Anodic oxidation method of high-strength medium-modulus polyacrylonitrile-based carbon fiber and carbon fiber

Through the two-stage anodization method, high-strength medium-mode carbon fibers are treated separately by inorganic and organic electrolytes, which solves the problem of reduced strength of carbon fibers and achieves a combination of high strength and high interface performance.

CN118996562APending Publication Date: 2024-11-22ZHONGFU SHENYING CARBON FIBER
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411126483.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the existing carbon fiber surface treatment methods improve the interface performance of high-strength medium-mode carbon fibers, it is easy to lead to a decrease in the strength of carbon fibers, especially the decrease in tensile strength, which cannot meet industrial needs.

Method used

Two-stage anodization method is adopted: first, the first-stage anodization treatment is performed in the inorganic electrolyte, the current density is not greater than 15A/m2, and the surface of the carbon fibers is etched to produce oxygen-containing and nitrogen-containing active functional groups; second-stage anodization is performed in the organic electrolyte The current density is 5-20A/m2, further increasing the surface roughness of carbon fiber and organic active functional groups to avoid strength damage.

Benefits of technology

It effectively improves the interface performance of high-strength medium-mode polyacrylonitrile-based carbon fiber, avoids a significant reduction in the strength of carbon fiber, maintains high tensile strength and modulus, and improves the bonding strength with the resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004996572650000101
    Figure BDA0004996572650000101
Patent Text Reader

Abstract

The invention relates to an anodic oxidation method of high-strength medium-modulus polyacrylonitrile-based carbon fibers and carbon fibers, and belongs to the technical field of carbon fiber surface treatment. The invention discloses an anodic oxidation method of high-strength medium-modulus polyacrylonitrile-based carbon fibers. The tensile strength of the high-strength medium-modulus polyacrylonitrile-based carbon fibers is 4500-7500 MPa, and the tensile modulus is 260-350 MPa; the anodic oxidation method comprises the steps that carbonized high-strength medium-modulus polyacrylonitrile-based carbon fibers are subjected to primary anodic oxidation treatment in inorganic electrolyte and then subjected to secondary anodic oxidation treatment in organic electrolyte; wherein the current density of the primary anodic oxidation treatment is not greater than 15A / m < 2 >. On the basis of improving the interface performance of the high-strength medium-modulus polyacrylonitrile-based carbon fiber, the strength of the carbon fiber is prevented from being greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of carbon fiber surface treatment, and in particular to an anodizing method for high-strength medium-modulus polyacrylonitrile-based carbon fiber and the carbon fiber. Background Art

[0002] Carbon fiber usually refers to carbon fiber with a carbon content of more than 90%. It has both the excellent inherent properties of carbon graphite materials and the good processing ability of textile fibers. It has the advantages of high strength, high modulus, good temperature resistance, excellent corrosion resistance, and low density. With decades of technological development, high-strength medium-modulus carbon fibers represented by T800, T1000, and T1100 grade carbon fibers have begun to emerge, gradually occupy the market, and become the focus of users. High-strength medium-modulus carbon fibers generally refer to carbon fibers with a tensile strength of 4500-7500MPa and a tensile modulus of 260-350GPa (GB / T 26752-2020).

[0003] The carbonization temperature of high-strength medium-modulus carbon fiber is relatively high, usually higher than 1400°C, the surface graphitization degree is relatively high, the surface inertness is high, and the bonding effect with the resin interface is weak, so surface treatment is more necessary to improve the interface performance. After surface treatment, oxygen-containing and nitrogen-containing active functional groups are introduced into the surface of the carbon fiber, the wettability of the fiber surface is enhanced, and the roughness is greatly increased. The physical intercalation and chemical bonding with the resin matrix are enhanced, and finally the performance of carbon fiber composite materials is improved.

[0004] The online supporting methods for carbon fiber surface treatment at home and abroad are mostly anodic oxidation. The advantages of this method are easy control, mild reaction conditions, short processing time, and great operational flexibility. The selective control of the degree of carbon fiber oxidation and surface functional groups can be achieved by controlling process conditions such as electrolyte type, electrolyte concentration, current density, and surface treatment level.

[0005] However, the anodic oxidation electrolytes currently used for carbon fiber surface treatment are mostly inorganic electrolytes, such as sulfuric acid, sodium hydroxide, ammonium bicarbonate, sodium bicarbonate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, etc. For high-strength and low-modulus carbon fibers, inorganic electrolytes basically meet their industrialization needs, but for high-strength and medium-modulus carbon fibers with higher surface inertness, in order to achieve the desired effect of improving interface performance, higher current density and more surface treatment levels are required, which often results in a decrease in carbon fiber performance, especially tensile strength. Therefore, there is an urgent need to improve the anodic oxidation process and equipment. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the embodiments of the present application includes providing an anodizing method for high-strength medium-modulus polyacrylonitrile-based carbon fiber and carbon fiber, which can improve the interface performance of the high-strength medium-modulus polyacrylonitrile-based carbon fiber while avoiding a significant reduction in the strength of the carbon fiber.

[0007] In the first aspect, the embodiment of the present application provides an anodizing method for high-strength medium-modulus polyacrylonitrile-based carbon fiber, wherein the tensile strength of the high-strength medium-modulus polyacrylonitrile-based carbon fiber is 4500-7500MPa, and the tensile modulus is 260-350MPa; the anodizing method comprises: subjecting the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber to a primary anodizing treatment in an inorganic electrolyte, and then subjecting the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber to a secondary anodizing treatment in an organic electrolyte; wherein the current density of the primary anodizing treatment is not greater than 15A / m 2 .

[0008] The present invention relates to a method for treating carbonized high-strength medium-modulus polyacrylonitrile-based carbon fibers by first using an inorganic electrolyte at a temperature not greater than 15A / m 2 The primary anodizing treatment is carried out at a current density of , which can effectively etch the surface of the carbon fiber to produce oxygen-containing and nitrogen-containing active functional groups, increase the surface roughness and wettability of the carbon fiber, and avoid excessive damage to the strength of the carbon fiber; the carbon fiber is then subjected to secondary anodizing treatment using an organic electrolyte. On the basis of avoiding further excessive damage to the strength of the carbon fiber, a large number of organic active functional groups can be further effectively etched on the surface of the carbon fiber to introduce further. The roughness of the carbon fiber surface is further increased; thereby achieving the improvement of the interface properties of the high-strength medium-modulus polyacrylonitrile-based carbon fiber while avoiding a significant reduction in the strength of the carbon fiber.

[0009] In some embodiments of the present application, the current density of the primary anodizing treatment is 2-15 A / m 2 .

[0010] In some embodiments of the present application, the current density of the primary anodizing treatment is 5-10 A / m 2 .

[0011] The present application sets a suitable current density for the primary anodizing treatment so as to avoid excessive damage to the strength of the carbon fiber while effectively etching the surface of the carbon fiber.

[0012] In some embodiments of the present application, the current density of the secondary anodizing treatment is 5-20A / m 2 .

[0013] In some embodiments of the present application, the current density of the secondary anodizing treatment is 7-15 A / m 2 .

[0014] The present application sets a suitable current density for the secondary anodizing treatment so that the organic electrolyte can effectively etch the carbon fiber surface and also reduce excessive damage to the strength of the carbon fiber to a certain extent.

[0015] In some embodiments of the present application, the inorganic electrolyte includes at least one of sulfuric acid, nitric acid, sodium hydroxide, potassium hydroxide, ammonium bicarbonate, sodium bicarbonate, and diammonium phosphate.

[0016] The present application can effectively perform primary anodization treatment on carbon fiber by adopting at least one of the above-mentioned inorganic electrolytes.

[0017] In some embodiments of the present application, the mass concentration of the inorganic electrolyte is 2-15%.

[0018] In some embodiments of the present application, the mass concentration of the inorganic electrolyte is 5-10%.

[0019] The present application can effectively perform primary anodization treatment on carbon fibers by using an inorganic electrolyte of suitable mass concentration, and also reduce excessive damage to the strength of the carbon fibers to a certain extent.

[0020] In some embodiments of the present application, the organic electrolyte includes at least one of citric acid, sodium citrate, tartaric acid, sodium tartrate, glyceric acid, and sodium glycerate.

[0021] The present application can effectively perform secondary anodization treatment on carbon fibers by adopting at least one of the above-mentioned organic electrolytes, and can reduce excessive damage to the strength of the carbon fibers.

[0022] In some embodiments of the present application, the mass concentration of the organic electrolyte is 2-20%.

[0023] In some embodiments of the present application, the mass concentration of the organic electrolyte is 5-15%.

[0024] The present application can effectively perform secondary anodization treatment on carbon fibers by adopting an organic electrolyte with a suitable mass concentration, and also reduce excessive damage to the strength of the carbon fibers to a certain extent.

[0025] In some embodiments of the present application, the temperature of the inorganic electrolyte and the organic electrolyte are both 30-70°C.

[0026] The present application can effectively perform anodization treatment on carbon fiber by performing primary anodization treatment and secondary anodization treatment on carbon fiber using inorganic electrolyte and organic electrolyte at suitable temperature.

[0027] In some embodiments of the present application, the speed of the primary anodizing treatment and the secondary anodizing treatment of the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber is 150-400 m / h.

[0028] In some embodiments of the present application, the speed of the primary anodizing treatment and the secondary anodizing treatment of the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber is 200-300 m / h.

[0029] The present application can effectively perform anodization treatment on carbon fiber by performing primary anodization treatment and secondary anodization treatment on carbon fiber at an appropriate speed.

[0030] In a second aspect, an embodiment of the present application provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber obtained after anodizing treatment according to the first aspect.

[0031] In the present application, after the high-strength medium-modulus polyacrylonitrile-based carbon fiber is subjected to the above-mentioned anodizing treatment, the high-strength medium-modulus polyacrylonitrile-based carbon fiber interface obtained has a high bonding strength with the resin, and at the same time, the strength of the carbon fiber will not be significantly reduced. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0033] Since the carbonization temperature of high-strength medium modulus carbon fiber is often higher than 1400°C, the degree of graphitization on its surface is relatively high, so that its surface inertia is high and the bonding effect with the resin interface is weak. In order to improve the current problems of high surface inertia and weak bonding effect with the resin interface of high-strength medium modulus carbon fiber, it is necessary to perform anodization treatment on the surface of high-strength medium modulus carbon fiber to improve the interface performance of the surface of high-strength medium modulus carbon fiber; however, when an inorganic electrolyte is currently used to perform anodization treatment on the surface of high-strength medium modulus carbon fiber, in order to achieve the desired effect of improving the interface performance, a higher current density and more surface treatment levels are required, which often results in a decrease in the performance of carbon fiber, especially the tensile strength. In order to improve the current problem of a significant decrease in the strength of carbon fiber when an inorganic electrolyte is used for anodization treatment on the surface of carbon fiber. The embodiment of the present application provides an anodizing method for high-strength medium-modulus polyacrylonitrile-based carbon fiber, wherein the tensile strength of the high-strength medium-modulus polyacrylonitrile-based carbon fiber is 4500-7500MPa, and the tensile modulus is 260-350MPa; the anodizing method comprises: subjecting the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber to a primary anodizing treatment in an inorganic electrolyte, and then subjecting the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber to a secondary anodizing treatment in an organic electrolyte; wherein the current density of the primary anodizing treatment is not greater than 15A / m 2 .

[0034] The carbonized high-strength medium-modulus polyacrylonitrile-based carbon fibers are first treated with an inorganic electrolyte at no more than 15A / m 2 The primary anodizing treatment is carried out at a current density of , which can effectively etch the surface of the carbon fiber to produce oxygen-containing and nitrogen-containing active functional groups, increase the surface roughness and wettability of the carbon fiber, and avoid excessive damage to the strength of the carbon fiber; the carbon fiber is then subjected to secondary anodizing treatment using an organic electrolyte. On the basis of avoiding further excessive damage to the strength of the carbon fiber, a large number of organic active functional groups can be further effectively etched on the surface of the carbon fiber to introduce further. The roughness of the carbon fiber surface is further increased; thereby achieving the improvement of the interface properties of the high-strength medium-modulus polyacrylonitrile-based carbon fiber while avoiding a significant reduction in the strength of the carbon fiber.

[0035] In some embodiments of the present application, the current density of the primary anodizing treatment is 2-15 A / m 2 Furthermore, the current density of the primary anodizing treatment is 5-10A / m 2 As an example, the current density of the primary anodizing treatment may be, but is not limited to, 2 A / m 2 , 3A / m 2 , 4A / m 2 , 5A / m 2 , 6A / m 2 , 7A / m 2 , 8A / m 2 , 9A / m 2 , 10A / m 2 , 11A / m 2 , 12A / m 2 , 13A / m 2 , 14A / m 2 , 15A / m 2 The current density of the primary anodizing treatment is set appropriately to avoid excessive damage to the strength of the carbon fiber while effectively etching the carbon fiber surface.

[0036] In some embodiments of the present application, the current density of the secondary anodizing treatment is 5-20A / m 2 Furthermore, the current density of the secondary anodizing treatment is 7-15A / m 2 As an example, the current density of the secondary anodizing treatment may be, but is not limited to, 5 A / m 2 , 6A / m 2 , 7A / m 2 , 8A / m 2 , 9A / m 2 , 10A / m 2 , 11A / m 2 , 12A / m2 , 13A / m 2 , 14A / m 2 , 15A / m 2 , 16A / m 2 , 17A / m 2 , 18A / m 2 , 19A / m 2 , 20A / m 2 The current density of the secondary anodizing treatment is set appropriately so that the organic electrolyte can effectively etch the carbon fiber surface and reduce excessive damage to the strength of the carbon fiber to a certain extent.

[0037] In some embodiments of the present application, the inorganic electrolyte includes at least one of sulfuric acid, nitric acid, sodium hydroxide, potassium hydroxide, ammonium bicarbonate, sodium bicarbonate, and ammonium dihydrogen phosphate. Using at least one of the above inorganic electrolytes, the carbon fiber can be effectively subjected to primary anodization treatment.

[0038] In some embodiments of the present application, the mass concentration of the inorganic electrolyte is 2-15%. Specifically, the mass concentration of the inorganic electrolyte in the electrolyte used for the primary anodizing treatment is 2-15%. Further, the mass concentration of the inorganic electrolyte is 5-10%. As an example, the mass concentration of the inorganic electrolyte can be, but is not limited to, any point value among 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, or a range value between any two. Using an inorganic electrolyte with an appropriate mass concentration, the carbon fiber can be effectively subjected to the primary anodizing treatment, and to a certain extent, it also reduces excessive damage to the strength of the carbon fiber.

[0039] In some embodiments of the present application, the organic electrolyte includes at least one of citric acid, sodium citrate, tartaric acid, sodium tartrate, glyceric acid, and sodium glycerate. Using at least one of the above organic electrolytes, the carbon fiber can be effectively subjected to secondary anodization treatment, and excessive damage to the strength of the carbon fiber can be reduced.

[0040] In some embodiments of the present application, the mass concentration of the organic electrolyte is 2-20%. Specifically, the mass concentration of the organic electrolyte in the electrolyte used for the secondary anodizing treatment is 2-20%. Further, the mass concentration of the organic electrolyte is 5-15%. As an example, the mass concentration of the organic electrolyte can be, but is not limited to, any point value among 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or any range value between two of them. Using an organic electrolyte with an appropriate mass concentration, the carbon fiber can be effectively subjected to secondary anodizing treatment, and to a certain extent, it also reduces excessive damage to the strength of the carbon fiber.

[0041] In some embodiments of the present application, the temperature of the inorganic electrolyte and the organic electrolyte are both 30-70°C. Specifically, the temperature of the electrolyte used for the primary anodizing treatment and the secondary anodizing treatment is 30-70°C. As an example, the temperature of the inorganic electrolyte and the organic electrolyte can be, but is not limited to, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, and 70°C. The use of inorganic electrolytes and organic electrolytes at suitable temperatures to perform primary anodizing and secondary anodizing treatments on carbon fibers can effectively perform anodizing on the carbon fibers.

[0042] In some embodiments of the present application, the speed of the primary anodizing treatment and the secondary anodizing treatment of the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber is 150-400m / h. Further, the speed of the primary anodizing treatment and the secondary anodizing treatment of the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber is 200-300m / h. As an example, the speed of the primary anodizing treatment and the secondary anodizing treatment of the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber can be, but not limited to, 150m / h, 180m / h, 200m / h, 220m / h, 250m / h, 280m / h, 300m / h, 320m / h, 350m / h, 380m / h, 400m / h. The carbon fiber can be effectively anodized by performing the primary anodizing treatment and the secondary anodizing treatment at an appropriate speed.

[0043] The embodiment of the present application provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber obtained after the above-mentioned anodizing method.

[0044] After the high-strength medium-modulus polyacrylonitrile-based carbon fiber is subjected to the above-mentioned anodizing treatment, the obtained high-strength medium-modulus polyacrylonitrile-based carbon fiber has a high bonding strength at the interface with the resin, and at the same time, the strength of the carbon fiber will not be greatly reduced.

[0045] In some embodiments of the present application, the high-strength medium-modulus polyacrylonitrile-based carbon fiber after anodizing treatment is further washed, sizing, dried, and wound to obtain a finished high-strength medium-modulus polyacrylonitrile-based carbon fiber.

[0046] In some embodiments of the present application, sizing can be performed using epoxy sizing agents or bismuth sizing agents.

[0047] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0048] Example 1

[0049] This embodiment provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and the anodizing method thereof comprises the following steps:

[0050] (1) The carbonized carbon fiber is charged at a current density of 5A / m 2 , a primary anodizing treatment is carried out in a NaOH electrolyte with a mass concentration of 5% and a processing speed of 200m / h;

[0051] (2) The primary anodized carbon fiber was subjected to a current density of 7 A / m 2 , secondary surface treatment is carried out in a sodium citrate electrolyte with a mass concentration of 5% and a treatment speed of 200m / h;

[0052] (3) The carbon fiber after the secondary anodizing treatment is washed with water, and then sizing is performed using an epoxy sizing agent, and then dried and wound to obtain a finished high-strength medium-modulus polyacrylonitrile-based carbon fiber CF-1.

[0053] Embodiment 2-6

[0054] Example 2-6 provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and its anodization method is different from that of Example 1 in that the current density of the primary anodization treatment and the secondary anodization treatment are different, as shown in Table 1 for details.

[0055] Embodiment 7-9

[0056] Embodiment 7-9 provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and the difference between the anodization method thereof and that of Embodiment 4 is that the mass concentrations of the inorganic electrolyte and the organic electrolyte are different, as shown in Table 1 for details.

[0057] Example 10

[0058] Example 10 provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and its anodizing method is different from that of Example 8 in that the speeds of the primary anodizing treatment and the secondary anodizing treatment are different, as shown in Table 1 for details.

[0059] Examples 11-13

[0060] Examples 11-13 provide a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and the anodization method thereof is different from that of Example 8 in that the type of inorganic electrolyte and the current density of the primary anodization treatment are different, as shown in Table 1 for details.

[0061] Embodiment 14

[0062] Example 14 provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and its anodizing method is different from that of Example 12 in that the speeds of the primary anodizing treatment and the secondary anodizing treatment are different, as shown in Table 1 for details.

[0063] Examples 15-17

[0064] Examples 15-17 provide a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and the anodization method thereof is different from that of Example 8 in that the type of inorganic electrolyte and the current density of the primary anodization treatment are different, as shown in Table 1 for details.

[0065] Embodiment 18

[0066] Example 18 provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and its anodizing method is different from that of Example 16 in that the speeds of the primary anodizing treatment and the secondary anodizing treatment are different, as shown in Table 1 for details.

[0067] Embodiment 19

[0068] Example 19 provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and its anodization method is different from that of Example 8 in that the type of organic electrolyte used is different, as shown in Table 1 for details.

[0069] Comparative Example 1

[0070] This comparative example provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and the difference between its anodizing method and that of Example 8 is that the current density of the primary anodizing treatment is 20A / m 2 ;

[0071] The obtained finished product is high-strength medium-modulus polyacrylonitrile-based carbon fiber G-1.

[0072] Comparative Example 2

[0073] This comparative example provides a high-strength medium-modulus polyacrylonitrile-based carbon fiber, and its anodizing method comprises the following steps:

[0074] (1) The carbonized carbon fiber is charged at a current density of 7A / m 2 , a primary anodizing treatment is carried out in a NaOH electrolyte with a mass concentration of 7% and a processing speed of 200m / h;

[0075] (2) The primary anodized carbon fiber was subjected to a current density of 10 A / m 2 , secondary surface treatment is carried out in a NaOH electrolyte with a mass concentration of 10% and a treatment speed of 200m / h;

[0076] (3) The carbon fiber after the secondary anodizing treatment is washed with water, and then sizing is performed using an epoxy sizing agent, and then dried and wound to obtain a finished high-strength medium-modulus polyacrylonitrile-based carbon fiber G-2.

[0077] The anodizing methods of carbon fibers provided in Examples 1-19 and Comparative Examples 1-2 are shown in Table 1.

[0078] Table 1 Anodizing method

[0079]

[0080] Test Example 1

[0081] In this test example, the carbon fibers provided in Examples 1-19 and Comparative Examples 1-2 were tested for surface oxygen content, tensile strength, tensile modulus, and interlaminar shear strength. The carbon fibers used were T800 grade carbon fibers, with a batch tensile modulus of 5951 MPa and a batch tensile modulus of 298 GPa. The surface oxygen content of the carbon fibers was measured by X-ray photoelectron spectroscopy, and the carbon fibers were subjected to a full spectrum scan. The surface oxygen content was the atomic percentage of oxygen. The tensile strength and tensile modulus were tested according to GB / T 3362-2017, and the interlaminar shear strength was tested according to GB / T 1450.1-2005. The results are shown in Table 2.

[0082] Table 2 Carbon fiber properties

[0083] Surface oxygen content (%) Tensile strength(MPa) Tensile modulus(GPa) Layer shear strength (MPa) CF-1 11.63 5888 297 76.31 CF-2 12.09 5876 297 78.42 CF-3 12.51 5864 296 79.08 CF-4 12.93 5830 298 85.24 CF-5 12.94 5824 297 87.25 CF-6 13.18 5811 298 91.14 CF-7 13.29 5806 297 94.25 CF-8 13.86 5805 297 98.14 CF-9 13.88 5801 297 98.17 CF-10 12.15 5846 296 89.75 CF-11 11.84 5840 298 85.57 CF-12 11.95 5814 296 85.46 CF-13 12.14 5791 296 91.04 CF-14 11.75 5748 297 89.01 CF-15 11.38 5904 298 69.37 CF-16 11.62 5875 296 82.94 CF-17 11.94 5865 296 88.99 CF-18 11.43 5889 297 87.56 CF-19 13.11 5765 297 92.85 G-1 12.61 5714 296 86.42 G-2 12.64 5582 298 77.85

[0084] It can be seen from the results in Table 2 that, compared with Examples 1-9, with the increase of current density and electrolyte concentration, the degree of etching increases, and the surface oxygen content and interlaminar shear strength both show an upward trend; however, too high inorganic electrolyte concentration and current density will cause fiber damage, causing the tensile strength of the carbon fiber after anodization to decrease to varying degrees, and the tensile modulus is less affected by anodization. The use of a suitable current density in an inorganic electrolyte for primary anodization and then a secondary anodization in an organic electrolyte can effectively improve the interface properties of high-strength medium-modulus polyacrylonitrile-based carbon fibers and avoid a substantial reduction in the strength of the carbon fibers.

[0085] Comparing Examples 11-13 with Examples 15-16, other inorganic electrolytes, such as sulfuric acid and ammonium bicarbonate, were selected. The anodization effect was similar to that of sodium hydroxide. With the increase of the current density of the inorganic electrolyte, the surface oxygen content and the interlaminar shear strength both showed an upward trend. Moderate electrolyte concentration and current density had the best anodization effect on carbon fiber.

[0086] Comparing Example 8 with Example 10, Example 12 with Example 14, and Example 16 with Example 18, the anodizing effect is weakened to a certain extent by increasing the line speed.

[0087] Comparing Example 8 with Example 19, other organic electrolytes, such as sodium tartrate, were selected, and the anodic oxidation effect was good, but slightly worse than that of sodium citrate.

[0088] Compared with Example 8 and Comparative Example 1, the current density of the inorganic electrolyte is too high, resulting in a large degree of surface group etching, a large loss of carbon fiber strength, and low interlayer shear strength.

[0089] Comparative Example 8 and Comparative Example 2, both stages use inorganic electrolytes for anodization, which will result in excessive surface group etching, excessive carbon fiber strength loss, and low interlaminar shear strength.

[0090] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

Claims

1. A method for anodizing high-strength medium-modulus polyacrylonitrile-based carbon fibers, characterized in that: The high-strength medium-modulus polyacrylonitrile-based carbon fiber has a tensile strength of 4500-7500 MPa and a tensile modulus of 260-350 MPa; the anodizing method comprises: subjecting the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber to a primary anodizing treatment in an inorganic electrolyte, and then to a secondary anodizing treatment in an organic electrolyte; The current density of the primary anodizing treatment is not more than 15A / m 2 .

2. The anodizing method according to claim 1, characterized in that: The current density of the primary anodizing treatment is 2-15A / m 2 ; preferably 5-10A / m 2 .

3. The anodizing method according to claim 1, characterized in that: The current density of the secondary anodizing treatment is 5-20A / m 2 ; preferably 7-15A / m 2 .

4. The anodizing method according to claim 1, characterized in that: The inorganic electrolyte includes at least one of sulfuric acid, nitric acid, sodium hydroxide, potassium hydroxide, ammonium bicarbonate, sodium bicarbonate, and diammonium phosphate.

5. The anodizing method according to claim 4, characterized in that: The mass concentration of the inorganic electrolyte is 2-15%, preferably 5-10%.

6. The anodizing method according to claim 1, characterized in that: The organic electrolyte includes at least one of citric acid, sodium citrate, tartaric acid, sodium tartrate, glyceric acid and sodium glycerate.

7. The anodizing method according to claim 6, characterized in that: The mass concentration of the organic electrolyte is 2-20%, preferably 5-15%.

8. The anodizing method according to claim 1, characterized in that: The temperature of the inorganic electrolyte and the organic electrolyte are both 30-70°C.

9. The anodizing method according to claim 1, characterized in that: The speed of the primary anodizing treatment and the secondary anodizing treatment of the carbonized high-strength medium-modulus polyacrylonitrile-based carbon fiber is 150-400 m / h, preferably 200-300 m / h.

10. A high-strength medium-modulus polyacrylonitrile-based carbon fiber obtained by anodizing treatment according to any one of claims 1 to 9.

Citation Information

Cited By

  • Wear-resistant nanofiber reinforced protective graphene fiber as well as preparation method and application thereof

    CN119900120A

  • Wear-resistant nanofiber-reinforced protective graphene fibers and their preparation methods and applications