Method for improving surface phosphatability of cold-rolled automobile steel
By comprehensively controlling the various factors on the surface of cold-rolled automobile plates, including flame cleaning, pickling, annealing and surface morphology characteristics, the problem of low phosphating performance of cold-rolled plates is solved, and high-quality phosphating film formation and resistance are achieved Corrosion performance is improved.
Patent Information
- Application Number
- CN202411051463.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-22
AI Technical Summary
The surface phosphating and corrosion resistance of cold-rolled automotive plates are low. The existing technology fails to fully consider the comprehensive factors such as surface oil coating, oil coating to phosphating interval time, surface roughness, peak density, slope and surface defects. Influence, the phosphated film quality is poor.
Through flame cleaning, pickling, annealing and flattening processes, surface roughness, peak density, slope and surface defects are controlled, the amount of oil applied and the time interval between oil applied to phosphating is defined, surface cleanliness and degreasing effect is ensured, and chrome plating is used to plating. The rollers are flattened to ensure that there are no scratches or rust points on the surface before phosphating, and to adjust the chemical composition and surface morphological characteristics parameters.
The uniformity and density of the phosphated film on the surface of the cold-rolled plate are improved, and the phosphated phase size is less than 5 μm, which enhances the adhesion and corrosion resistance of the electrophoretic paint film.
Smart Images

Figure CN118996408A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal material surface treatment, and in particular relates to a method for improving the phosphating property of the surface of cold-rolled automobile steel. Background Art
[0002] The corrosion protection of automobile bodies is mainly achieved through painting. Therefore, painting is an important aspect of automobile body manufacturing process, and the quality of painting directly affects the corrosion resistance and decorative performance of the automobile body. During the painting process, a series of complex chemical reactions occur on the surface of the body material. Phosphating treatment, as an important pre-painting treatment method, aims to form a uniform and dense phosphating film on the surface of the steel plate, thereby improving the surface corrosion resistance and enhancing the adhesion of the primer. It has been widely used in the field of automobile production.
[0003] The phosphating reaction process on the surface of automobile steel sheets determines the quality of phosphating film. The surface quality of cold-rolled automobile sheets is an important factor affecting the phosphating quality and paintability. The surface quality of cold-rolled automobile sheets mainly includes the following aspects: First, surface cleanliness. Carbon pollution on the surface of cold-rolled automobile sheets is very unfavorable for phosphating treatment. In the parts with high carbon concentration on the surface of steel sheets, the phosphate crystallization is not completely formed, which easily leads to the appearance of phosphating film defects, affecting the phosphating and painting quality of cold-rolled automobile sheets. Second, the enrichment and selective oxidation state of elements on the surface of cold-rolled automobile sheets. The enrichment and oxidation of easily oxidized elements in steel on the surface of steel sheets will lead to uneven surface reaction activity, causing coarse grains of phosphating film in local locations, and the corrosion resistance of the paint film after painting is reduced. Third, surface morphology. The surface morphology of steel sheets is mainly reflected in the requirements for the surface roughness of steel sheets. In addition to the Ra value, the peak density, i.e., the RPc value, is also a key factor affecting the quality of body painting. Fourth, surface defects. Due to the potential difference between the inclusions and precipitates on the surface of the strip and the surrounding matrix, as well as the difference in wettability to the phosphating solution, the surface uniformity is reduced and the local activity is high, which is not conducive to the formation of a continuous, uniform and dense phosphating film.
[0004] In short, a uniform phosphating reaction requires not only that the chemical composition and organizational structure of the substrate before coating be evenly distributed, that there be no obvious element enrichment on the surface, that the surface be highly clean, free of any pollution, defects, or rust, but also that the substrate surface have a high surface energy and a certain roughness value to promote the phosphating nucleation reaction and reduce the nucleation barrier, but also that the surface adjustment, phosphating solution components, and film-forming conditions be strictly controlled.
[0005] The crystal state and grain size of the phosphate film are effective methods for evaluating the quality of the phosphate film. Automobile OEMs require that the crystal state of the phosphate film on the surface of the cold-rolled automobile sheet be continuous and densely distributed in a granular form, and that phosphating defects must not occur. On the other hand, the grain size of the phosphate film is also required to be less than 10μm. In order to improve the paintability of cold-rolled automobile sheets, it is necessary to adjust and optimize the entire production process, improve the surface quality of the cold-rolled automobile sheets, and control the surface roughness within a reasonable range, thereby improving its phosphability during the coating process and the crystal state of the phosphate film, improving the paintability of the cold-rolled automobile sheets and the corrosion resistance after coating.
[0006] Patent CN105420607A discloses a control method for improving the paintability and surface quality of cold-rolled automobile sheets. The paintability of cold-rolled automobile sheets is improved by controlling the element distribution, oxidation state and surface roughness of the cold-rolled automobile sheets, and focuses on the control of the production process.
[0007] Patent CN111647733A discloses a method for improving the phosphating performance of low-carbon aluminum-killed steel automobile plates, and automobile plates. By controlling the composition of the ingot, hot rolling, cold rolling, annealing and smoothing processes, the surface quality of the steel plates is improved, thereby improving the phosphating performance of the low-carbon aluminum-killed steel automobile plates.
[0008] Patent CN114231822A discloses a method for improving the paintability of the surface of cold-rolled automobile plates. Through smelting, rolling, continuous annealing, pickling, surface conditioning and phosphating processes, the phosphating film layer on the surface of the cold-rolled automobile plate prepared has a dense structure, uniform crystallization, and is granular. The average grain size is 2-3μm, the porosity is small, and it has high paintability.
[0009] In summary, the above-mentioned patents for improving the phosphating performance of cold-rolled sheets each have their own advantages and disadvantages, and many influencing factors have been explained, but the effects of the amount of surface oiling, the interval time from oiling to phosphating, surface scratches, etc. on the phosphating performance of the cold-rolled sheet surface have not been comprehensively considered. Summary of the invention
[0010] The purpose of the present invention is to provide a method for improving the phosphating property of the surface of cold-rolled automobile steel, and the purpose is to analyze the surface oil coating amount, the time interval from production to phosphating, the surface roughness, the peak density, the skewness, and the surface defect control, comprehensively consider various factors affecting the quality of the phosphating film on the surface of the cold-rolled plate, improve the phosphating property of the surface of the cold-rolled plate, and solve the problems of low phosphating property and corrosion resistance of the current cold-rolled automobile plate.
[0011] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0012] The present invention discloses a method for improving the phosphating property of the surface of cold-rolled automobile steel, which is applicable to cold-rolled automobile plates;
[0013] Used for flame cleaning of continuous casting billet surface in the production of cold-rolled automobile steel before loading into furnace for heating. Flame cleaning thickness is 3.0-5.0cm. The total amount of residue on the surface of cold-rolled cold-hardened strip after pickling is ≤240mg / m 2 , chrome-plated rollers are used for annealing and leveling;
[0014] Surface morphology characteristic parameters of cold-rolled automotive steel: roughness Ra is 0.9-1.3μm, peak density RPc value is 90-140, surface maximum profile peak height Sp is 3.0-4.0μm, while ensuring that the skewness Ssk is -0.6-0.2, the steepness Sku is 1.5-2.5, the root mean square slope Sdq is 0.35-0.40, the surface area growth rate Sdr% is 4.0-5.5, the surface area ratio is ≥1.04, and the strip surface oil coating amount is 600-1000mg / m 2 ;
[0015] The time interval from oiling to phosphating is ≤ 60 days.
[0016] Furthermore, the chemical composition and weight percentage of the cold-rolled automotive steel are C: 0.002-0.080%, Si: 0.01-0.05%, Mn: 0.01-0.06%, P≤0.030%, S≤0.025%, Alt: 0.010-0.050%, Ti: 0.02-0.10%, Nb: 0.02-0.10%, and the balance is Fe and unavoidable impurities.
[0017] Furthermore, the surface of the cold-rolled sheet was inspected before phosphating, and no scratches or rust spots were visible to the naked eye within an area of 70 cm × 150 cm.
[0018] Furthermore, sufficient degreasing is performed before phosphating to ensure that the surface of the cold-rolled sheet is completely exposed and fully covered with a water film.
[0019] Furthermore, the flame cleaning thickness of the continuous casting slab surface is 3.5 cm.
[0020] Furthermore, the total amount of residue on the surface of cold-rolled cold-hardened strip after pickling is 140 mg / m 2 .
[0021] Furthermore, the chemical composition and weight percentage of the cold-rolled automobile steel are C: 0.030%, Si: 0.03%, Mn: 0.05%, P: 0.025%, S: 0.014%, Alt: 0.031%, Ti: 0.03%, Nb: 0.05%, and the balance is Fe and unavoidable impurities.
[0022] Compared with the prior art, the beneficial technical effects of the present invention are:
[0023] The present invention regulates aspects such as chemical composition design, removal of oxides on the surface of the ingot, control of surface residues in the cold-rolled state, types of work rolls produced, surface micromorphology characterization parameters, amount of oiling, time interval from oiling to phosphating, control of surface defects and rust spots, and degreasing effect, so as to improve the surface quality of the steel plate. There are many factors that affect the phosphating film formation of cold-rolled plates. It is impossible to prepare a high-quality phosphating film simply by controlling characteristics such as grain size and surface roughness. Therefore, this application limits the cleaning of the slab surface before hot rolling to ensure that the substrate surface has a high degree of cleanliness and less residues, avoids the enrichment of harmful elements on the substrate surface, and thus improves the phosphating performance of the automotive plate; in order to ensure the degreasing and cleaning effect, the present invention limits the amount of oiling on the strip surface and the time interval from oiling to phosphating, further improving the phosphating film formation quality of the automotive plate.
[0024] The present invention provides a method for improving the phosphating property of the surface of a cold-rolled sheet. The phosphating film has uniform thickness, complete coverage, and a dense structure. The phosphating phase is granular and the size of the phosphating phase is ≤5 μm. The subsequent electrophoresis process is well organized and the corrosion resistance of the electrophoretic paint film is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The present invention will be further described below in conjunction with the accompanying drawings.
[0026] Figure 1 This is the morphology of the phosphating film in Example 1;
[0027] Figure 2 This is the morphology of the phosphating film in Comparative Example 1;
[0028] Figure 3 This is the morphology of the phosphating film in Comparative Example 2;
[0029] Figure 4 This is the morphology of the phosphating film in comparative example 3. DETAILED DESCRIPTION
[0030] A method for improving the phosphatability of the surface of cold-rolled automotive steel, specifically comprising:
[0031] (1) The chemical composition and weight percentage of cold-rolled automobile steel are C: 0.002-0.080%, Si: 0.01-0.05%, Mn: 0.01-0.06%, P≤0.030%, S≤0.025%, Alt: 0.010-0.050%, Ti: 0.02-0.10%, Nb: 0.02-0.10%, and the balance is Fe and unavoidable impurities.
[0032] (2) For the production of cold-rolled automobile steel, the surface of the continuous casting billet is flame cleaned and then heated in the furnace. The flame cleaning thickness is 3.0-5.0 cm. The total amount of residue (residual oil + residual iron) on the surface of the cold-rolled cold-hardened strip after pickling is ≤240 mg / m 2, chrome-plated rollers are used for annealing and leveling.
[0033] (3) Surface morphology characteristic parameters of cold-rolled automotive steel: roughness Ra is 0.9-1.3 μm, peak density RPc value is 90-140, surface maximum profile peak height Sp is 3.0-4.0 μm, while ensuring that the skewness Ssk is -0.6-0.2, the steepness Sku is 1.5-2.5, the root mean square slope Sdq is 0.35-0.40, the surface area growth rate Sdr% is 4.0-5.5, the surface area ratio is ≥1.04, and the strip surface oil coating amount is 600-1000 mg / m 2 .
[0034] (4) The time interval from oiling to phosphating is ≤ 60 days.
[0035] (5) Before phosphating, check the surface of the cold-rolled sheet. There should be no scratches or rust spots visible to the naked eye within an area of 70 cm × 150 cm.
[0036] (6) Degrease thoroughly before phosphating to ensure that the surface of the cold-rolled sheet is completely exposed and fully covered with water film.
[0037] The present invention is described in detail below through specific examples. The examples are intended to help understand the present invention but are not intended to limit the present invention.
[0038] Example 1 and Comparative Examples 1, 2, and 3 mainly investigate the effects of peak density RPc, surface scratch defects, and insufficient surface degreasing on the phosphatability of cold-rolled sheets.
[0039] Table 1 Chemical composition (wt%), flame cleaning thickness (cm) of ingot surface, total amount of residue on the surface of chilled strip (mg / m 2 )
[0040]
[0041] Table 2 Surface morphology characteristic parameters of Example 1 of the present invention and Comparative Examples 1-3
[0042]
[0043]
[0044] Table 3 Surface oil coating amount (mg / m 2 ), the time interval from oiling to phosphating (days), whether there are visible scratches and rust spots on the surface, whether the degreasing is complete
[0045]
[0046] It can be seen from Comparative Example 1 that the peak density RPc of the cold-rolled sheet surface has an impact on the morphology of the phosphate film. When the peak density RPc is reduced to below 90, the morphology of the phosphate film grains changes from granular to short rod-shaped, the length increases, and the density decreases. When the peak density RPc value is not less than 90, the number of surface peaks and valleys is large, the effective contact area between the steel plate surface and the liquid is large when the phosphate film is formed, and the steel plate surface can accumulate more conversion film-forming substances more evenly. In the phosphating surface adjustment process, more colloidal titanium is physically adsorbed in the "pits" on the surface of the cold-rolled sheet, providing more crystal nuclei for the nucleation of the phosphating phase. At the same time, the increase in the actual area is conducive to the formation of mechanical locks between the surface and the phosphate film, and the anchoring effect is significant, and the adhesion of the phosphate film and the electrophoretic paint film is enhanced accordingly.
[0047] It can be seen from Comparative Example 2 that the absence of visible scratches and rust spots on the surface of the cold-rolled sheet has an impact on the phosphating property of the cold-rolled sheet. The phosphating film in the normal area of the surface is intact, but the phosphating film in the area where the scratches are visible to the naked eye has holes and is loose. The scratches are deep, and the ion diffusion rate is slow, which affects the accumulation and growth of phosphate crystals. The grooves cannot be filled within the reaction time, so the continuity of the phosphating film is destroyed.
[0048] It can be seen from Comparative Example 3 that whether the cold-rolled sheet surface is completely degreased has an impact on the phosphating property of the cold-rolled sheet. The oil stains remaining on the surface of the sheet after degreasing and cleaning block the contact between the metal surface and the conversion film liquid. Due to the reduction of activation points, the formation of a dense and uniform conversion film cannot be guaranteed, and the phosphating film formed is ultimately loose and porous.
[0049] Embodiment 1 of the present invention, as Figure 1 As shown, the phosphating film has uniform thickness, complete coverage, dense structure, granular phosphating phase, and phosphating phase size ≤ 5μm, which makes organizational preparation for the subsequent electrophoretic process and improves the corrosion resistance of the electrophoretic paint film.
[0050] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for improving the phosphating property of cold-rolled automotive steel surface. It is characterized in that Applicable to cold rolled automotive sheets; Used for flame cleaning of continuous casting billet surface in the production of cold-rolled automobile steel before loading into furnace for heating. Flame cleaning thickness is 3.0-5.0cm. The total amount of residue on the surface of cold-rolled cold-hardened strip after pickling is ≤240mg / m 2 , chrome-plated rollers are used for annealing and leveling; Surface morphology characteristic parameters of cold-rolled automotive steel: roughness Ra is 0.9-1.3μm, peak density RPc value is 90-140, surface maximum profile peak height Sp is 3.0-4.0μm, while ensuring that the skewness Ssk is -0.6-0.2, the steepness Sku is 1.5-2.5, the root mean square slope Sdq is 0.35-0.40, the surface area growth rate Sdr% is 4.0-5.5, the surface area ratio is ≥1.04, and the strip surface oil coating amount is 600-1000mg / m 2 ; The time interval from oiling to phosphating is ≤ 60 days.
2. The method for improving the phosphating property of the surface of cold-rolled automobile steel according to claim 1, It is characterized in that The chemical composition and weight percentage of the cold-rolled automobile steel are as follows: C: 0.002-0.080%, Si: 0.01-0.05%, Mn: 0.01-0.06%, P≤0.030%, S≤0.025%, Alt: 0.010-0.050%, Ti: 0.02-0.10%, Nb: 0.02-0.10%, and the balance is Fe and unavoidable impurities.
3. The method for improving the phosphating property of the surface of cold-rolled automobile steel according to claim 1, It is characterized in that Before phosphating, check the surface of the cold-rolled sheet and find no scratches or rust spots visible to the naked eye within an area of 70cm×150cm.
4. The method for improving the phosphatability of the surface of cold-rolled automobile steel according to claim 1, It is characterized in that Before phosphating, sufficient degreasing is carried out to ensure that the surface of the cold-rolled plate is completely exposed and fully covered with water film.
5. The method for improving the phosphating property of the surface of cold-rolled automobile steel according to claim 1, It is characterized in that The surface of the continuous casting billet is flame cleaned to a thickness of 3.5 cm.
6. The method for improving the phosphatability of the surface of cold-rolled automobile steel according to claim 1, It is characterized in that The total amount of residue on the surface of cold-rolled cold-hardened strip after pickling is 140mg / m 2 .
7. The method for improving the phosphatability of the surface of cold-rolled automobile steel according to claim 2, It is characterized in that The chemical composition and weight percentage of the cold-rolled automobile steel are C: 0.030%, Si: 0.03%, Mn: 0.05%, P: 0.025%, S: 0.014%, Alt: 0.031%, Ti: 0.03%, Nb: 0.05%, and the balance is Fe and unavoidable impurities.