Preparation method of bio-based corrosion and rust inhibitor composition for steel

By preparing a bio-based corrosion-proofing and anti-rust agent composition containing rosin, resin acid and other components, the problem that traditional anti-rust agents cannot prevent bio-based damage of steel is solved, and the multi-layer film formation and corrosion prevention on the surface of the steel are realized. Significantly extends the service life of the steel.

CN118995299APending Publication Date: 2024-11-22SANXIANG POLYMER (HUBEI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411089985.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional anti-rust agents cannot prevent damage to the steel biomass during use, resulting in the inability to increase the service life of the steel.

Method used

Using a bio-based corrosion inhibiting and anti-rust composition including rosin, resin acid, maleic anhydride, catalyst, methylphenyl sulfur and glacial acetic acid, it is prepared by extraction and heating, and it can form a multi-forming agent on the surface of the steel. Layer film, anti-rust agent to prevent corrosion.

Benefits of technology

This method can effectively prevent steel from rusting, has good hydrolysis resistance and anti-rust water thickening effect, so that the anti-rust agent firmly adheres to the metal surface, significantly extending the service life of the steel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a bio-based corrosion inhibition antirust agent composition for steel, and relates to the technical field of antirust agents, and the preparation method comprises the following steps: step 1, preparing the bio-based corrosion inhibition antirust agent composition from the following components in parts by weight: 1-3 parts of rosin, 1-2 parts of resin acid, 2-5 parts of maleic anhydride, 2-4 parts of a catalyst, 2-4 parts of methyl benzene sulfur and 6-12 parts of a solvent glacial acetic acid; 2, resin acid is extracted from rosin, the resin acid and maleic anhydride are mixed and heated, and continuous heating is conducted for 5-9 h. The solution can prevent steel from rusting, has good hydrolysis resistance, and has a thickening effect on antirust water, so that an antirust agent is prevented from being lost from the metal surface, and the antirust agent is firmly attached to the metal surface. The antirust agent can form multiple layers of films on the surface of carbon steel within a short time, the inner layer is a reaction deposition type film, the binding force between the inner layer and matrix metal is high, and therefore the metal is effectively prevented from being rusted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of rust inhibitors, and in particular to a method for preparing a bio-based corrosion inhibitor and rust inhibitor composition for steel. Background Art

[0002] Metal parts are prone to rusting during production, processing, and transportation, necessitating the use of rust-preventing oils, which form a thin film on the metal surface and prevent chemical corrosion. Rust is a mixture of oxides and hydroxides formed by the action of oxygen and water on the metal surface. Iron rust is red, copper rust is green, and aluminum and zinc rust is called white rust. During operation and storage, machinery is often exposed to oxygen, moisture, or other corrosive media in the air. These substances will electrochemically corrode the metal surface, causing rust. Preventing rust requires preventing these substances from coming into contact with the metal. Rust inhibitors are one type of rust-preventing product; other types include rust-preventing oils and paper.

[0003] However, traditional rust inhibitors cannot inhibit the corrosion of steel when used, cannot prevent the biomass of steel from being damaged when used, and cannot extend the service life of steel. Summary of the Invention

[0004] (1) Technical problems solved In view of the shortcomings of the existing technology, the present invention provides a method for preparing a bio-based corrosion inhibitor and rust preventive composition for steel, so as to solve the problem that the bio-based steel cannot be prevented from being damaged during use and the service life of the steel cannot be increased.

[0005] (2) Technical solution To achieve the above objectives, the present invention is implemented through the following technical solutions: A method for preparing a bio-based corrosion inhibitor and rust preventer composition for steel, comprising the following steps: Step 1: The following preparation methods are included by weight: 1-3 parts of rosin, 1-2 parts of resin acid, 2-5 parts of maleic anhydride, 2-4 parts of catalyst, 2-4 parts of methylbenzene sulfide, and 6-12 parts of glacial acetic acid as solvent; Step 2: Extract resin acid from rosin, mix resin acid with maleic anhydride and heat, and continue heating for 5-9 hours.

[0006] Preferably, the resin acid in step 1 is extracted from rosin. During the extraction, the rosin powder is first dissolved and then allowed to stand. The liquid will precipitate after standing. After precipitation, the upper layer of the liquid is clear and the lower layer of the liquid is precipitated material. After clarification, the liquid is filtered to remove impurities.

[0007] Preferably, the filtered filtrate is transferred to a heating tank for heating, cyclohexylamine is added during the heating process of the filtrate, and the material is precipitated after cooling, the precipitated material is vacuum dried, the precipitated material is mixed, stirred and heated with ether, and the liquid is separated after mixing and heating.

[0008] Preferably, during the mixing in step 2, the resin acid, methylbenzenesulfuric acid, maleic anhydride and glacial acetic acid are stirred and mixed respectively, and nitrogen is injected into the materials in the tank after mixing.

[0009] Preferably, after nitrogen is filled, the mixing tank is heated and heated, and after the temperature is raised, the stability of the mixing tank is reduced, and after the stability is reduced, glacial acetic acid is heated, and after the mixing tank is added, it is cooled to room temperature, and then quickly cooled with cold water to obtain a white pure product after cooling.

[0010] Preferably, in step 2, when mixing the materials, the amounts of resin acid and maleic anhydride are gradually increased so that the yield of maleic anhydride increases and the reaction between the resin acid and maleic anhydride is complete.

[0011] (3) Beneficial effects The present invention provides a method for preparing a bio-based corrosion inhibitor and rust preventer composition for steel, which has the following beneficial effects: (1) A method for preparing a bio-based corrosion inhibitor and rust preventer composition for steel. The solution of the present invention can prevent steel from rusting and has good hydrolysis resistance. At the same time, it has a thickening effect on the rust-preventing water, thereby preventing the rust inhibitor from escaping from the metal surface and ensuring that the rust inhibitor firmly adheres to the metal surface. The rust inhibitor can form a multi-layer film on the carbon steel surface in a very short time. The inner layer is a reaction-deposited film with strong bonding with the base metal, thereby effectively preventing the metal from rusting. DETAILED DESCRIPTION

[0012] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.

[0013] The present invention provides a method for preparing a bio-based corrosion inhibitor and rust preventer composition for steel, comprising the following steps: Step 1: The following preparation methods are included by weight: 1-3 parts of rosin, 1-2 parts of resin acid, 2-5 parts of maleic anhydride, 2-4 parts of catalyst, 2-4 parts of methylbenzene sulfide, and 6-12 parts of glacial acetic acid as solvent; Step 2: Extract resin acid from rosin, mix resin acid with maleic anhydride and heat, and continue heating for 5-9 hours.

[0014] Weigh 145.0g of rosin powder and place it in a mixing tank. Add acetone solution to the tank and dissolve it in 445.0mL of acetone at 39.0°C until clear. Heat the mixture during mixing and filter it after heating to remove impurities. Transfer the filtered filtrate to a flask with reflux stirring and heat it to 38.0°C. Dissolve 40.0g of cyclohexylamine in 70.0mL of acetone. Transfer the filtrate to a constant pressure dropping funnel and slowly add the cyclohexylamine acetone solution, producing a large amount of white precipitate. Keep the reaction at 380.0°C for 2 hours. After the reaction, cool the mixture to 4.0°C in an ice-water bath and hold for 35 minutes. Filter the mixture and wash the precipitate with 65.0mL of ice-cold acetone. Dry the precipitate in a vacuum at 30.0°C.

[0015] Add 150.0 g of the precipitate and 200.0 mL of diethyl ether to a flask with a concave flow stirring apparatus. Stir the concave flow and slowly add 3.0 mol / L of hydrochloric acid dropwise until the white powder disappears. Continue the reaction at room temperature for 40 min. Then, transfer the reaction solution to a separatory funnel, remove the aqueous layer, and repeatedly wash the organic phase with water until the pH of the aqueous phase reaches 6.5. Vacuum away most of the diethyl ether from the organic phase, and vacuum dry the viscous liquid at 30.0°C to obtain a fluffy yellow solid. The yield of the resin acid is approximately 80%.

[0016] During the synthesis, 90.1 g of resin acid, 3.8 g of p-toluenesulfonic acid, 15.2 g of maleic anhydride, and 50.0 mL of glacial acetic acid were added to a mixing tank in a stirring reflux apparatus. After nitrogen was introduced for 20 minutes, the mixture was heated to 130.0°C and reacted under reflux for 6.0 hours. The mixture was then rapidly cooled to 105.0°C. 200.0 mL of glacial acetic acid was added to the cooled mixing tank. The mixture was rapidly cooled to room temperature and then cooled in an ice-water bath. A crude white product was obtained by filtration. The product was recrystallized using glacial acetic acid. The pure maleopimaric anhydride was vacuum-dried at 70.0°C to obtain a pure white block.

[0017] In step 1, the resin acid is extracted from rosin. During the extraction, the rosin powder is first dissolved and then allowed to stand. The liquid will precipitate after standing. After precipitation, the upper layer of the liquid is clear and the lower layer of the liquid is precipitated material. After clarification, the liquid is filtered to remove impurities.

[0018] The filtered filtrate is transferred to a heating tank for heating. Cyclohexanamine is added during the heating process of the filtrate. After the liquid cools down, it is precipitated. The precipitated material is vacuum dried. The precipitated material is mixed, stirred and heated with ether. After mixing and heating, the liquid is separated.

[0019] During the mixing in step 2, resin acid, methylbenzenesulfuric acid, maleic anhydride and glacial acetic acid are stirred and mixed respectively, and nitrogen is injected into the materials in the tank after mixing.

[0020] After filling with nitrogen, the mixing tank is heated to raise its temperature. After reaching the temperature, the stability of the mixing tank is lowered. After the stability is lowered, glacial acetic acid is added. After adding, the mixing tank is cooled to room temperature, and then quickly cooled with cold water. After cooling, a white pure product is obtained.

[0021] In step 2, when mixing the materials, the amount of resin acid and maleic anhydride used is gradually increased, so that the yield of maleic anhydride increases, and the reaction between the resin acid and maleic anhydride is complete.

[0022] When the molar ratio of resin acid to maleic anhydride is less than 3.0:1.5, as the molar ratio of resin acid to maleic anhydride increases, the yield of maleopimaric anhydride also increases according to the quality of the resin acid and maleic anhydride. Since only the resin acid with conjugated double bonds among the separated resin acids is easily isomerized, an excess of resin acid is required to achieve a relatively complete reaction of maleic anhydride. When the molar ratio is higher than 3.0:1.5, the yield of maleopimaric anhydride no longer increases, and the yield decreases slightly.

[0023] When the amount of glacial acetic acid used during the reaction is less than 70 mL, the yield of maleopimaric anhydride increases with increasing glacial acetic acid usage. The presence of a large amount of glacial acetic acid can significantly reduce the viscosity of the reaction system, thereby facilitating the cycloaddition reaction of levorotatory pimaric acid and maleic anhydride. However, when the amount of glacial acetic acid used is too high, the concentration of the reactants is reduced, thus hindering product formation. Furthermore, when the amount of glacial acetic acid is too high, the reaction system cannot reach the required temperature, resulting in a decrease in product yield.

[0024] When the reaction temperature is less than 130°C, the yield of the product increases with increasing reaction temperature. This is because the isomerization reaction of the resin acid is faster when the temperature rises, and the production of more levorotatory pimaric acid promotes the formation of maleopimaric anhydride. Therefore, increasing the temperature is beneficial to the reaction. When the reaction temperature is higher than 130°C, the yield of maleopimaric anhydride decreases. This may be because the temperature is too high, causing some decomposition between the resin acid and maleopimaric anhydride, which in turn reduces the yield.

[0025] A solution of resin acid, maleic anhydride, and methylbenzenesulfide was prepared in a ratio of resin acid:maleic anhydride:methylbenzenesulfide of 3.5:7:2. The pH was adjusted to 5-9 (the pH value of a 2% solution of the above mixture dissolved in pure water) using tris(hydroxymethyl)methylglycine and sodium hydroxide. The mixture was then mixed uniformly according to the ratio to obtain the rust remover provided by the present invention.

[0026] Those skilled in the art will clearly understand that, for the convenience and brevity of description, the specific working processes of the systems, devices and units described above can refer to the corresponding processes in the aforementioned method embodiments and will not be repeated here.

[0027] In the several embodiments provided in this application, it should be understood that the disclosed systems, devices and methods can be implemented in other ways. For example, the device embodiments described above are merely schematic. For example, the division of the units is merely a division of some logical functions. In actual implementation, there may be other division methods, such as multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be through some interfaces, indirect coupling or communication connection of devices or units, which can be electrical, mechanical or other forms.

[0028] The above description is merely a specific embodiment of the present application, but the scope of protection of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in this application should be included in the scope of protection of this application. Therefore, the scope of protection of this application should be based on the scope of protection of the claims.

Claims

1. A method for preparing a bio-based corrosion inhibitor and rust preventive composition for steel, characterized in that: The following steps are involved: Step 1: The following preparation methods are included by weight: 1-3 parts of rosin, 1-2 parts of resin acid, 2-5 parts of maleic anhydride, 2-4 parts of catalyst, 2-4 parts of methylbenzene sulfide, and 6-12 parts of glacial acetic acid as solvent; Step 2: Extract resin acid from rosin, mix resin acid with maleic anhydride and heat, and continue heating for 5-9 hours.

2. The method for preparing a bio-based corrosion inhibitor and rust preventive composition for steel according to claim 1, characterized in that: In step 1, the resin acid is extracted from rosin. During the extraction, the rosin powder is first dissolved and then allowed to stand. The liquid will precipitate after standing. After precipitation, the upper layer of the liquid is clear and the lower layer of the liquid is precipitated material. After clarification, the liquid is filtered to remove impurities.

3. The method for preparing a bio-based corrosion inhibitor and rust preventive composition for steel according to claim 2, characterized in that: The filtered filtrate is transferred to a heating tank for heating. Cyclohexanamine is added during the heating process of the filtrate. After the liquid cools down, it is precipitated. The precipitated material is vacuum dried. The precipitated material is mixed, stirred and heated with ether. After mixing and heating, the liquid is separated.

4. The method for preparing a bio-based corrosion inhibitor and rust preventive composition for steel according to claim 1, characterized in that: During the mixing in step 2, resin acid, methylbenzenesulfuric acid, maleic anhydride and glacial acetic acid are stirred and mixed respectively, and nitrogen is injected into the materials in the tank after mixing.

5. The method for preparing a bio-based corrosion inhibitor and rust preventive composition for steel according to claim 4, characterized in that: After filling with nitrogen, the mixing tank is heated to raise its temperature. After reaching the temperature, the stability of the mixing tank is lowered. After the stability is lowered, glacial acetic acid is added. After adding, the mixing tank is cooled to room temperature, and then quickly cooled with cold water. After cooling, a white pure product is obtained.

6. The method for preparing a bio-based corrosion inhibitor and rust preventive composition for steel according to claim 1, characterized in that: In step 2, when mixing the materials, the amount of resin acid and maleic anhydride used is gradually increased, so that the yield of maleic anhydride increases, and the reaction between the resin acid and maleic anhydride is complete.