Anti-freezing and anti-seepage coating based on fluorosilane modified epoxy resin and preparation method of anti-freezing and anti-seepage coating

By introducing fluorosilanes and silanes into fluorosilane-modified epoxy resin to form a covalent network structure, the problem of insufficient adhesion of fluorosilane coatings is solved, achieving high adhesion and antifreeze and seepage prevention effects on concrete surfaces.

CN118995008AActive Publication Date: 2024-11-22BEIJING ACAD OF BUILDING ENG +1

Patent Information

Application Number
CN202411330760.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-22
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

Fluorosilane coatings have poor adhesion to concrete surfaces and are prone to peeling off under freeze-thaw cycles, failing to effectively prevent water penetration and resist frost damage.

Method used

By introducing fluorosilane-modified epoxy resin, combining fluoroalkanes and silanes with epoxy compounds to form a covalent network structure, the adhesion between the coating and concrete is enhanced, thus preparing an antifreeze and seepage-proof coating.

Benefits of technology

It improves the adhesion of the coating to the concrete surface, enhances the antifreeze and anti-seepage properties, and extends the service life of the concrete structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995008A_ABST
    Figure CN118995008A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of concrete protection, and particularly relates to an anti-freezing and anti-seepage coating based on fluorosilane modified epoxy resin and a preparation method of the anti-freezing and anti-seepage coating. The anti-freezing and anti-seepage coating based on the fluorosilane modified epoxy resin is prepared from 30 to 40 parts of fluorosilane modified epoxy resin, 30 to 60 parts of a curing agent, 0.5 to 1.5 parts of a curing accelerator and 1 to 2.5 parts of a wetting agent, wherein the fluorosilane modified epoxy resin is synthesized by grafting reaction of fluoroalkyl, silane substances and an epoxy compound; the epoxy compound is composed of bisphenol A epoxy resin and polyfunctional glycidyl ether resin. The curing agent comprises a polyamine curing agent and a polysulfide rubber curing agent. The anti-freezing and anti-seepage coating based on the fluorosilane modified epoxy resin can form a hydrophobic low-surface-energy structure on the surface of concrete, and corrosion ions and an aqueous solution are inhibited from permeating into the concrete; meanwhile, the coating based on the fluorosilane modified resin has good permeability and water vapor permeability, the coating is endowed with excellent freeze-thaw resistance, and the service life of concrete engineering is effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete protection, and specifically relates to an antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin and a preparation method thereof. Background Art

[0002] Concrete has the advantages of good structural stability, durability, and economy. It can meet various engineering needs and plays an important role in modern construction and infrastructure construction. In the complex climate environment of cold regions, the coupling of multiple factors such as freeze-thaw cycles, salt erosion, and dry-wet alternation leads to significant deterioration of the mechanical properties of concrete materials. Under the action of freeze-thaw cycles, concrete will produce internal and external cracks, resulting in a decrease in structural strength and stiffness, and even causing steel corrosion. Freeze-thaw cycles will cause the basic mechanical properties and deformation properties of concrete, such as compressive strength, tensile strength, elastic modulus, and deformation characteristics, to decrease, thereby reducing the performance and bearing capacity of concrete structures, and significantly affecting the durability of hydraulic concrete in cold regions.

[0003] Inhibiting the penetration of water into concrete is an effective way to enhance the frost resistance and cold resistance of concrete. Applying organic coatings on the surface of concrete, such as epoxy, acrylic, chlorinated rubber, polyurethane, etc., forms a dense protective film on the surface of concrete to prevent the penetration and diffusion of water in the pores of concrete, thereby achieving the effect of waterproofing and antifreeze. Traditional organic coatings achieve waterproofing by sealing the pores of concrete, but it is difficult to achieve a hydrophobic effect and cannot guarantee the use of concrete projects in high-cold areas to resist frost damage. Fluorocarbon and silane materials have low surface energy, and fluorosilane has good permeability in concrete. It is easy to form a hydrophobic structure on the surface of concrete and the surface of pores, greatly enhancing the hydrophobicity of concrete. However, the existing fluorosilane coatings have low adhesion on the concrete surface and are easy to fall off in harsh and complex environments, which seriously restricts the frost resistance and anti-seepage performance of concrete.

[0004] Therefore, there is an urgent need to develop concrete coatings with high adhesion and excellent anti-freeze and anti-seepage properties to enable the concrete to serve stably in high cold and harsh environments. Summary of the invention

[0005] Technical issues:

[0006] Since concrete needs to experience temperatures as low as minus twenty degrees Celsius during freeze-thaw cycles, the resin molecular chains in the fluorosilane coating freeze, reducing the bonding effect between the coating and the concrete interface, causing the coating on the concrete surface to peel off and fall off, and the purpose of concrete antifreeze cannot be achieved. In response to the above difficulties, the present invention uses a technical method to enhance the adhesion of concrete surface coatings through resin molecular network design, and introduces components that strongly interact with concrete into the coating to enhance the adhesion of the coating during freeze-thaw cycles, thereby achieving the purpose of concrete antifreeze and anti-seepage.

[0007] Technical solution:

[0008] One object of the present invention is to provide a frost-resistant and anti-seepage coating for concrete surface to solve the problem of frost damage in current concrete engineering in cold regions.

[0009] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:

[0010] An antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin and a preparation method thereof, characterized in that the coating comprises the following raw materials in parts by weight: 30-40 parts of fluorosilane-modified epoxy resin, 30-60 parts of curing agent, 0.5-1.5 parts of curing accelerator, and 1-2.5 parts of wetting agent.

[0011] Furthermore, the fluorosilane-modified epoxy resin is composed of fluoroalkane, silane-like substances and epoxy compounds, and the mass ratio of the fluorosilane to the epoxy compound is 1:3-1:10.

[0012] Furthermore, the fluoroalkane is one of perfluorooctane sulfonamide and perfluorohexyl sulfonamide; the silane is one of aminopropyl di-terminated polydimethylsiloxane, 3-aminopropyl triethoxysilane, and aminopropyl isooctyl cage-shaped silsesquioxane.

[0013] Furthermore, the epoxy compound is composed of bisphenol A epoxy resin and multifunctional glycidyl ether resin, and the mass ratio of the bisphenol A epoxy resin to the multifunctional glycidyl ether resin is 4:1-10:1.

[0014] Furthermore, the mass percentage of fluorocarbon in the fluorocarbon and silane substances is 20%-40%, and the rest is silane.

[0015] Furthermore, the bisphenol A epoxy resin is any one of E51, E35, and E20; the multifunctional glycidyl ether resin is one of glycerol triglycidyl ether, trimethylol propane triglycidyl ether, and polypropylene glycol diglycidyl ether.

[0016] Furthermore, the curing agent is one of triethylenetetramine, polyamide 650 and diaminodiphenylmethane.

[0017] Furthermore, the curing agent accelerator is one of aminophenol, methyldiethanolamine and salicylic acid.

[0018] Furthermore, the wetting agent is one of octadecenylamine acetate, aminopropylamine dioleate, and fatty acid ethylene oxide adduct.

[0019] Another object of the present invention is to provide a method for preparing an antifreeze and anti-seepage coating based on a fluorosilane-modified epoxy resin, comprising the following steps:

[0020] (1) mixing a bisphenol A epoxy resin and a multifunctional glycidyl ether resin, and mixing them under mechanical stirring (300-600 r / min) for 10-20 min to obtain an epoxy compound;

[0021] (2) uniformly mixing the epoxy compound with fluoroalkane and silane, and reacting at 60-90° C. for 5-10 hours to obtain a fluorosilane-modified epoxy resin;

[0022] (3) The fluorosilane-modified epoxy resin, curing agent, curing agent accelerator, and wetting agent are mixed evenly and allowed to stand for 10-15 minutes to obtain an antifreeze and anti-seepage coating based on the fluorosilane-modified epoxy resin.

[0023] Beneficial effects:

[0024] (1) The antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin provided by the present invention introduces fluorosilane substances with low surface energy and high permeability into the resin network structure in a covalent manner through a polymer chemical modification method, thereby giving the coating excellent water-blocking and antifreeze properties and improving the service life of concrete.

[0025] (2) The antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin provided by the present invention utilizes the interfacial effect between the silane structure in the resin molecular chain and concrete to significantly enhance the adhesion of the coating; the antifreeze and anti-seepage coating provided by the present invention has a simple construction method, a wide range of applications, is easy to apply on a large scale, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the molecular structure of the fluorosilane-modified epoxy resin in Example 1.

[0027] Figure 2 This is a test diagram of the adhesion of the antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin on the concrete surface in Example 1. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It is worth noting that the following embodiments are only preferred embodiments of the present invention and should not be construed as limiting the present invention. The protection scope of the present invention shall be subject to the contents recorded in the claims. Any modification or replacement made by a person skilled in the art to the technical solution of the present invention without creative work shall fall within the protection scope of the present invention.

[0029] Example 1

[0030] (1) 5 g of E51 epoxy resin and 1 g of glycerol triglycidyl ether were mixed and mixed for 10 min under mechanical stirring (300 r / min) to obtain an epoxy compound;

[0031] (2) 5 g of epoxy compound, 0.5 g of perfluorooctane sulfonamide and 0.5 g of aminopropyl dicapped polydimethylsiloxane were mixed evenly and reacted at 60° C. for 6 h to obtain fluorosilane-modified epoxy resin ( Figure 1 );

[0032] (3) Take 3 parts of fluorosilane-modified epoxy resin, 3 parts of polyamide 650, 0.5 parts of aminophenol, and 1 part of aminopropylamine dioleate, mix them evenly, and let them stand for 10 minutes to obtain an antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin.

[0033] Figure 2 This is a test diagram of the adhesion of the antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin on the concrete surface in this embodiment. It can be seen that the bonding force is as high as 8.07 MPa, indicating that the prepared antifreeze and anti-seepage coating has excellent adhesion performance on the concrete surface.

[0034] Example 2

[0035] (1) 5 g of E44 epoxy resin and 1 g of polypropylene glycol diglycidyl ether were mixed and mixed for 10 min under mechanical stirring (300 r / min) to obtain an epoxy compound;

[0036] (2) 5 g of epoxy compound, 0.5 g of perfluorooctane sulfonamide and 0.5 g of aminopropyl di-terminated polydimethylsiloxane were mixed evenly, and reacted at 60° C. for 6 h to obtain a fluorosilane-modified epoxy resin;

[0037] (3) Take 3 parts of fluorosilane-modified epoxy resin, 3 parts of polyamide 650, 0.5 parts of aminophenol, and 1 part of aminopropylamine dioleate, mix them evenly, and let them stand for 10 minutes to obtain an antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin.

[0038] Example 3

[0039] (1) 5 g of E51 epoxy resin and 1 g of glycerol triglycidyl ether were mixed and mixed for 10 min under mechanical stirring (300 r / min) to obtain an epoxy compound;

[0040] (2) 5 g of epoxy compound, 0.5 g of perfluorooctane sulfonamide and 0.5 g of aminopropyl isooctyl cage-shaped silsesquioxane were mixed evenly, and reacted at 60° C. for 6 h to obtain a fluorosilane-modified epoxy resin;

[0041] (3) Take 3 parts of fluorosilane-modified epoxy resin, 3 parts of polyamide 650, 0.5 parts of aminophenol, and 1 part of aminopropylamine dioleate, mix them evenly, and let them stand for 15 minutes to obtain an antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin.

[0042] Example 4

[0043] (1) 5 g of E51 epoxy resin and 1 g of trimethylolpropane triglycidyl ether were mixed and mixed for 12 min under mechanical stirring (300 r / min) to obtain an epoxy compound;

[0044] (2) 5 g of epoxy compound, 0.5 g of perfluorohexylsulfonamide and 0.5 g of aminopropylisooctyl cage-shaped silsesquioxane were mixed evenly, and reacted at 60° C. for 6 h to obtain a fluorosilane-modified epoxy resin;

[0045] (3) Take 3 parts of fluorosilane-modified epoxy resin, 3 parts of diaminodiphenylmethane, 0.5 parts of aminophenol, and 1 part of aminopropylamine dioleate, mix them evenly, and let them stand for 15 minutes to obtain an antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin.

[0046] Comparative Example 1

[0047] (1) 5 g of E51 epoxy resin and 1 g of glycerol triglycidyl ether were mixed and mixed for 10 min under mechanical stirring (300 r / min) to obtain an epoxy compound;

[0048] (2) 3 parts of epoxy compound, 3 parts of polyamide 650, 0.5 parts of aminophenol and 1 part of aminopropylamine dioleate were mixed evenly and allowed to stand for 10 minutes to obtain an antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin.

[0049] Comparative Example 2

[0050] (1) 5 g of E51 epoxy resin and 1 g of glycerol triglycidyl ether were mixed and mixed for 10 min under mechanical stirring (300 r / min) to obtain an epoxy compound;

[0051] (2) 5 g of epoxy compound and 0.5 g of perfluorohexylsulfonamide were mixed evenly and reacted at 60° C. for 6 h to obtain a fluorocarbon-modified epoxy resin;

[0052] (2) 3 parts of fluorosilane-modified epoxy resin, 3 parts of polyamide 650, 0.5 parts of aminophenol, and 1 part of aminopropylamine dioleate were mixed evenly and allowed to stand for 10 minutes to obtain an antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin.

[0053] Comparative Example 3

[0054] (1) 5 g of E51 epoxy resin and 1 g of glycerol triglycidyl ether were mixed and mixed for 10 min under mechanical stirring (300 r / min) to obtain an epoxy compound;

[0055] (2) 5 g of the epoxy compound and 0.5 g of aminopropyl dicapped polydimethylsiloxane were mixed uniformly, and reacted at 60° C. for 6 h to obtain a fluorocarbon-modified epoxy resin;

[0056] (2) Take 3 parts of silane-modified epoxy resin, 3 parts of polyamide 650, 0.5 parts of aminophenol, and 1 part of aminopropylamine dioleate, mix them evenly, and let them stand for 10 minutes to obtain an antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin.

Claims

1. An antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin, characterized in that: The coating comprises the following raw materials in parts by weight: 30-40 parts of fluorosilane-modified epoxy resin, 30-60 parts of curing agent, 0.5-1.5 parts of curing accelerator, and 1-2.5 parts of wetting agent; the fluorosilane-modified epoxy resin is composed of fluorocarbon and silane substances and epoxy compounds, and the mass ratio of the fluorocarbon and silane substances to the epoxy compounds is 1:3-1:

10.

2. The antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin according to claim 1, characterized in that: The mass percentage of fluorocarbon in the fluorocarbon and silane substances is 20%-40%, and the rest is silane.

3. The antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin according to claim 1, characterized in that: The fluoroalkane is one of perfluorooctane sulfonamide and perfluorohexyl sulfonamide; the silane is one of aminopropyl di-terminated polydimethylsiloxane, 3-aminopropyl triethoxysilane, and aminopropyl isooctyl cage-shaped silsesquioxane.

4. The antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin according to claim 1, characterized in that: The epoxy compound is composed of bisphenol A epoxy resin and multifunctional glycidyl ether resin, and the mass ratio of the bisphenol A epoxy resin to the multifunctional glycidyl ether resin is 4:1-10:

1.

5. The antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin according to claim 4, characterized in that: The bisphenol A epoxy resin is any one of E44, E35, and E20; the multifunctional glycidyl ether resin is one of glycerol triglycidyl ether, trimethylol propane triglycidyl ether, and polypropylene glycol diglycidyl ether.

6. The antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin according to claim 1, characterized in that: The curing agent is one of triethylenetetramine, polyamide 650 and diaminodiphenylmethane.

7. The antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin according to claim 1, characterized in that: The curing agent accelerator is one of aminophenol, methyldiethanolamine and salicylic acid.

8. The antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin according to claim 1, characterized in that: The wetting agent is one of octadecenylamine acetate, aminopropylamine dioleate, and fatty acid ethylene oxide adduct.

9. A method for preparing an antifreeze and anti-seepage coating based on fluorosilane-modified epoxy resin according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) fully mixing a bisphenol A epoxy resin and a multifunctional glycidyl ether resin to obtain an epoxy compound; (2) uniformly mixing the epoxy compound with fluoroalkane and silane, and reacting at 60-90° C. for 5-10 hours to obtain a fluorosilane-modified epoxy resin; (3) Evenly mix the fluorosilane-modified epoxy resin, curing agent, curing agent accelerator, and wetting agent, and let stand for 10-15 minutes to obtain an antifreeze and anti-seepage coating.

Citation Information

Patent Citations

  • Permeable epoxy resin waterproof coating for concrete

    CN102504670A

  • Fluorine-containing epoxy resin and preparation method thereof, and double-super-hydrophobic surface preparing from fluorine-containing epoxy resin

    CN103588955A

  • Flurosilicon graft polymer-grafted epoxy resin and preparation method thereof

    CN103627003A

  • Super-amphiphobic anticorrosive coating based on fluorine-silicon modified epoxy resin and preparation method of super-amphiphobic anticorrosive coating

    CN106928807A

  • Fluorine-containing epoxy resin, black hydrophobic oleophobic composition prepared from resin and waterproof oleophobic gas-permeable film and structure

    CN108546326A

Cited By

  • Surface treatment mode of corrosion-resistant high-strength steel bar and concrete of corrosion-resistant high-strength steel bar

    CN120815705A

  • Surface treatment method of corrosion-resistant high-strength steel bar and concrete thereof

    CN120815705B

  • Anti-permeability composite coating, anti-permeability composite coating and preparation method and application of anti-permeability composite coating

    CN121518032A