxane resistant to low temperature radiation, so as to solve the problem that the existing phenyl polysiloxane in the background technology has poor low temperature radiation resistance.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A low temperature radiation resistant phenyl polymer polysiloxane, the chemical structure is:

[0007] The molecular weight is 3×10 5 -10×10 5 , phenyl content is 5-25 mol%, vinyl content is 0.1-0.35 mol%;

[0008] The phenyl high molecular weight polysiloxane is prepared by the following steps:

[0009] S1. Octamethylcyclotetrasiloxane was stirred at 50-70°C for 0.5-1h, tetramethylammonium hydroxide (TMAH) alkali gel catalyst was added for 2-4h, then dimethylbisphenylcyclosiloxane and tetramethyldivinyldisiloxane were added, the temperature was raised to 90-110°C, CH2=CH-nBuL i alkali gel catalyst was added, and the reaction was continued for 2-4h to obtain a matrix;

[0010] S2. Under vacuum conditions, hexamethyldisiloxane is added to the matrix, the temperature is raised to 160-180°C, the pressure of the reaction system is controlled to a negative pressure state for 1-2 hours, small molecules in the system are removed until no liquid drips out, and the system is naturally cooled to room temperature (25-30°C) to obtain phenyl high molecular weight polysiloxane resistant to low temperature radiation.

[0011] Furthermore, the weight proportions of octamethylcyclotetrasiloxane, bismethylbisphenylcyclosiloxane, tetramethyldivinyldisiloxane, tetramethylammonium hydroxide alkali gel catalyst and CH2=CH-nBuL i alkali gel catalyst in S1 are 100-120 parts, 7-30 parts, 2-4 parts, 3-6 parts and 1-4 parts respectively.

[0012] Furthermore, the weight proportions of the matrix and hexamethyldisiloxane in S2 are 100-120 parts and 0.04-0.1 parts respectively.

[0013] Furthermore, the preparation method of the CH2=CH-nBuL i alkali-gel catalyst comprises the following steps:

[0014] n-Butyl lithium (nBuLi) is added to a mixed monomer of octamethylcyclotetrasiloxane and tetramethyldivinyldisiloxane, and the mixture is stirred at 50-70°C for 1-2 hours. DMF (N,N-dimethylformamide) is added and the reaction is continued for 1-3 hours to obtain vinyl-nBuLi alkaline gel.

[0015] Furthermore, the molar ratio of octamethylcyclotetrasiloxane to tetramethyldivinyldisiloxane is 2:3.

[0016] Furthermore, the weight proportions of the mixed monomer, n-butyl lithium and DMF are 60-80 parts, 1-2 parts and 10-12 parts respectively.

[0017] Furthermore, the stirring speed is 100-300 rpm.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. The present invention discloses a phenyl high molecular weight polysiloxane resistant to low temperature radiation, which is synthesized by a two-step dual catalytic system. First, octamethylcyclotetrasiloxane is ring-opened by a tetramethylammonium hydroxide alkali colloid catalyst with relatively large activity to form an active center. Then, a vinyl-nBuLi alkali colloid catalyst with relatively small activity is used to connect dimethyldiphenylcyclosiloxane and tetramethyldivinyldisiloxane to the ring-opened chain to complete the chain growth. Finally, a capping agent hexamethyldisiloxane is used to react with the active center to promote chain termination to obtain a silicone rubber raw rubber methylphenylvinyl high molecular weight polysiloxane. The silicone rubber raw rubber methylphenylvinyl high molecular weight polysiloxane is transparent or opalescent, free of mechanical impurities, has a phenyl content of 5-25 mol%, a vinyl content of 0.1-0.35 mol%, and a molecular weight of 3×10 5 -10×10 5 .

[0020] 2. The low temperature radiation resistant phenyl high molecular weight polysiloxane prepared by the present invention not only has a series of characteristics of ethylene silicone rubber, but also improves its low temperature resistance, radiation resistance, burning resistance and self-extinguishing properties by introducing phenyl groups. It is one of the materials for aerospace industry and cutting-edge technology. It can be widely used as various molded and extruded products, and used for sealing rings, pads, pipes, and rods in cold-resistant and burning-resistant, heat-resistant, aging-resistant and radiation-resistant parts. It can also be used to make various purpose products, such as: making damping materials, pressure-sensitive adhesives, etc.

[0021] 3. Through the dual-catalyst two-step method, the large difference in the ring-opening reaction activity of phenylcyclosiloxane monomer and methylcyclosiloxane monomer and the large steric hindrance of phenylcyclosiloxane monomer, which leads to large hysteresis in the ring-opening polymerization process and affects the degree of polymerization, are avoided. The prepared silicone rubber has low by-product content, the reaction process is stable, controllable and easy to reproduce, the phenyl and vinyl contents are stable, and chain branching is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The present invention will be further described below in conjunction with the accompanying drawings.

[0023] Figure 1 The present invention is a schematic diagram of the preparation process of the low-temperature radiation-resistant phenyl high-molecular polysiloxane. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The preparation method of CH2=CH-nBuL i alkali gel catalyst comprises the following steps:

[0026] To 60-80 parts of a mixed monomer of octamethylcyclotetrasiloxane and tetramethyldivinyldisiloxane (the molar ratio of octamethylcyclotetrasiloxane to tetramethyldivinyldisiloxane is 2:3), 1-2 parts of n-butyllithium (nBuL i) are added, and the mixture is stirred at 50-70° C. and 100-300 rpm for reaction for 1-2 hours. After adding 10-12 parts of DMF, the reaction is continued for 1-3 hours to obtain CH2=CH-nBuL i alkali gel.

[0027] A low temperature radiation resistant phenyl polymer polysiloxane, the chemical structure is:

[0028] The molecular weight is 3×10 5 -10×10 5 , phenyl content is 5-25 mol%, vinyl content is 0.1-0.35 mol%;

[0029] Please refer to Figure 1 , the phenyl polymer polysiloxane is prepared by the following steps:

[0030] S1. 100-120 parts of octamethylcyclotetrasiloxane are stirred at 100-300 rpm at 50-70 ° C for 0.5-1h, 3-6 parts of tetramethylammonium hydroxide alkali gel catalyst (TMAH) are added and reacted for 2-4h, and then 7-30 parts of dimethylbisphenylcyclosiloxane and 2-4 parts of tetramethyldivinyldisiloxane are added, the temperature is raised to 90-110 ° C, 1-4 parts of CH2=CH-nBuL i alkali gel catalyst are added, and the reaction is continued for 2-4h to obtain a matrix;

[0031] S2. Under vacuum conditions, add 0.04-0.1 parts of hexamethyldisiloxane to 100-120 parts of the matrix, raise the temperature to 160-180°C, control the pressure of the reaction system to a negative pressure state for 1-2 hours, remove small molecules in the system until no liquid drips out, and naturally cool to room temperature (25-30°C) to obtain a phenyl high molecular weight polysiloxane resistant to low temperature radiation.

[0032] Example 1

[0033] The preparation method of CH2=CH-nBuL i alkali gel catalyst comprises the following steps:

[0034] 1.5 parts of n-butyl lithium were added to 70 parts of a mixed monomer of octamethylcyclotetrasiloxane and tetramethyldivinyldisiloxane (the molar ratio of octamethylcyclotetrasiloxane to tetramethyldivinyldisiloxane was 2:3), and the mixture was stirred at 60°C and 200 rpm for 1.5 h. After adding 11 parts of DMF, the reaction was continued for 2 h to obtain a CH2=CH-nBuL i alkali gel catalyst.

[0035] The CH2=CH-nBuL i alkali gel catalysts in the following examples and comparative examples are all prepared by the preparation method of this example.

[0036] Example 2

[0037] Please refer to Figure 1 , a phenyl high molecular weight polysiloxane resistant to low temperature radiation, is prepared by the following steps:

[0038] S1. 110 parts of octamethylcyclotetrasiloxane were stirred at 200 rpm at 60 ° C for 1 h, 5 parts of TMAH alkali gel catalyst were added and reacted for 3 h, then 20 parts of dimethylbisphenylcyclosiloxane and 3 parts of tetramethyldivinyldisiloxane were added, the temperature was raised to 95 ° C, 2 parts of CH2=CH-nBuL i alkali gel catalyst were added, and the reaction was continued for 3 h to obtain a matrix;

[0039] S2. Under vacuum conditions, add 0.06 parts of hexamethyldisiloxane to 110 parts of the matrix, raise the temperature to 170°C, control the pressure of the reaction system to a negative pressure state for 1.5 hours, remove small molecules in the system until no liquid drips out, and naturally cool to room temperature to obtain a phenyl polymer polysiloxane resistant to low-temperature radiation.

[0040] Example 3

[0041] Please refer to Figure 1 , a phenyl high molecular weight polysiloxane resistant to low temperature radiation, is prepared by the following steps:

[0042] S1. 100 parts of octamethylcyclotetrasiloxane were stirred at 200 rpm at 60 ° C for 1 h, 6 parts of TMAH alkali gel catalyst were added and reacted for 3 h, and then 8 parts of dimethylbisphenylcyclosiloxane and 3.8 parts of tetramethyldivinyldisiloxane were added, the temperature was raised to 95 ° C, 1 part of CH2=CH-nBuL i alkali gel catalyst was added, and the reaction was continued for 3 h to obtain a matrix;

[0043] S2. Under vacuum conditions, add 0.1 parts of hexamethyldisiloxane to 110 parts of the matrix, raise the temperature to 170°C, control the pressure of the reaction system to a negative pressure state for 1.5 hours, remove small molecules in the system until no liquid drips out, and naturally cool to room temperature to obtain a phenyl high molecular weight polysiloxane resistant to low-temperature radiation.

[0044] Example 4

[0045] Please refer to Figure 1 , a phenyl high molecular weight polysiloxane resistant to low temperature radiation, is prepared by the following steps:

[0046] S1. 120 parts of octamethylcyclotetrasiloxane were stirred at 200 rpm at 60 ° C for 1 h, 3 parts of TMAH alkali gel catalyst were added and reacted for 3 h, then 28 parts of dimethylbisphenylcyclosiloxane and 2.1 parts of tetramethyldivinyldisiloxane were added, the temperature was raised to 95 ° C, 4 parts of CH2=CH-nBuL i alkali gel catalyst were added, and the reaction was continued for 3 h to obtain a matrix;

[0047] S2. Under vacuum conditions, add 0.04 parts of hexamethyldisiloxane to 110 parts of the matrix, raise the temperature to 170°C, control the pressure of the reaction system to a negative pressure state for 1.5 hours, remove small molecules in the system until no liquid drips out, and naturally cool to room temperature to obtain a phenyl high molecular weight polysiloxane resistant to low-temperature radiation.

[0048] Comparative Example 1

[0049] A phenyl high molecular weight polysiloxane is prepared by the following steps:

[0050] S1. 110 parts of octamethylcyclotetrasiloxane, 20 parts of bismethylbisphenylcyclosiloxane and 3 parts of tetramethyldivinyldisiloxane were stirred at 60 ° C at a speed of 200 rpm for 1 h, 5 parts of TMAH alkali gel catalyst and 2 parts of CH2=CH-nBuL i alkali gel catalyst were added, and the temperature was raised to 95 ° C and the reaction was continued for 3 h to obtain a matrix;

[0051] S2. Under vacuum conditions, add 0.06 parts of hexamethyldisiloxane to 110 parts of the matrix, raise the temperature to 170°C, control the pressure of the reaction system to a negative pressure state for 1.5 hours, remove small molecules in the system until no liquid drips out, and naturally cool to room temperature to obtain phenyl high molecular weight polysiloxane.

[0052] Comparative Example 2

[0053] A phenyl high molecular weight polysiloxane is prepared by the following steps:

[0054] S1. 110 parts of octamethylcyclotetrasiloxane were stirred at 200 rpm at 60 ° C for 1 h, 5 parts of TMAH alkali gel catalyst were added and reacted for 3 h, then 20 parts of dimethylbisphenylcyclosiloxane and 3 parts of tetramethyldivinyldisiloxane were added, the temperature was raised to 95 ° C, and 2 parts of TMAH alkali gel catalyst were added, and the reaction was continued for 3 h to obtain a matrix;

[0055] S2. Under vacuum conditions, add 0.06 parts of hexamethyldisiloxane to 110 parts of the matrix, raise the temperature to 170°C, control the pressure of the reaction system to a negative pressure state for 1.5 hours, remove small molecules in the system until no liquid drips out, and naturally cool to room temperature to obtain phenyl high molecular weight polysiloxane.

[0056] Comparative Example 3

[0057] A phenyl high molecular weight polysiloxane is prepared by the following steps:

[0058] S1. 110 parts of octamethylcyclotetrasiloxane were stirred at 200 rpm at 60 ° C for 1 h, 2 parts of CH2 = CH-nBuL i alkali gel catalyst were added and reacted for 3 h, then 20 parts of dimethylbisphenylcyclosiloxane and 3 parts of tetramethyldivinyldisiloxane were added, the temperature was raised to 95 ° C, 5 parts of TMAH alkali gel catalyst were added, and the reaction was continued for 3 h to obtain a matrix;

[0059] S2. Under vacuum conditions, add 0.06 parts of hexamethyldisiloxane to 110 parts of the matrix, raise the temperature to 170°C, control the pressure of the reaction system to a negative pressure state for 1.5 hours, remove small molecules in the system until no liquid drips out, and naturally cool to room temperature to obtain phenyl high molecular weight polysiloxane.

[0060] Comparative Example 4

[0061] A phenyl high molecular weight polysiloxane is prepared by the preparation steps of Example 2, except that dimethyldiphenylcyclosiloxane is replaced by tetramethyltetraphenylcyclotetrasiloxane; the chemical structure of the product is Formula A:

[0062]

[0063] Comparative Example 5

[0064] A phenyl high molecular weight polysiloxane is prepared by the preparation steps of Example 2, except that bismethylbisphenylcyclosiloxane is replaced by octaphenylcyclotetrasiloxane; the chemical structural formula of the product is Formula B:

[0065]

[0066] Performance Test:

[0067] The vinyl content and introduction rate of the phenyl high molecular weight polysiloxane raw rubber prepared in Examples 2-4 and Comparative Examples 1-5 were tested by iodine titration. The test results are shown in Table 1:

[0068] Table 1

[0069]

[0070]

[0071] 100 parts by weight of the phenyl high molecular weight polysiloxane prepared in Examples 2-4 and Comparative Examples 1-5 were dried respectively, and then 30 parts by weight of white carbon black and an appropriate amount of DCM were added, and the mixture was shaken and stirred evenly. 0.5 parts by weight of a vulcanizing agent (2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane) was added and mixed evenly. The mixture was allowed to stand to remove bubbles, and the mixture was spread flat in a metal mold. The mixture was hot-pressed at 150°C and 10 MPa to form a film to obtain a phenyl high molecular weight silicone rubber.

[0072] The tensile strength of the vulcanized silicone rubber is tested in accordance with GB / T528-2009; the tear strength is tested in accordance with GB / T529-2008; the elongation is tested in accordance with GB / T531.1-2008, and the low temperature performance is tested by DSC to test its glass transition temperature Tg; the test results are shown in Table 2:

[0073] Table 2

[0074]

[0075] It can be seen from Table 1 and Table 2 that the present invention adopts a dual-catalyst two-step method and uses dimethyldiphenylcyclosiloxane as a phenyl introduction monomer to further increase the number of siloxane segments. The two-step catalysis and the ring-opening of the phenyl and vinyl groups on the siloxane complement each other. The prepared phenyl polymer polysiloxane has a high and stable vinyl introduction amount, and has excellent performance after raw rubber vulcanization.

[0076] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0077] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A phenyl polymer polysiloxane resistant to low temperature radiation, It is characterized in that The chemical structural formula of the polysiloxane is: The molecular weight is 3×10 5 -10×10 5 , the phenyl content is 5-25 mol%, and the vinyl content is 0.1-0.35 mol%.

2. The low-temperature radiation-resistant phenyl polymer polysiloxane according to claim 1, It is characterized in that The polysiloxane is prepared by the following steps: S1. Stir octamethylcyclotetrasiloxane at 50-70℃ for 0.5-1h, add tetramethylammonium hydroxide alkali gel catalyst and react for 2-4h, then add dimethylbisphenylcyclosiloxane and tetramethyldivinyldisiloxane, heat to 90-110℃, add CH 2 =CH-nBuLi alkali gel catalyst, continue the reaction for 2-4h to obtain the matrix; S2. Add hexamethyldisiloxane to the matrix under vacuum conditions, raise the temperature to 160-180°C, control the pressure of the reaction system to a negative pressure state for 1-2 hours, remove small molecules in the system until no liquid drips out, and cool naturally to room temperature.

3. A low temperature radiation resistant phenyl polymer polysiloxane according to claim 2, It is characterized in that The octamethylcyclotetrasiloxane, dimethylbisphenylcyclosiloxane, tetramethyldivinyldisiloxane, tetramethylammonium hydroxide alkali gel catalyst and CH 2 =The weight proportions of CH-nBuLi alkali gel catalyst are 100-120 parts, 7-30 parts, 2-4 parts, 3-6 parts and 1-4 parts respectively.

4. The low-temperature radiation-resistant phenyl polymer polysiloxane according to claim 2, It is characterized in that The weight proportions of the matrix and hexamethyldisiloxane in S2 are 100-120 parts and 0.04-0.1 parts respectively.

5. The low-temperature radiation-resistant phenyl high molecular weight polysiloxane according to claim 2, It is characterized in that The stirring speed is 100-300 rpm.

6. The low-temperature radiation-resistant phenyl high molecular weight polysiloxane according to claim 2, It is characterized in that The CH 2 =The preparation method of CH-nBuLi alkali colloid catalyst comprises the following steps: n-Butyl lithium is added to a mixed monomer of octamethylcyclotetrasiloxane and tetramethyldivinyldisiloxane, and the mixture is stirred and reacted at 50-70° C. for 1-2 hours. DMF is added and the reaction is continued for 1-3 hours to obtain vinyl-nBuLi alkaline gum.

7. The low-temperature radiation-resistant phenyl high molecular weight polysiloxane according to claim 6, It is characterized in that The molar ratio of the octamethylcyclotetrasiloxane to the tetramethyldivinyldisiloxane is 2:

3.

8. The low-temperature radiation-resistant phenyl high molecular weight polysiloxane according to claim 6, It is characterized in that The weight proportions of the mixed monomer, n-butyl lithium and DMF are 60-80 parts, 1-2 parts and 10-12 parts respectively.

9. The low-temperature radiation-resistant phenyl high molecular weight polysiloxane according to claim 6, It is characterized in that The stirring speed is 100-300 rpm.