Silica sol modified natural rubber and preparation method thereof

By adding phosphate flame retardant, modified silica sol and other components to the natural rubber, the modified silica sol is formed to form a silicon sol modified natural rubber, which solves the problem of insufficient tear resistance and flame retardant properties of natural rubber, and significantly improves its flame retardant performance and mechanical strength.

CN118994753AInactive Publication Date: 2024-11-22SHANDONG KEHAN SILICON SOURCE NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411278731.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The tear resistance and flame retardancy of existing natural rubbers are insufficient, which limits its application and development.

Method used

The method of modifying natural rubber in silica sol is used to form a silicone sol with good tear resistance and flame retardant by adding phosphate flame retardant, modified silica sol, vulcanized natural rubber, hydroxyethyl cellulose and carbon black. Modified natural rubber.

Benefits of technology

It significantly improves the flame retardant properties and mechanical strength of rubber, enhances its resistance to external forces and fires, and improves tear resistance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005040998680000111
    Figure BDA0005040998680000111
Patent Text Reader

Abstract

The invention relates to the technical field of natural rubber, and discloses silica sol modified natural rubber and a preparation method thereof. The phosphate flame retardant, the modified silica sol, the vulcanized natural rubber, the hydroxyethyl cellulose and the carbon black are added into a reactor to react, and the silica sol modified natural rubber is obtained. The phosphorus element promotes a carbonized layer formed on the surface of the rubber to block heat transfer; the nitrogen element has the effects of insulating heat and effectively preventing air from entering the rubber bottom layer; silicon dioxide generated by the silicon element at a high temperature can form an isolating membrane, so that a flame-retardant effect is achieved; incombustible gas generated in the combustion process of the sulfur element slows down the spreading of the fire behavior; the quaternary ammonium salt group enhances the tensile strength of the rubber by increasing cross-linking points; benzoxazine can form a protective layer on the rubber surface; the silica sol reacts with the coupling agent, so that the adhesive force and catalytic activity of the silica sol are improved, and the density of the rubber is increased; and a cross-linked structure generated by sulfur and rubber improves the strength and elasticity of the rubber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of natural rubber, in particular to a silica sol-modified natural rubber and a preparation method thereof. Background Art

[0002] Natural rubber is a high molecular compound extracted from the latex of rubber trees. It is mainly composed of cis-1,4-polyisoprene and has excellent resilience, insulation, water-proofness and plasticity. It is widely used in the manufacture of various rubber products such as gloves, tires, and tapes. However, natural rubber itself still has many shortcomings, such as low tear resistance and flame retardancy, which limits its application and development. For example, patent CN102124034B discloses a method for modifying natural rubber and modified natural rubber, which only improves the molecular weight and processing performance of natural rubber, and its tear resistance and flame retardancy need to be improved. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies of the prior art, the present invention provides a silica sol-modified natural rubber and a preparation method thereof, which has good tear resistance and flame retardancy.

[0005] (II) Technical solution

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a silica sol modified natural rubber, comprising the following weight components: 8-10 weight parts of phosphate flame retardant, 10-15 weight parts of modified silica sol, 18-26 weight parts of vulcanized natural rubber, 1-3 weight parts of hydroxyethyl cellulose, and 4-6 weight parts of carbon black.

[0007] Preferably, the preparation method of the phosphate flame retardant is:

[0008] S1. Add 4-aminophenyltrimethylsilane, benzyl dihydrogen phosphate, N-hydroxysuccinimide condensation agent, and p-toluenesulfonic acid catalyst to toluene solvent, introduce nitrogen protection, react at 50-78°C for 6-10h, and after the reaction is completed, filter, wash and dry to obtain a phosphate flame retardant.

[0009] Preferably, the mass ratio of 4-aminophenyltrimethylsilane, benzyl dihydrogen phosphate, N-hydroxysuccinimide and p-toluenesulfonic acid in S1 is 1:1.25-1.3:0.2-0.4:0.04-0.06.

[0010] Preferably, the preparation method of the modified silica sol is:

[0011] (1) Add di(dimethylamino)methylvinylsilane and 4-chloro-1-butanol to tetrahydrofuran solvent, stir to dissolve, and reflux at 80-95° C. for 3.5-5.5 h. After the reaction is completed, cool, wash and dry to obtain intermediate 1;

[0012] (2) adding intermediate 1 and 3-mercapto-1-propylamine to N,N-dimethylformamide solvent, stirring and mixing, reacting at 42-50° C. for 1.5-2 h, filtering, washing and drying after the reaction to obtain intermediate 2;

[0013] (3) adding intermediate 2, p-hydroxybenzaldehyde and polyformaldehyde to a toluene solvent, reacting at 85-105° C. for 4-6 hours, cooling and distilling under reduced pressure to obtain a quaternary ammonium salt-modified benzoxazine;

[0014] (4) adding silica sol and sodium dodecyl sulfate emulsifier to deionized water, stirring at 50-80° C. for 0.5-1 h, adjusting the pH of the silica sol solution to 6.3-6.5 with acetic acid, heating to 40-60° C., adding 3-aminopropyl triethoxysilane coupling agent, stirring for 1-1.5 h, and after the reaction is completed, concentrating by rotary evaporation to obtain intermediate 3;

[0015] (5) Adding quaternary ammonium salt-modified benzoxazine, intermediate 3, and acetic acid catalyst to methanol solvent, reacting at 30-35° C. for 2.5-4.5 hours, and after the reaction is completed, distilling under reduced pressure to obtain modified silica sol.

[0016] Preferably, the mass ratio of di(dimethylamino)methylvinylsilane to 4-chloro-1-butanol in (1) is 1:1.2-1.4.

[0017] Preferably, the mass ratio of the intermediate 1 to 3-mercapto-1-propylamine in (2) is 1:0.85-0.9.

[0018] Preferably, the mass ratio of the intermediate 2, p-hydroxybenzaldehyde and paraformaldehyde in (3) is 1:1.8-2.2:0.4-0.6.

[0019] Preferably, the mass ratio of silica sol, sodium dodecyl sulfate, acetic acid and 3-aminopropyltriethoxysilane in (4) is 1:0.1-0.3:0.01-0.012:0.35-0.5.

[0020] Preferably, the mass ratio of the quaternary ammonium salt-modified benzoxazine, the intermediate 3, and the acetic acid in (5) is 1:1.3-1.5:0.03-0.035.

[0021] Preferably, the preparation method of the vulcanized natural rubber is:

[0022] Step 1. Add natural rubber to a rubber mixer, mix at 65-85°C for 0.5-1h, then add sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, antioxidant 4020, and continue mixing for 0.5-1.2h. After mixing, let stand for 3-5h to obtain a mixed rubber;

[0023] Step 2. Place the mixed rubber on a vulcanizer and vulcanize it at 170-180°C for 12-20 minutes at a vulcanization pressure of 15-18MPa. After the vulcanization is completed, let it stand for 18-24 hours to obtain vulcanized natural rubber.

[0024] Preferably, in the step 1, the mass ratio of natural rubber, sulfur, lanthanum di-n-octyl dithiocarbamate accelerator, zinc oxide, stearic acid, and antioxidant 4020 is 1:0.5-0.7:0.04-0.08:0.02-0.06:0.1-0.3:0.05-0.07.

[0025] Preferably, the preparation method of the silica sol modified natural rubber is: adding phosphate flame retardant, modified silica sol, vulcanized natural rubber, hydroxyethyl cellulose and carbon black into a reactor, reacting at 95-105° C. for 4.5-6.5 hours to obtain silica sol modified natural rubber.

[0026] (III) Beneficial technical effects

[0027] The invention adds phosphate flame retardant, modified silica sol, vulcanized natural rubber, hydroxyethyl cellulose and carbon black into a reactor, and reacts at 95-105° C. for 4.5-6.5 hours to obtain silica sol modified natural rubber.

[0028] The amino group in 4-aminophenyltrimethylsilane reacts with the phosphoric acid group in benzyl dihydrogen phosphate to introduce phosphorus, nitrogen and silicon elements to obtain a phosphate flame retardant. Di(dimethylamino)methylvinylsilane reacts with 4-chloro-1-butanol to form a quaternary ammonium salt, and silicon and nitrogen are introduced to obtain intermediate 1. The double bond in intermediate 1 reacts with the thiol in 3-mercapto-1-propylamine to introduce sulfur and amino groups to obtain intermediate 2. The amino in intermediate 2 reacts with the phenolic hydroxyl in p-hydroxybenzaldehyde and polyformaldehyde to obtain quaternary ammonium salt-modified benzoxazine and introduce aldehyde groups. Sodium dodecyl sulfate and silica sol are mixed and stirred to obtain an emulsified silica sol solution. The hydroxyl on the surface of the silica particles in the silica sol solution reacts with 3-aminopropyltriethoxysilane coupling agent to form Si-O-Si covalent bonds and introduce amino groups to obtain intermediate 3. The amino in intermediate 3 reacts with the aldehyde in the quaternary ammonium salt-modified benzoxazine to obtain modified silica sol. The polysulfur free radicals generated by sulfur under the action of the accelerator react with the rubber molecular chain to form a cross-linked structure, thereby obtaining vulcanized natural rubber.

[0029] The strong acid generated by phosphorus has dehydration ability, which promotes the rapid dehydration and carbonization of the rubber surface. The formed carbonized layer can effectively block heat transfer, reduce heat conduction, and inhibit carbon oxidation; nitrogen can promote the formation of a stable carbonized layer on the rubber surface, which plays a role in heat insulation and effectively blocks air from entering the rubber bottom layer; silicon dioxide produced by silicon at high temperature can form a dense isolation film on the rubber surface, preventing oxygen from contacting the combustion material, thereby playing a flame retardant role; sulfur can generate non-combustible gas during the combustion process, which can dilute the oxygen concentration in the air and slow down the spread of fire; phosphorus, silicon, nitrogen, and sulfur produce a synergistic effect to further improve the flame retardant properties and mechanical properties of rubber. Mechanical strength; the quaternary ammonium salt groups in the modified silica sol increase the tensile strength of the rubber by increasing the cross-linking points, making the rubber less likely to break when subjected to external forces; benzoxazine can form a solid protective layer on the rubber surface, improving the surface hardness and cutting resistance; the silica sol reacts with the coupling agent to form a stable covalent bond and increase the amino functional group, which improves the adhesion and catalytic activity of the silica sol, fills the gaps in the rubber structure, and increases its density. The addition of the emulsifier also enhances its compatibility and dispersibility with rubber, thereby improving the mechanical strength and stability of the rubber; the cross-linking structure generated by sulfur and rubber strengthens the connection between the rubber molecular chains, thereby improving the strength and elasticity of the rubber. DETAILED DESCRIPTION

[0030] Example 1

[0031] (1) adding 4-aminophenyltrimethylsilane, dihydrogen benzyl phosphate, N-hydroxysuccinimide condensation agent, and p-toluenesulfonic acid catalyst to a toluene solvent, wherein the mass ratio of 4-aminophenyltrimethylsilane, dihydrogen benzyl phosphate, N-hydroxysuccinimide, and p-toluenesulfonic acid is 1:1.25:0.2:0.04, passing nitrogen protection, reacting at 50° C. for 6 hours, filtering after the reaction, washing, and drying to obtain a phosphate flame retardant;

[0032] (2) adding di(dimethylamino)methylvinylsilane and 4-chloro-1-butanol to tetrahydrofuran solvent, wherein the mass ratio of di(dimethylamino)methylvinylsilane to 4-chloro-1-butanol is 1:1.2, stirring and dissolving, and reflux heating at 80° C. for 3.5 h. After the reaction is completed, cooling, washing and drying to obtain intermediate 1;

[0033] (3) adding intermediate 1 and 3-mercapto-1-propylamine to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 1 to 3-mercapto-1-propylamine is 1:0.85, stirring and mixing, reacting at 42° C. for 1.5, and filtering, washing and drying after the reaction to obtain intermediate 2;

[0034] (4) adding intermediate 2, p-hydroxybenzaldehyde and polyformaldehyde to a toluene solvent, wherein the mass ratio of intermediate 2, p-hydroxybenzaldehyde and polyformaldehyde is 1:1.8:0.4, reacting at 85° C. for 4 h, cooling and distilling under reduced pressure after the reaction is completed, to obtain a quaternary ammonium salt-modified benzoxazine;

[0035] (5) Add silica sol and sodium dodecyl sulfate emulsifier to deionized water, stir at 50° C. for 0.5 h, adjust the pH of the silica sol solution to 6.3 with acetic acid, heat to 40° C., and then add 3-aminopropyl triethoxysilane coupling agent, wherein the mass ratio of silica sol, sodium dodecyl sulfate, acetic acid, and 3-aminopropyl triethoxysilane is 1:0.1:0.01:0.35, stir for 1 h, and after the reaction is completed, concentrate by rotary evaporation to obtain intermediate 3;

[0036] (6) adding quaternary ammonium salt-modified benzoxazine, intermediate 3, and acetic acid catalyst to a methanol solvent, wherein the mass ratio of quaternary ammonium salt-modified benzoxazine, intermediate 3, and acetic acid is 1:1.3:0.03, reacting at 30° C. for 2.5 hours, and after the reaction is completed, distilling under reduced pressure to obtain a modified silica sol;

[0037] (7) adding natural rubber to a rubber mixer, mixing at 65° C. for 0.5 h, then adding sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, and antioxidant 4020, wherein the mass ratio of natural rubber, sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, and antioxidant 4020 is 1:0.5:0.04:0.02:0.1:0.05, and mixing is continued for 0.5 h. After the mixing is completed, the mixture is allowed to stand for 3 h to obtain a mixed rubber;

[0038] (8) placing the mixed rubber on a vulcanizer, vulcanizing at 170° C. for 12 min at a vulcanizing pressure of 15 MPa, and standing for 18 h after the vulcanization to obtain a vulcanized natural rubber;

[0039] (9) 8 parts by weight of a phosphate flame retardant, 10 parts by weight of modified silica sol, 18 parts by weight of vulcanized natural rubber, 1 part by weight of hydroxyethyl cellulose, and 4 parts by weight of carbon black were added into a reactor and reacted at 95° C. for 4.5 hours to obtain silica sol-modified natural rubber.

[0040] Example 2

[0041] (1) adding 4-aminophenyltrimethylsilane, dihydrogen benzyl phosphate, N-hydroxysuccinimide condensation agent, and p-toluenesulfonic acid catalyst to a toluene solvent, wherein the mass ratio of 4-aminophenyltrimethylsilane, dihydrogen benzyl phosphate, N-hydroxysuccinimide, and p-toluenesulfonic acid is 1:1.3:0.4:0.06, passing nitrogen protection, reacting at 78° C. for 10 hours, filtering after the reaction, washing, and drying to obtain a phosphate flame retardant;

[0042] (2) adding di(dimethylamino)methylvinylsilane and 4-chloro-1-butanol to tetrahydrofuran solvent, wherein the mass ratio of di(dimethylamino)methylvinylsilane to 4-chloro-1-butanol is 1:1.4, stirring and dissolving, and reflux heating at 95° C. for 5.5 h. After the reaction is completed, cooling, washing and drying to obtain intermediate 1;

[0043] (3) adding intermediate 1 and 3-mercapto-1-propylamine to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 1 to 3-mercapto-1-propylamine is 1:0.9, stirring and mixing, reacting at 50° C. for 2 h, and filtering, washing and drying after the reaction to obtain intermediate 2;

[0044] (4) adding intermediate 2, p-hydroxybenzaldehyde and polyformaldehyde to a toluene solvent, wherein the mass ratio of intermediate 2, p-hydroxybenzaldehyde and polyformaldehyde is 1:2.2:0.6, reacting at 105° C. for 6 h, cooling and distilling under reduced pressure after the reaction is completed, to obtain a quaternary ammonium salt-modified benzoxazine;

[0045] (5) Add silica sol and sodium dodecyl sulfate emulsifier to deionized water, stir at 80° C. for 1 h, adjust the pH of the silica sol solution to 6.5 with acetic acid, heat to 60° C., and then add 3-aminopropyl triethoxysilane coupling agent, wherein the mass ratio of silica sol, sodium dodecyl sulfate, acetic acid, and 3-aminopropyl triethoxysilane is 1:0.3:0.012:0.5, stir for 1.5 h, and after the reaction is completed, concentrate by rotary evaporation to obtain intermediate 3;

[0046] (6) adding quaternary ammonium salt-modified benzoxazine, intermediate 3, and acetic acid catalyst to a methanol solvent, wherein the mass ratio of quaternary ammonium salt-modified benzoxazine, intermediate 3, and acetic acid is 1:1.5:0.035, reacting at 35° C. for 4.5 hours, and after the reaction is completed, distilling under reduced pressure to obtain a modified silica sol;

[0047] (7) adding natural rubber to a rubber mixer, mixing at 85° C. for 1 h, then adding sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, and antioxidant 4020, wherein the mass ratio of natural rubber, sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, and antioxidant 4020 is 1:0.7:0.08:0.06:0.3:0.07, and mixing is continued for 1.2 h. After the mixing is completed, the mixture is allowed to stand for 5 h to obtain a mixed rubber;

[0048] (8) placing the mixed rubber on a vulcanizer, vulcanizing at 180° C. for 20 min at a vulcanizing pressure of 18 MPa, and standing for 24 h after the vulcanization to obtain a vulcanized natural rubber;

[0049] (9) 10 parts by weight of a phosphate flame retardant, 15 parts by weight of a modified silica sol, 26 parts by weight of vulcanized natural rubber, 3 parts by weight of hydroxyethyl cellulose, and 6 parts by weight of carbon black were added into a reactor and reacted at 105° C. for 6.5 hours to obtain a silica sol-modified natural rubber.

[0050] Example 3

[0051] (1) adding 4-aminophenyltrimethylsilane, dihydrogen benzyl phosphate, N-hydroxysuccinimide condensation agent, and p-toluenesulfonic acid catalyst to a toluene solvent, wherein the mass ratio of 4-aminophenyltrimethylsilane, dihydrogen benzyl phosphate, N-hydroxysuccinimide, and p-toluenesulfonic acid is 1:1.27:0.3:0.05, introducing nitrogen protection, reacting at 64° C. for 8 hours, filtering after the reaction, washing, and drying to obtain a phosphate flame retardant;

[0052] (2) adding di(dimethylamino)methylvinylsilane and 4-chloro-1-butanol to tetrahydrofuran solvent, wherein the mass ratio of di(dimethylamino)methylvinylsilane to 4-chloro-1-butanol is 1:1.3, stirring and dissolving, and reflux heating at 87° C. for 4.5 h. After the reaction is completed, cooling, washing and drying to obtain intermediate 1;

[0053] (3) adding intermediate 1 and 3-mercapto-1-propylamine to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 1 to 3-mercapto-1-propylamine is 1:0.87, stirring and mixing, reacting at 46° C. for 1.7 h, and filtering, washing and drying after the reaction to obtain intermediate 2;

[0054] (4) adding intermediate 2, p-hydroxybenzaldehyde and polyformaldehyde to a toluene solvent, wherein the mass ratio of intermediate 2, p-hydroxybenzaldehyde and polyformaldehyde is 1:2:0.5, reacting at 95° C. for 5 h, cooling and distilling under reduced pressure after the reaction is completed, to obtain a quaternary ammonium salt-modified benzoxazine;

[0055] (5) Add silica sol and sodium dodecyl sulfate emulsifier to deionized water, stir at 65° C. for 0.7 h, adjust the pH of the silica sol solution to 6.4 with acetic acid, heat to 50° C., and then add 3-aminopropyl triethoxysilane coupling agent, wherein the mass ratio of silica sol, sodium dodecyl sulfate, acetic acid, and 3-aminopropyl triethoxysilane is 1:0.2:0.011:0.4, stir for 1.2 h, and after the reaction is completed, concentrate by rotary evaporation to obtain intermediate 3;

[0056] (6) adding quaternary ammonium salt-modified benzoxazine, intermediate 3, and acetic acid catalyst to a methanol solvent, wherein the mass ratio of quaternary ammonium salt-modified benzoxazine, intermediate 3, and acetic acid is 1:1.4:0.032, reacting at 32° C. for 3.5 hours, and after the reaction is completed, distilling under reduced pressure to obtain a modified silica sol;

[0057] (7) adding natural rubber to a rubber mixer, mixing at 75° C. for 0.7 h, then adding sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, and antioxidant 4020, wherein the mass ratio of natural rubber, sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, and antioxidant 4020 is 1:0.6:0.06:0.04:0.2:0.06, and mixing is continued for 0.8 h. After the mixing is completed, the mixture is allowed to stand for 4 h to obtain a mixed rubber;

[0058] (8) placing the mixed rubber on a vulcanizer, vulcanizing at 175° C., the vulcanizing time is 16 min, the vulcanizing pressure is 16.5 MPa, and after the vulcanization is completed, standing for 21 h to obtain a vulcanized natural rubber;

[0059] (9) 9 parts by weight of a phosphate flame retardant, 12 parts by weight of a modified silica sol, 17 parts by weight of a vulcanized natural rubber, 2 parts by weight of hydroxyethyl cellulose, and 5 parts by weight of carbon black were added into a reactor and reacted at 100° C. for 5.5 hours to obtain a silica sol-modified natural rubber.

[0060] Example 4

[0061] (1) adding 4-aminophenyltrimethylsilane, dihydrogen benzyl phosphate, N-hydroxysuccinimide condensation agent, and p-toluenesulfonic acid catalyst to a toluene solvent, wherein the mass ratio of 4-aminophenyltrimethylsilane, dihydrogen benzyl phosphate, N-hydroxysuccinimide, and p-toluenesulfonic acid is 1:1.25:0.2:0.04, passing nitrogen protection, reacting at 50° C. for 6 hours, filtering after the reaction, washing, and drying to obtain a phosphate flame retardant;

[0062] (2) adding di(dimethylamino)methylvinylsilane and 4-chloro-1-butanol to tetrahydrofuran solvent, wherein the mass ratio of di(dimethylamino)methylvinylsilane to 4-chloro-1-butanol is 1:1.2, stirring and dissolving, and reflux heating at 80° C. for 3.5 h. After the reaction is completed, cooling, washing and drying to obtain intermediate 1;

[0063] (3) adding intermediate 1 and 3-mercapto-1-propylamine to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 1 to 3-mercapto-1-propylamine is 1:0.85, stirring and mixing, reacting at 42° C. for 1.5, and filtering, washing and drying after the reaction to obtain intermediate 2;

[0064] (4) adding intermediate 2, p-hydroxybenzaldehyde and polyformaldehyde to a toluene solvent, wherein the mass ratio of intermediate 2, p-hydroxybenzaldehyde and polyformaldehyde is 1:2.2:0.6, reacting at 105° C. for 6 h, cooling and distilling under reduced pressure after the reaction is completed, to obtain a quaternary ammonium salt-modified benzoxazine;

[0065] (5) Add silica sol and sodium dodecyl sulfate emulsifier to deionized water, stir at 80° C. for 1 h, adjust the pH of the silica sol solution to 6.5 with acetic acid, heat to 60° C., and then add 3-aminopropyl triethoxysilane coupling agent, wherein the mass ratio of silica sol, sodium dodecyl sulfate, acetic acid, and 3-aminopropyl triethoxysilane is 1:0.3:0.012:0.5, stir for 1.5 h, and after the reaction is completed, concentrate by rotary evaporation to obtain intermediate 3;

[0066] (6) adding quaternary ammonium salt-modified benzoxazine, intermediate 3, and acetic acid catalyst to a methanol solvent, wherein the mass ratio of quaternary ammonium salt-modified benzoxazine, intermediate 3, and acetic acid is 1:1.5:0.035, reacting at 35° C. for 4.5 hours, and after the reaction is completed, distilling under reduced pressure to obtain a modified silica sol;

[0067] (7) adding natural rubber to a rubber mixer, mixing at 75° C. for 0.7 h, then adding sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, and antioxidant 4020, wherein the mass ratio of natural rubber, sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, and antioxidant 4020 is 1:0.6:0.06:0.04:0.2:0.06, and mixing is continued for 0.8 h. After the mixing is completed, the mixture is allowed to stand for 4 h to obtain a mixed rubber;

[0068] (8) placing the rubber mixture on a vulcanizer, vulcanizing the mixture at 175° C. for 16 min at a vulcanizing pressure of 16.5 MPa, and standing the mixture for 21 h to obtain a vulcanized natural rubber;

[0069] (9) 9 parts by weight of a phosphate flame retardant, 12 parts by weight of a modified silica sol, 17 parts by weight of a vulcanized natural rubber, 2 parts by weight of hydroxyethyl cellulose, and 5 parts by weight of carbon black were added into a reactor and reacted at 100° C. for 5.5 hours to obtain a silica sol-modified natural rubber.

[0070] Comparative Example 1

[0071] Compared with Example 4, the comparative example is characterized in that no phosphate flame retardant is added.

[0072] Comparative Example 2

[0073] Compared with Example 4, this comparative example is characterized in that no modified silica sol is added.

[0074] The limiting oxygen index of the material was tested using an oxygen index meter, and the combustion grade of the material was tested using a horizontal and vertical combustion instrument. The test results are shown in Table 1.

[0075] Table 1: Flame retardancy tests.

[0076] project Limiting oxygen index (%) Combustion level Example 1 32 V-0 Example 2 31 V-0 Example 3 34 V-0 Example 4 33 V-0 Comparative Example 1 23 V-1 Comparative Example 2 22 V-1

[0077] It can be seen from Table 1 that Examples 1-4 of the present invention have better flame retardant effects than Comparative Examples 1-2.

[0078] The tensile stress, tensile strength and elongation at break are tested according to the corresponding national standards. The tensile rate is 450mm / min, and the tear strength test uses a right-angle specimen.

[0079] Table 2: Tests of various physical performance indicators.

[0080]

[0081] It can be seen from Table 2 that Examples 1-4 and Comparative Example 1 of the present invention have better tear resistance than Comparative Example 2.

[0082] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A silica sol modified natural rubber, characterized in that: The invention comprises the following components by weight: 8-10 parts by weight of a phosphate flame retardant, 10-15 parts by weight of a modified silica sol, 18-26 parts by weight of vulcanized natural rubber, 1-3 parts by weight of hydroxyethyl cellulose and 4-6 parts by weight of carbon black.

2. The silica sol-modified natural rubber according to claim 1, characterized in that: The preparation method of the phosphate flame retardant is: S1. Add 4-aminophenyltrimethylsilane, benzyl dihydrogen phosphate, N-hydroxysuccinimide condensation agent, and p-toluenesulfonic acid catalyst to toluene solvent, introduce nitrogen protection, react at 50-78°C for 6-10h, and after the reaction, filter, wash and dry to obtain a phosphate flame retardant. The mass ratio of 4-aminophenyltrimethylsilane, benzyl dihydrogen phosphate, N-hydroxysuccinimide, and p-toluenesulfonic acid in S1 is 1:1.25-1.3:0.2-0.4:0.04-0.

06.

3. The silica sol-modified natural rubber according to claim 1, characterized in that: The preparation method of the modified silica sol is: (1) Add di(dimethylamino)methylvinylsilane and 4-chloro-1-butanol to tetrahydrofuran solvent, stir to dissolve, and reflux at 80-95° C. for 3.5-5.5 h. After the reaction is completed, cool, wash and dry to obtain intermediate 1; (2) adding intermediate 1 and 3-mercapto-1-propylamine to N,N-dimethylformamide solvent, stirring and mixing, reacting at 42-50° C. for 1.5-2 h, filtering, washing and drying after the reaction to obtain intermediate 2; (3) adding intermediate 2, p-hydroxybenzaldehyde and polyformaldehyde to a toluene solvent, reacting at 85-105° C. for 4-6 hours, cooling and distilling under reduced pressure to obtain a quaternary ammonium salt-modified benzoxazine; (4) adding silica sol and sodium dodecyl sulfate emulsifier to deionized water, stirring at 50-80° C. for 0.5-1 h, adjusting the pH of the silica sol solution to 6.3-6.5 with acetic acid, heating to 40-60° C., adding 3-aminopropyl triethoxysilane coupling agent, stirring for 1-1.5 h, and after the reaction is completed, concentrating by rotary evaporation to obtain intermediate 3; (5) Adding quaternary ammonium salt-modified benzoxazine, intermediate 3, and acetic acid catalyst to methanol solvent, reacting at 30-35° C. for 2.5-4.5 hours, and after the reaction is completed, distilling under reduced pressure to obtain modified silica sol.

4. The silica sol-modified natural rubber according to claim 3, characterized in that: The mass ratio of di(dimethylamino)methylvinylsilane to 4-chloro-1-butanol in (1) is 1:1.2-1.

4.

5. The silica sol-modified natural rubber according to claim 3, characterized in that: The mass ratio of the intermediate 1 and 3-mercapto-1-propylamine in (2) is 1:0.85-0.

9.

6. The silica sol-modified natural rubber according to claim 3, characterized in that: The mass ratio of the intermediate 2, p-hydroxybenzaldehyde and paraformaldehyde in (3) is 1:1.8-2.2:0.4-0.

6.

7. The silica sol-modified natural rubber according to claim 3, characterized in that: The mass ratio of silica sol, sodium dodecyl sulfate, acetic acid and 3-aminopropyltriethoxysilane in (4) is 1:0.1-0.3:0.01-0.012:0.35-0.

5.

8. The silica sol-modified natural rubber according to claim 3, characterized in that: The mass ratio of the quaternary ammonium salt-modified benzoxazine, the intermediate 3, and the acetic acid in (5) is 1:1.3-1.5:0.03-0.

035.

9. The silica sol-modified natural rubber according to claim 1, characterized in that: The preparation method of the vulcanized natural rubber is: Step 1. Add natural rubber to a rubber mixer, mix at 65-85°C for 0.5-1h, add sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, antioxidant 4020, and continue mixing for 0.5-1.2h. After the mixing is completed, let it stand for 3-5h to obtain a mixed rubber. The mass ratio of natural rubber, sulfur, lanthanum dioctyl dithiocarbamate accelerator, zinc oxide, stearic acid, and antioxidant 4020 in the step 1 is 1: 0.5-0.7: 0.04-0.08: 0.02-0.06: 0.1-0.3: 0.05-0.07; Step 2. Place the mixed rubber on a vulcanizer and vulcanize it at 170-180°C for 12-20 minutes at a vulcanization pressure of 15-18MPa. After the vulcanization is completed, let it stand for 18-24 hours to obtain vulcanized natural rubber.

10. A method for preparing silica sol-modified natural rubber according to any one of claims 1 to 9, characterized in that: The preparation method of the silica sol modified natural rubber is as follows: adding phosphate flame retardant, modified silica sol, vulcanized natural rubber, hydroxyethyl cellulose and carbon black into a reactor, reacting at 95-105° C. for 4.5-6.5 hours to obtain the silica sol modified natural rubber.

Citation Information

Patent Citations

  • Method for modifying natural rubber, and modified natural rubber

    CN102124034B

  • Silicone resins and their use in polymers

    CN103946279A

  • High-strength oil-resistant modified natural rubber composite

    CN105754168A

  • Halogen-free environment-friendly flame-retardant rubber and preparation method thereof

    CN116082718A

  • Rubber composition for railway vehicle cushion rubber

    JP2019001833A

Cited By

  • Anti-caking composite rubber antioxidant 6PPD and preparation method thereof

    CN120484524A

  • High-performance natural rubber containing modified silica sol and preparation method thereof

    CN121378902A