Advanced composite membrane material for water electrolysis hydrogen production process and manufacturing technology

By using binder resin, hydrophilic inorganic particles and coupling agents in the composite film material, the problem of vulnerability in the composite film material structure is solved, the service life and stability of the electrolytic cell are improved, and the replacement cost is reduced.

CN118996527AInactive Publication Date: 2024-11-22CEMT CO LTD

Patent Information

Application Number
CN202411496230.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing composite film materials have problems of particle powder falling and structural vulnerability during use, resulting in reduced performance of the electrolytic cell and short service life, which increases replacement cost.

Method used

Using composite film materials containing binder resin, hydrophilic inorganic particles and coupling agents, the coupling agent has inorganic and organic functional groups, which enhances the bonding strength between the bonding resin and hydrophilic inorganic particles, and improves the alkali resistance of the composite film. and resilience.

Benefits of technology

It significantly improves the structural stability and service life of composite film materials, reduces the frequency of composite film materials replacement in alkaline water electrolytic cells, and reduces labor time and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an advanced composite membrane material for a water electrolysis hydrogen production process and a manufacturing technology. The composite membrane material comprises a base membrane and coatings arranged on the two sides of the base membrane, and each coating comprises bonding resin, hydrophilic inorganic particles and a coupling agent. The coupling agent is introduced into the coating of the composite membrane material, so that the composite membrane material has strong alkali resistance, high strength, good toughness, good hydrophilicity, high wetting speed and low surface resistance, the structural stability of the composite membrane material can be effectively improved, and the service life of the composite membrane material can be effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the hydrogen energy industry and relates to an advanced composite membrane material and manufacturing technology for a water electrolysis hydrogen production process. Background Art

[0002] The resource shortage and environmental pollution problems faced by traditional energy sources are becoming increasingly serious. Hydrogen energy, as a green, clean, renewable, high-energy-density energy, is gradually gaining attention. At present, the global hydrogen energy industry has entered a stage of rapid development, but the preparation of hydrogen is still a difficult problem that needs to be overcome.

[0003] As a traditional method, water electrolysis for hydrogen production has the advantages of relatively simple operation and relatively mature technology. Among the many hydrogen production methods, alkaline water electrolyzer has the advantages of low cost, high efficiency and mature technology. Composite membrane plays a decisive role in the performance of electrolyzers. In the early days, asbestos was used as a diaphragm material, but asbestos contained very fine fibers that were almost invisible to the naked eye. These fibers would be inhaled into the body and deposited in the lungs in large quantities, causing diseases to the human body and even cell cancer, thus gradually being eliminated; the second-generation composite membrane introduced hydrophilic functional groups on the molecular chain branches by modifying PPS, but the functional groups were not stable, resulting in a short life of the diaphragm. As a result, the third-generation composite membrane was developed. Taking Agfa's zirfon product as an example, polyphenylene sulfide (PPS) was used as the substrate, and a slurry mixture containing polysulfone and zirconium oxide was coated on it to prepare a third-generation composite membrane with certain strength and good hydrophilicity.

[0004] The existing composite membranes have the following disadvantages: First, there is a phenomenon of particle powder falling off during the use of the composite membrane, which damages the composite membrane structure and affects the performance of the electrolytic cell; Second, the composite membrane structure is fragile, resulting in a reduced lifespan, which inevitably leads to the replacement of the composite membrane of the electrolytic cell, which is time-consuming, labor-intensive, expensive, and not conducive to long-term use.

[0005] Therefore, it is necessary to provide a new type of composite membrane material with excellent stability to improve the service life of the electrolytic cell. Summary of the invention

[0006] In view of the above problems existing in the prior art, the purpose of the present invention is to provide an advanced composite membrane material and manufacturing technology for the process of producing hydrogen by electrolysis of water.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a composite membrane material, comprising a base membrane and a coating layer disposed on both sides of the base membrane, wherein the coating layer comprises a bonding resin, hydrophilic inorganic particles and a coupling agent.

[0009] In the composite film material of the present invention, the coating contains a coupling agent, which has two functional groups of different properties, one is an inorganic-philic group, and the other is an organic-philic group, so it plays a role in dispersing the casting liquid and enhancing the bonding strength between the adhesive resin and the hydrophilic inorganic particles in the casting liquid of the composite film material. The composite film material of the present invention has strong alkali resistance, high strength, good toughness, good hydrophilicity, fast wetting speed, low surface resistance, and can effectively improve its structural stability and service life.

[0010] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0011] Preferably, the coupling agent includes at least one of a silane coupling agent and a titanate coupling agent, preferably a silane coupling agent.

[0012] Preferably, the silane coupling agent includes at least one of vinyl triethoxysilane, aminopropyl triethoxysilane and trichloropropylene silane, preferably aminopropyl triethoxysilane.

[0013] Preferably, the titanate coupling agent includes at least one of monoalkoxy titanate, monoalkoxy pyrophosphate coupling agent, triisostearoyl isopropyl titanate and diisostearoyl ethyl phthalate.

[0014] Preferably, the bonding resin includes at least one of polysulfone, polyethersulfone, polyphenol, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene terephthalate and polybutylene terephthalate, preferably polysulfone.

[0015] Preferably, the hydrophilic inorganic particles include at least one of zirconium oxide, silicon oxide, magnesium oxide, zirconium hydroxide and magnesium hydroxide.

[0016] Preferably, the hydrophilic inorganic particles are monoclinic zirconium oxide with an average particle size of 20nm-100nm, for example, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm or 100nm.

[0017] Preferably, the thickness of the composite membrane material is 220μm-400μm, for example, 220μm, 230μm, 240μm, 250μm, 260μm, 270μm, 280μm, 290μm, 300μm, 310μm, 320μm, 330μm, 340μm, 350μm, 360μm, 370μm, 380μm, 390μm or 400μm, etc.

[0018] Preferably, the porosity of the composite membrane material is 40%-60%, for example 40%, 42%, 45%, 46%, 47%, 48%, 50%, 52%, 54%, 55%, 57%, 58% or 60%, etc.

[0019] Preferably, the tensile strength of the composite membrane material is greater than 20 MPa, for example, 22 MPa, 25 MPa, 28 MPa, 30 MPa, 33 MPa, 36 MPa, 40 MPa, 43 MPa, 45 MPa, 48 MPa, 50 MPa, 55 MPa, 60 MPa, 65 MPa or 70 MPa.

[0020] In a second aspect, the present invention provides a method for preparing the composite membrane material according to the first aspect, the preparation method comprising the following steps:

[0021] Placing the composite membrane material casting liquid on a coating machine glass plate, soaking polyphenylene sulfide (PPS), coating, pre-evaporating, and then immersing in a non-solvent for phase conversion to obtain the composite membrane material;

[0022] The composite membrane material casting solution comprises an organic solvent, a bonding resin, hydrophilic inorganic particles and a coupling agent.

[0023] The composite membrane material of the invention has simple raw materials and equipment for preparation, and a simple preparation process, and can meet the requirements of large-scale production.

[0024] In one embodiment, the PPS is a woven structure filter mesh structure.

[0025] Preferably, the temperature of the coater is set to 50°C-70°C, for example, 50°C, 57°C, 60°C, 63°C, 66°C or 70°C.

[0026] Preferably, the pre-evaporation is carried out at room temperature, and the ambient humidity is 30%-50%, for example, 30%, 32%, 35%, 37%, 40%, 42%, 44%, 45%, 47%, 48% or 50%, etc.

[0027] Preferably, the pre-evaporation time is 10 s to 30 s, for example, it can be 10 s, 12 s, 13 s, 14 s, 15 s, 16 s, 18 s, 20 s, 25 s or 30 s.

[0028] Preferably, the phase inversion time is 40 s to 70 s, for example, 40 s, 45 s, 50 s, 55 s, 60 s, 65 s or 70 s.

[0029] As a preferred technical solution of the method for preparing the composite membrane material of the present invention, the composite membrane material casting solution includes an organic solvent, a bonding resin, hydrophilic inorganic particles and a coupling agent.

[0030] Preferably, the solvent includes at least one of N-methylpyrrolidone, N-ethylpyrrolidone, N-butylpyrrolidone, 1,3-dimethylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide, preferably at least one of N-methylpyrrolidone and N,N-dimethylacetamide.

[0031] Preferably, the solvent accounts for 30%-50% of the total mass of the composite membrane material casting solution, for example, 30%, 32%, 33%, 35%, 37%, 38%, 40%, 42%, 44%, 46%, 48% or 50%.

[0032] Preferably, the bonding resin accounts for 10%-18% of the total mass of the composite membrane material casting liquid, for example, 10%, 10.5%, 11%, 11.5%, 12%, 13%, 14%, 15%, 16%, 17% or 18%.

[0033] Preferably, the hydrophilic inorganic particles account for 30%-60% of the total mass of the composite membrane material casting liquid, for example, 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 45%, 47%, 48%, 50%, 52%, 54%, 56%, 58% or 60%, etc.

[0034] Preferably, the mass ratio of the hydrophilic inorganic particles to the binding resin is greater than 65 / 35, such as 2, 2.5, 3, 3.5, 4, 4.5 or 5, and preferably greater than 75 / 25.

[0035] Preferably, the coupling agent accounts for 0.5%-8% of the total mass of the composite membrane material casting liquid, for example, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5% or 8%, etc., preferably 2%-8%.

[0036] Preferably, the composite membrane material casting solution also includes a porogen.

[0037] Preferably, the porogen comprises polyvinyl pyrrolidone (PVP).

[0038] In one embodiment, the molecular weight of polyvinyl pyrrolidone is 8000-100000, for example, 8000, 10000, 20000, 30000, 40000, 50000, 60000, 70000, 80000, 90000 or 100000, etc.

[0039] In one embodiment, the polyvinyl pyrrolidone is of type K25-K60.

[0040] Preferably, the porogen accounts for 1%-10% of the total mass of the composite membrane material casting solution, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%.

[0041] As a preferred technical solution of the method for preparing the composite membrane material of the present invention, the method for preparing the composite membrane material casting solution comprises the following steps:

[0042] Putting an organic solvent into a vacuum disperser, adding a binder resin, stirring once, adding hydrophilic inorganic particles, stirring twice, adding a coupling agent, stirring three times, and obtaining the composite membrane material casting solution;

[0043] The temperature of the primary stirring is 50°C-80°C, for example, 50°C, 52°C, 55°C, 57°C, 60°C, 62°C, 65°C, 68°C, 70°C, 75°C or 80°C; the primary stirring is low-speed stirring, with a rotation speed of 300r / min-1000r / min, for example, 300r / min, 350r / min, 400r / min, 450r / min, 500r / min, 550r / min, 600r / min, 650r / min, 700r / min, 750r / min, 800r / min, 900r / min or 1000r / min; the time is 1h-3h, for example, 1h, 1.2h, 1.5h, 1.7h, 1.8h, 2h, 2.3h, 2.6h, 2.8h or 3h, etc.

[0044] The secondary stirring is high-speed stirring with a rotation speed of 1200r / min-2500r / min, for example, 1200r / min, 1300r / min, 1400r / min, 1500r / min, 1600r / min, 1700r / min, 1800r / min, 1900r / min, 2000r / min, 2100r / min, 2200r / min, 2300r / min, 2400r / min or 2500r / min, etc.

[0045] The secondary stirring time is 12 h to 18 h, for example, 12 h, 12.5 h, 13 h, 13.5 h, 14 h, 15 h, 16 h, 17 h or 18 h.

[0046] The three stirrings are high-speed stirrings with a rotation speed of 1200r / min-2500r / min, for example 1200r / min, 1300r / min, 1400r / min, 1500r / min, 1600r / min, 1700r / min, 1800r / min, 1900r / min, 2000r / min, 2100r / min, 2200r / min, 2300r / min, 2400r / min or 2500r / min, etc.

[0047] The present invention improves the agglomeration of the casting liquid by adding a coupling agent to the casting liquid of the composite membrane material so that the organophilic groups in the coupling agent react chemically with the adhesive resin or generate hydrogen bonds and dissolve therein, and the inorganic philic groups in the coupling agent react chemically with the inorganic surface to enhance the structural strength, so that the adhesive resin and the hydrophilic inorganic particles in the composite membrane material can be better dispersed and combined, and the powder falling phenomenon is reduced, thereby effectively improving the defect of the existing composite membrane material being easily damaged, improving the performance of the composite membrane material, and increasing the service life of the composite membrane material.

[0048] The composite membrane material prepared by using the composite membrane material casting liquid of the present invention has high flatness, balanced thickness and high strength, thereby improving the service life of the composite membrane material.

[0049] Preferably, in the method for preparing the composite membrane material casting solution, the bonding resin is added in batches.

[0050] Preferably, the preparation method further comprises adding a porogen and stirring after the first stirring and before adding the hydrophilic inorganic particles.

[0051] Preferably, the preparation method further comprises vacuum degassing the slurry after three stirrings.

[0052] Preferably, the vacuum degassing is carried out under a negative pressure of 0.5 bar to 3 bar, for example, 0.5 bar, 1 bar, 1.5 bar, 2 bar, 2.5 bar or 3 bar.

[0053] Preferably, the vacuum degassing time is 1 h to 3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h.

[0054] In a third aspect, the present invention provides an electrolytic cell, comprising the composite membrane material described in the first aspect.

[0055] Preferably, the electrolytic cell is an alkaline electrolytic cell.

[0056] By adopting the composite membrane material of the present invention, the stability of the alkaline water electrolyzer can be enhanced, the service life of the alkaline water electrolyzer can be increased, the replacement work of the composite membrane material caused by the short service life of the composite membrane material of the alkaline water electrolyzer can be reduced, the labor time consumption can be reduced, and the cost can be reduced.

[0057] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0058] Compared with the prior art, the present invention has the following beneficial effects:

[0059] (1) In the composite membrane material of the present invention, the coating contains a coupling agent, which has two functional groups with different properties, one is an inorganic-philic group and the other is an organic-philic group. Therefore, it plays a role in dispersing the casting liquid in the composite membrane material and enhancing the bonding strength between the adhesive resin and the hydrophilic inorganic particles.

[0060] (2) The composite membrane material of the present invention has strong alkali resistance, high strength, good toughness, good hydrophilicity, fast wetting speed and low surface resistance.

[0061] (3) By adopting the composite membrane material of the present invention, the stability of the alkaline water electrolyzer can be enhanced, and the service life of the alkaline water electrolyzer can be increased. The replacement work of the composite membrane material of the alkaline water electrolyzer due to the short service life of the composite membrane material is reduced, the labor time is reduced, and the cost is reduced. DETAILED DESCRIPTION

[0062] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0063] Example 1

[0064] The present embodiment provides an advanced composite membrane material for a water electrolysis hydrogen production process, wherein the composite membrane material has a thickness of 350 μm, comprises a polyphenylene sulfide (PPS) base membrane and a coating disposed on both sides of the base membrane, wherein the coating comprises a bonding resin, hydrophilic inorganic particles and a coupling agent, wherein the bonding resin is polysulfone, the hydrophilic inorganic particles are zirconium oxide, and the coupling agent is aminopropyltriethoxysilane.

[0065] The method for preparing the composite membrane material for an electrolytic cell provided in this embodiment comprises the following steps:

[0066] (1) Place the adhesive resin, hydrophilic inorganic particles and porogen (K30) in a forced air drying oven, set the temperature to 80°C, and bake for at least 4 hours until the weighed weight no longer changes.

[0067] (2) 30g of polysulfone was added to 80g of organic solvent N-methylpyrrolidone in batches, the speed was adjusted to 500r / min, and after stirring at 60°C for 3h, a uniformly dispersed polysulfone solution was obtained. Then 8g of porogen was added thereto at a speed of 500r / min. After stirring for 1h, 70g of hydrophilic inorganic particles were added in batches and stirred at a speed of 2000r / min for 15h. After adding 6g of coupling agent, stirring was continued at a speed of 2000r / min for 1h to obtain a uniformly dispersed milky white casting liquid. Transfer to a vacuum degassing device and degass at a negative pressure of 1bar for 2h to obtain a bubble-free casting liquid.

[0068] (3) Set the coating machine temperature to 50°C, pour the casting liquid onto the glass plate, soak the PPS in the casting liquid, set the thickness of the composite film material to 350 μm, and set the speed to 20 mm / min. After coating, pre-evaporate for 15 seconds at room temperature of 25°C and humidity of 45%, immerse in non-solvent water for phase inversion for 60 seconds, take out the composite film material, and store it in water.

[0069] Example 2

[0070] The present embodiment provides an advanced composite membrane material for a water electrolysis hydrogen production process, wherein the composite membrane material has a thickness of 350 μm, comprises a polyphenylene sulfide (PPS) base membrane and a coating disposed on both sides of the base membrane, wherein the coating comprises a bonding resin, hydrophilic inorganic particles and a coupling agent, wherein the bonding resin is polysulfone, the hydrophilic inorganic particles are zirconium oxide, and the coupling agent is aminopropyltriethoxysilane.

[0071] The method for preparing the composite membrane material for an electrolytic cell provided in this embodiment comprises the following steps:

[0072] (1) Place the adhesive resin, hydrophilic inorganic particles and porogen (K30) in a forced air drying oven, set the temperature to 80°C, and bake for at least 4 hours until the weighed weight no longer changes.

[0073] (2) Add 20g of polysulfone in batches into 80g of organic solvent N-methylpyrrolidone, adjust the speed to 500r / min, stir at 80℃ for 2h, and obtain a uniformly dispersed polysulfone solution. Then add 6g of porogen, stir at 700r / min for 0.5h, then add 70g of hydrophilic inorganic particles in batches, stir at 1500r / min for 15h, add 6g of coupling agent, continue to stir at 1500r / min for 1h, and obtain a uniformly dispersed milky white casting solution. Transfer to a vacuum degassing device and degas at a negative pressure of 1bar for 2h to obtain a bubble-free casting solution.

[0074] (3) Set the coating machine temperature to 50°C, pour the casting liquid onto the glass plate, soak the PPS in the casting liquid, set the thickness of the composite film material to 350 μm, and set the speed to 20 mm / min. After coating, pre-evaporate for 15 seconds at room temperature of 25°C and humidity of 30-50%, immerse in non-solvent water for phase inversion for 60 seconds, take out the composite film material, and store it in water after post-treatment.

[0075] Example 3

[0076] This embodiment provides an advanced composite membrane material for a water electrolysis hydrogen production process. The difference between the preparation method thereof and that of Embodiment 2 is that the amount of coupling agent used is 2 g.

[0077] Example 4

[0078] This embodiment provides an advanced composite membrane material for a water electrolysis hydrogen production process. The difference between the preparation method thereof and that of Embodiment 2 is that the amount of coupling agent used is 20 g.

[0079] Example 5

[0080] The present embodiment provides an advanced composite membrane material for a water electrolysis hydrogen production process, wherein the composite membrane material has a thickness of 350 μm, comprises a polyphenylene sulfide (PPS) base membrane and a coating disposed on both sides of the base membrane, wherein the coating comprises a bonding resin, hydrophilic inorganic particles and a coupling agent, wherein the bonding resin is polysulfone, the hydrophilic inorganic particles are zirconium oxide, and the coupling agent is aminopropyltriethoxysilane.

[0081] The method for preparing the composite membrane material for an electrolytic cell provided in this embodiment comprises the following steps:

[0082] (1) Place the adhesive resin, hydrophilic inorganic particles and porogen (K60) in a forced air drying oven at 75°C for at least 6 hours until the weight no longer changes.

[0083] (2) Add 20g of polysulfone in batches into 80g of organic solvent (N,N-dimethylacetamide), adjust the speed to 400r / min, and stir for a period of time to obtain a uniformly dispersed polysulfone solution. Then add 8g of porogen, continue to stir at the original speed for a period of time, then add 70g of hydrophilic inorganic particles in batches, stir for 12h, add 10g of coupling agent, stir for a period of time, and obtain a uniformly dispersed milky white casting liquid. Transfer to a vacuum degassing equipment and degas at a negative pressure of 1bar for 2h to obtain a bubble-free casting liquid.

[0084] (3) The coating machine temperature was set to 65°C, and the casting liquid was poured onto the glass plate. PPS was immersed in the casting liquid. The thickness of the composite film material described above was set to 220 μm, and the speed was set to 15 mm / min. After coating, the film was pre-evaporated for 20 seconds at room temperature of 25°C and humidity of 40%. The film was immersed in non-solvent water for phase inversion for 50 seconds, and the composite film material was taken out and stored in water after post-treatment.

[0085] Example 6

[0086] This embodiment provides an advanced composite membrane material for a water electrolysis hydrogen production process, which is different from Embodiment 1 in that the coupling agent is a monoalkoxy titanate.

[0087] Comparative Example 1

[0088] This comparative example provides an advanced composite membrane material for use in a water electrolysis hydrogen production process. The difference between its preparation method and that of Example 2 is that the amount of coupling agent used is 0 g.

[0089] Performance Test:

[0090] (1) Tensile strength:

[0091] Refer to the national standard GB / T528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber". The tensile strength test is carried out at room temperature to obtain the tensile strength.

[0092] (2) Surface resistance:

[0093] The composite diaphragms provided in the above embodiments and comparative examples were installed in an alkaline electrolytic cell device, and the electrochemical impedance was measured using a chemical workstation in a 30% KOH solution environment at 90° C. to calculate the surface resistance.

[0094] (3) Weight loss rate in alkali boiling experiment:

[0095] The composite diaphragm provided in the above embodiment and comparative example was placed in 30% KOH and heated to 95°C, kept for 24 hours, and then taken out and repeatedly washed in deionized water or distilled water until the pH value was 7. The weight of the diaphragm after alkali boiling was obtained by drying and weighing, and the alkali loss of the diaphragm was calculated as (weight before alkali boiling - weight after alkali boiling) / weight before alkali boiling * 100%.

[0096] The above tests were performed on Examples 1-6 and the composite membrane material, and the results are shown in Table 1.

[0097] Table 1

[0098]

[0099] As shown in Table 1, the present invention can significantly improve the strength and toughness of the composite membrane material by introducing a coupling agent into the casting solution and using the composite membrane material for the electrolytic cell, and reduce the mass loss caused by alkali boiling, and has the characteristics of low surface resistance, which can significantly improve the life of the alkaline water electrolytic cell. The composite diaphragm of Comparative Example 1 does not contain a coupling agent, and the strength of the composite membrane material is low, and the weight loss rate in the alkali boiling experiment (24h) is high, resulting in a short life of the alkaline hydrolysis cell.

[0100] From the comparison between Example 1 and Example 2, it can be seen that the mass ratio of the hydrophilic inorganic particles to the binding resin is preferably greater than 75 / 25.

[0101] By comparing Example 2 with Examples 3-4, it can be seen that there is a preferred range for the amount of coupling agent used. If the content of the coupling agent is too little, it is not conducive to the complete reaction of the adhesive resin and the hydrophilic inorganic particles, and the bonding strength is weak; if the content of the coupling agent is too much, part of the coupling agent will remain in the composite membrane material, which is not conducive to the bonding of the adhesive resin and the hydrophilic inorganic particles, resulting in increased surface resistance and a high weight loss rate in the alkali boiling experiment.

[0102] By comparing Example 1 with Example 6, it can be seen that there are preferred types of coupling agents. Compared with the titanate coupling agent in Example 6, the silane coupling agent used in Example 1 can better enhance the coupling effect between materials. This is because the titanate coupling agent is easily hydrolyzed in water and loses its coupling effect.

[0103] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An advanced composite membrane material for water electrolysis hydrogen production process, characterized in that: The composite film material comprises a base film and coatings arranged on both sides of the base film, wherein the coatings comprise a bonding resin, hydrophilic inorganic particles and a coupling agent.

2. The advanced composite membrane material for the process of producing hydrogen by electrolysis of water according to claim 1, characterized in that: The coupling agent includes at least one of a silane coupling agent and a titanate coupling agent; The bonding resin includes at least one of polysulfone, polyethersulfone, polyphenol, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene terephthalate and polybutylene terephthalate, preferably polysulfone; The hydrophilic inorganic particles include at least one of zirconium oxide, silicon oxide, magnesium oxide, zirconium hydroxide and magnesium hydroxide.

3. The advanced composite membrane material for the process of producing hydrogen by electrolysis of water according to claim 1, characterized in that: The base film is polyphenylene sulfide; The thickness of the composite membrane material is 220 μm-400 μm; The porosity of the composite membrane material is 40%-60%; The tensile strength of the composite membrane material is greater than 20 MPa.

4. A method for preparing an advanced composite membrane material for the process of producing hydrogen by electrolysis of water as claimed in any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: Placing the composite membrane material casting liquid on a coating machine glass plate, soaking the polyphenylene sulfide, coating it, pre-evaporating it, and then immersing it in a non-solvent for phase conversion to obtain the composite membrane material; The composite membrane material casting solution comprises an organic solvent, a bonding resin, hydrophilic inorganic particles and a coupling agent.

5. The method for preparing a composite membrane material according to claim 4, characterized in that: The temperature of the coating machine is set to 50°C to 70°C; The pre-evaporation is carried out at room temperature, and the ambient humidity is 30%-50%; The pre-evaporation time is 10s to 30s; The phase conversion time is 40s to 70s.

6. The method for preparing a composite membrane material according to claim 4, characterized in that: The solvent accounts for 30%-50% of the total mass of the composite membrane material casting solution; The bonding resin accounts for 10%-18% of the total mass of the composite membrane material casting liquid; The hydrophilic inorganic particles account for 30%-60% of the total mass of the composite membrane material casting solution; The mass ratio of the hydrophilic inorganic particles to the binding resin is greater than 65 / 35; The coupling agent accounts for 0.5%-8% of the total mass of the composite membrane material casting solution.

7. The method for preparing a composite membrane material according to claim 4, characterized in that: The composite membrane material casting solution also includes a porogen; The porogen includes polyvinyl pyrrolidone; The porogen accounts for 1%-10% of the total mass of the composite membrane material casting solution.

8. A method for preparing a composite membrane material as claimed in claim 4, characterized in that: The method for preparing the composite membrane material casting solution comprises the following steps: Putting an organic solvent into a vacuum disperser, adding a binder resin, stirring once, adding hydrophilic inorganic particles, stirring twice, adding a coupling agent, stirring three times, and obtaining the composite membrane material casting solution; The temperature of the first stirring is 50°C to 80°C, the first stirring is low-speed stirring, the speed is 300r / min-1000r / min, and the time is 1h to 3h; The secondary stirring is high-speed stirring, with a rotation speed of 1200r / min-2500r / min; The secondary stirring time is 12h~18h; The three stirrings are high-speed stirrings with a rotation speed of 1200r / min-2500r / min.

9. The method for preparing a composite membrane material according to claim 8, characterized in that: In the method for preparing the composite membrane material casting solution, the bonding resin is added in batches; The preparation method further comprises adding a porogen and stirring after the first stirring and before adding the hydrophilic inorganic particles; The preparation method further comprises vacuum degassing the slurry after three stirrings; The vacuum degassing is carried out under a negative pressure of 0.5 bar to 3 bar; The vacuum degassing time is 1 h to 3 h.

10. An electrolytic cell, characterized in that: The electrolytic cell comprises the composite membrane material according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • High-temperature-resistant alkaline water electrolytic bath composite diaphragm and preparation method thereof

    CN114432906A

  • Polysulfon-ZrO2 composite membrane material as well as preparation method and application thereof

    CN115181996A

  • Composite diaphragm for hydrogen production from alkaline electrolyzed water and capable of enhancing gas barrier property and preparation method of composite diaphragm

    CN117107297A

  • Alkaline electrolyzed water composite diaphragm as well as preparation method, device and application thereof

    CN117305902A

  • Method of producing inorganic organic composite film

    JP2019123904A

Cited By

  • Composite diaphragm for alkaline electrolyzed water and preparation method of composite diaphragm

    CN121228289A

  • Multi-layer cross-linked coupling diaphragm for hydrogen production by water electrolysis and preparation method of multi-layer cross-linked coupling diaphragm

    CN122147447A