Cubic-phase all-inorganic lead-based perovskite material, preparation method and application
By doping Cd elements into lead-based perovskite materials, CsPbmCd1-mBr3 is formed, and the problem of structural distortion in the material during cooling is solved, and cubic phase all-inorganic lead-based perovskite with high symmetry and strong stability is achieved. Materials improve their optoelectronic performance and applicability.
Patent Information
- Application Number
- CN202410949220.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-22
AI Technical Summary
Existing all-inorganic lead-based perovskite materials are prone to spontaneous polarization and structural distortion during the cooling process, resulting in a decrease in symmetry and it is difficult to maintain the cubic phase structure, affecting its stability and performance.
By doping an appropriate amount of Cd elements into the lead-based perovskite material CsPbBr3, the chemical formula of CsPbmCd1-mBr3 is formed, and single crystals are grown by melt method to ensure that the material maintains a cubic phase structure during the cooling process. In the chemical formula, 0.7 < m < 0.82 , in the specific embodiment, 0.72≤m≤0.76, the preferred chemical formula is CsPb0.72Cd0.28Br3.
A cubic phase all-inorganic lead-based perovskite material with high symmetry, simple structure and strong stability is realized, which enhances its photon signal absorption capacity and electron mobility, is suitable for large-area detection applications, and reduces the preparation cost.
Smart Images

Figure CN118996628A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of perovskite photoelectric materials, and in particular to a cubic phase all-inorganic lead-based perovskite material, a preparation method and an application thereof. Background Art
[0002] Perovskite is a crystalline material with a molecular formula of ABX3, an octahedral shape, and excellent structural characteristics. The preparation process of perovskite crystals is simple and the photoelectric conversion efficiency is high. In recent years, it has been widely used in photovoltaics, LEDs, and radiation detection. Perovskite materials are considered to be one of the most promising optoelectronic materials of the next generation due to their high light absorption coefficient, large carrier mobility, and simple synthesis methods.
[0003] Lead-based halide perovskite materials have advantages such as high absorption coefficient, long carrier diffusion length, adjustable band gap, small effective mass (high mobility), and defect tolerance characteristics brought by antibonding orbitals; while all-inorganic perovskites show high stability (voltage stability, temperature stability) and large attenuation coefficient; large-sized all-inorganic perovskite single crystals can be grown using the melt method, which has strong applications in many fields. In general, all-inorganic lead-based perovskite materials, including Rb / Cs+Pb+Cl / Br / I, can be used for radiation detection or other scenarios.
[0004] At present, there are many studies on all-inorganic lead-based perovskite materials, and the research generally focuses on replacing Cs at the A position with larger ions, but the only ions larger than Cs can be organic ions (such as MA + , FA + etc.), which leads to the loss of other properties (i.e. stability, attenuation coefficient, size). In the process of cooling the CsPbBr3 perovskite crystal prepared by the melt method from high temperature to room temperature, thermal motion will cause spontaneous polarization. Spontaneous polarization is mainly caused by the deviation of certain ions in the crystal from the equilibrium position, which causes the appearance of dipole moments in the unit cell. Due to the interaction between the dipole moments, the ions that deviate from the equilibrium position stabilize at the new position, and the crystal structure is distorted. The structural distortion process of the perovskite material during the cooling process reduces its symmetry. If distortion occurs in one axis, it will change from cubic phase to tetragonal phase. If distortion occurs in two axes, it will become orthorhombic phase.
[0005] Therefore, preparing new perovskite materials with high performance, such as high symmetry and strong stability, has become one of the important tasks for materials scientists. Summary of the invention
[0006] In view of this, the purpose of the present application is to provide a new perovskite material with a stable cubic phase and a preparation method thereof. Compared with other phase materials, the new perovskite material with a cubic phase has the following advantages: high symmetry. The cubic symmetry enables the cubic phase to play an important role in crystallography and is widely used in the preparation and application of many materials; simple structure. The structure of the cubic phase material is simple and clear, with a high degree of regularity, which is suitable for the preparation of high-quality single crystals, and its research in crystallographic theory is relatively easy; strong stability. The physical properties of the cubic phase material are stable, and the stability is higher under high temperature, high pressure and the like.
[0007] To achieve the above objectives, this application provides the following technical solutions:
[0008] In the first aspect, the present application provides a cubic all-inorganic lead-based perovskite material, wherein the cubic all-inorganic lead-based perovskite material is doped with Cd element at the B position of the lead-based perovskite material CsPbBr3, and its chemical formula is CsPb m Cd 1- m Br3, wherein 0.7<m<0.82.
[0009] In certain embodiments, the chemical formula of the cubic all-inorganic lead-based perovskite material is CsPb m Cd 1- m Br3, where 0.72≤m≤0.76.
[0010] In certain preferred embodiments, the chemical formula of the cubic all-inorganic lead-based perovskite material is CsPb 0.72 Cd 0.28 Br3.
[0011] In a second aspect, the present application provides a method for preparing the aforementioned cubic all-inorganic lead-based perovskite material, comprising:
[0012] Take the raw material CsPbBr3 and the raw material CsCdBr3, grind them into powder respectively;
[0013] The powdered raw material CsPbBr3 and the raw material CsCdBr3 are uniformly mixed to obtain a mixed raw material;
[0014] The mixed raw materials are placed at 600-700° C. for heat preservation treatment; then the mixed raw materials are cooled to room temperature to obtain raw material powder of single crystal alloy;
[0015] The single crystal alloy raw material powder is placed in a heating furnace for single crystal growth to obtain a cubic phase all-inorganic lead-based perovskite material.
[0016] In a third aspect, the present application provides the application of the aforementioned cubic phase all-inorganic lead-based perovskite material and / or the aforementioned preparation method in the preparation of energy spectrum CT and area array imaging detectors.
[0017] This application discloses a cubic all-inorganic lead-based perovskite material, preparation method and application, which has at least the following advantages compared with the prior art:
[0018] (1) The present application provides a cubic phase all-inorganic lead-based perovskite new material prepared by doping B-site ions. The lattice structure of the perovskite new material is a pure cubic phase. Compared with the existing perovskite photoelectric materials, it has more obvious advantages, which are manifested in high symmetry, simple structure, strong stability, strong defect tolerance, etc.; using the cubic phase all-inorganic lead-based perovskite new material as a photoelectric material can absorb more photon signals, thereby generating a larger electrical signal and having a higher electron mobility. In addition, the cubic phase all-inorganic lead-based perovskite new material has a large crystal size, is easy to process, and is suitable for large-area detection.
[0019] (2) The preparation method of the cubic phase all-inorganic lead-based perovskite new material provided in this application has a simple process, low cost, low instrument requirements, and is suitable for large-scale development. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The cubic all-inorganic lead-based perovskite material CsPb prepared in Example 1 0.72 Cd 0.28 Br3 crystal sample picture.
[0021] Figure 2 The cubic all-inorganic lead-based perovskite material CsPb prepared in Example 1 0.72 Cd 0.28 Br3 binary phase diagram.
[0022] Figure 3 The cubic all-inorganic lead-based perovskite material CsPb prepared in Example 1 0.72 Cd 0.28 XRD test results of Br3.
[0023] Figure 4 These are the standard XRD cards corresponding to the three crystal space groups of 221, 194, and 62.
[0024] Figure 5 The cubic all-inorganic lead-based perovskite material CsPb prepared in Example 1 0.72 Cd 0.28 Attenuation performance test results of Br3.
[0025] Figure 6The cubic all-inorganic lead-based perovskite material CsPb prepared in Example 1 0.72 Cd 0.28 IV test results of Br3.
[0026] Figure 7 The cubic all-inorganic lead-based perovskite material CsPb prepared in Example 1 0.72 Cd 0.28 It test results of Br3. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0028] Explanation of terms
[0029] In this application, the term "cubic phase" refers to the presence of cubic symmetry in the crystal structure. The crystal structure of the cubic phase material has a simple cubic system or a body-centered cubic system structure. The most basic unit cell contains a cubic symmetry element. The lattice structure of this material is relatively simple, regular and has high stability. The total number of crystal space groups is 230, which is obtained by combining 32 point groups with translation operations in three-dimensional space. Each space group can uniquely describe the structure of a crystalline material. These space groups are numbered from 1 to 230, and they can be classified according to 7 crystal systems: triclinic, monoclinic, orthorhombic, tetragonal, hexagonal and cubic. The term "221 cubic phase" or "221 space group" means that the material belongs to the cubic system, the 221st space group. Similarly, the terms "194 space group" and "62 space group" belong to the 194th and 62nd space groups of 230 space groups, respectively.
[0030] In this application, the term "tetragonal phase" refers to a common, stable type of crystal structure, which is composed of tetrahedrons and octahedrons, wherein the tetrahedron is a triangular pyramid structure composed of four atoms, and the octahedron is a polyhedron structure composed of eight atoms. The unit cell of the tetragonal phase crystal structure is a cube, in which there is a tetrahedron and an octahedron at each corner. This structure has a high symmetry because it has four-fold axial symmetry and four-fold rotational symmetry.
[0031] In this application, the term "orthorhombic phase" refers to a crystal structure having three mutually perpendicular two-fold axes, ie, three equivalent axes that are mutually perpendicular. There are two forms of orthorhombic lattices: simple orthorhombic and body-centered orthorhombic.
[0032] In the present application, the term "solid solution" refers to an alloy phase in which solute atoms are dissolved in a solvent lattice while still maintaining the solvent type, and refers to a crystal composed of one chemical substance as a matrix and atoms or molecules of other substances dissolved therein.
[0033] In the present application, the term "preferred" is only used to describe an implementation method or example with better effects, and it should be understood that it does not constitute a limitation on the scope of protection of the present invention.
[0034] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0035] In the present application, reference to a numerical range includes both endpoints of the numerical range unless otherwise specified.
[0036] The ideal perovskite (ABX3) is a cubic structure, with each octahedron connected at a vertex, and A is in the gap of the octahedron, so it is a cubic structure. If B is displaced along the longitudinal axis of the octahedron, it becomes a tetragonal system. If different degrees of expansion and contraction occur in the two axial directions, it becomes an orthorhombic system. The embodiment of the present application dopes the B site of the traditional lead-based perovskite material with a suitable content of Cd element content, so that the octahedral structure cannot be displaced in the longitudinal direction. The single crystal grown by the melt method will not be distorted during the cooling process, and the cubic phase structure is always maintained to form a new all-inorganic lead-based perovskite. The new all-inorganic lead-based perovskite is embodied as a "221 cubic phase", which not only has the performance of traditional all-inorganic lead-based perovskite materials, but also has more obvious advantages, which are manifested in high symmetry, simple structure, strong stability and other aspects. Using this cubic phase of all-inorganic lead-based perovskite new material as a photoelectric material can absorb more photon signals, thereby generating larger electrical signals and having a higher electron mobility. In addition, this cubic phase of all-inorganic lead-based perovskite new material has a large crystal size, is easy to process, and is suitable for large-area detection.
[0037] Based on this, the embodiment of the present application provides a cubic phase all-inorganic lead-based perovskite material, wherein the cubic phase all-inorganic lead-based perovskite material is doped with Cd element at the B position of the lead-based perovskite material CsPbBr3, and its chemical formula is CsPb m Cd 1-m Br3, wherein 0.7<m<0.82.
[0038] In certain embodiments, the chemical formula of the cubic all-inorganic lead-based perovskite material is CsPb m Cd 1-m Br3, where 0.72≤m≤0.76.
[0039] In certain preferred embodiments, the chemical formula of the cubic all-inorganic lead-based perovskite material is CsPb0.72 Cd 0.28 Br3, that is, when the molar ratio of Pb element to Cd in the B-site doping element of the cubic phase all-inorganic lead-based perovskite material is 0.72:0.28, it is shown that the cubic phase all-inorganic lead-based perovskite material can exhibit excellent performance.
[0040] Based on this, an embodiment of the present application also provides a method for preparing the aforementioned cubic phase all-inorganic lead-based perovskite material, including: taking the raw material CsPbBr3 and the raw material CsCdBr3, and grinding them into powder respectively; mixing the powdered raw material CsPbBr3 and the raw material CsCdBr3 evenly to obtain a mixed raw material; placing the mixed raw material at 600-700°C for heat preservation treatment; then cooling the mixed raw material to room temperature to obtain a raw material powder of a single crystal alloy; placing the single crystal alloy raw material powder in a heating furnace for single crystal growth to obtain a cubic phase all-inorganic lead-based perovskite material.
[0041] In the embodiment of the present application, the heating furnace is a type of equipment suitable for growing single crystal materials by the melt method. As long as the functions are met, a more representative equipment is the Bridgman furnace.
[0042] In the embodiments of the present application, the mixing ratio of the raw material CsPbBr3 and the raw material CsCdBr3 determines the chemical formula of the final product. In some embodiments, the molar ratio of the raw material CsPbBr3 and the raw material CsCdBr3 is 0.7-0.76:0.24-0.3. In some preferred embodiments, the molar ratio of the raw material CsPbBr3 and the raw material CsCdBr3 is 0.72:0.28, thereby obtaining a preferred cubic phase all-inorganic lead-based perovskite material, whose chemical formula is CsPb 0.72 Cd 0.28 Br3.
[0043] In some embodiments, the mixed raw material is heat-treated at 600-700° C. for more than 12 hours.
[0044] In some preferred embodiments, the heating furnace is a Bridgman furnace, which is a five-temperature-zone device, namely SV1 to SV5 from top to bottom, and each temperature zone is set at a different temperature. To ensure that the raw material powder of the single crystal alloy is recrystallized (grown in the form of a single crystal) after melting, the temperatures of the five temperature zones SV1 to SV5 are set to a gradient from high temperature to low temperature according to the running trajectory of the raw material powder of the single crystal alloy in the Bridgman furnace. Specifically, if the raw powder of the single crystal alloy is pulled along the direction of the SV1 to SV5 temperature zones, the insulation temperatures of the upper SV1 and SV2 temperature zones are set to 540°C, the insulation temperature of the middle SV3 temperature zone is 580°C, the temperature of the lower SV4 temperature zone is set to 410°C, and the temperature of the lower SV4 temperature zone is set to 450°C. Here, the insulation temperature of the middle SV3 temperature zone is set to 580°C, which is higher than the temperature of the upper SV1 and SV2 temperature zones. It mainly serves to balance the excessive temperature difference between the upper and lower temperature zones to maintain the stability of crystallization. The insulation temperature of the lowest SV5 temperature zone is higher than that of the SV4 temperature zone. This is because the lowest temperature zone is in contact with the external air and heat loss will occur.
[0045] In the embodiment of the present application, the five temperature zones of the Bridgman furnace are set through a program and go through six stages of "start-first insulation-heating (or cooling)-second insulation-cooling-end". Each stage has a corresponding temperature and retention time set in each temperature zone. At the same time, the raw material powder of the single crystal alloy is sealed and placed in the upper middle part of the furnace. When each temperature zone reaches the second insulation temperature at the same time, it is slowly pulled downward over time.
[0046] Based on this, the embodiments of the present application provide the application of the aforementioned cubic phase all-inorganic lead-based perovskite material and / or the aforementioned preparation method in the preparation of energy spectrum CT and area array imaging detectors.
[0047] The technical solution of the present application and the technical effects achieved are described in detail below through more specific embodiments.
[0048] Example 1
[0049] The present embodiment provides a preparation method of a cubic phase all-inorganic lead-based perovskite material, and the specific method includes: taking a first preparation raw material CsPbBr3 and a second preparation raw material CsCdBr3 containing an A-site element, a B-site element and an X-site element, grinding them into powder; adding the first preparation raw material CsPbBr3 and the second preparation raw material CsCdBr3 to a clean and pollution-free quartz crucible at a molar ratio of 0.72:0.28, and mixing them thoroughly to obtain a mixed raw material; sealing the quartz crucible containing the mixed raw material with a tube sealing machine, and then placing it in a rocking furnace for insulation treatment, wherein the insulation temperature is 600°C and the insulation time is 12 hours; then cooling to room temperature to obtain a single crystal alloy raw material powder; placing the quartz crucible containing the single crystal alloy raw material powder in a Bridgman furnace, and setting the temperature program of the five Bridgman temperature zones as follows:
[0050] SV1: Start; heat up to 520℃ for 4h and then keep warm, the first heat preservation time is 14h; heat up to 540℃ for 3h and then keep warm for 800h; cool down to 120℃ for 4h; cool down to 40℃ for 72h and then end;
[0051] SV2: Start; when the temperature rises to 520℃ for 4h, the first heat preservation is carried out, and the heat preservation time is 14h; when the temperature rises to 540℃ for 3h, the second heat preservation is carried out, and the heat preservation time is 800h; when the temperature falls to 120℃ for 4h; when the temperature falls to 40℃, the temperature is kept for 72 hours and the end is completed;
[0052] SV3: Start; heat up to 530℃ for 4h and then keep warm for 14h; heat up to 580℃ for 3h and then keep warm for 800h; cool down to 120℃ for 4h; cool down to 40℃ and keep warm for 72h;
[0053] SV4: Start; heat up to 650℃ for 4h and keep warm for 14h; cool down to 410℃ for 3h and keep warm for 800h; cool down to 120℃ for 4h; cool down to 40℃ and keep warm for 72h;
[0054] SV5: Start; heat up to 650℃ for 4h and keep warm for 14h; cool down to 450℃ for 3h and keep warm for 800h; cool down to 120℃ for 4h; cool down to 40℃ and keep warm for 72h;
[0055] When all five temperature zones are in the second holding temperature stage, the pulling speed of the crucible in the Bridgman furnace is controlled to be 0.3 mm / h, and finally a cubic all-inorganic lead-based perovskite material CsPb is obtained. 0.72 Cd 0.28 Br3.
[0056] The cubic all-inorganic lead-based perovskite material CsPb prepared in Example 1 0.72 Cd 0.28 Br3 performance verification mainly includes binary phase diagram analysis, XRD detection analysis, size measurement, attenuation performance analysis, IV test, It test, etc.
[0057] Figure 1 The cubic all-inorganic lead-based perovskite material CsPb finally prepared in Example 1 0.72 Cd 0.28 Br3 crystal sample picture. 0.72 Cd 0.28 Br3 was analyzed by differential scanning calorimetry to determine the melting point of the material, and finally the cubic phase of the all-inorganic lead-based titanium ore material CsPb was obtained. 0.72 Cd 0.28 Binary phase diagram of Br3.
[0058] Differential scanning calorimetry refers to the measurement of the relationship between the power difference (such as in the form of heat) input to the sample and the reference (doped with Cd in different proportions) and the temperature under program-controlled temperature. The curve recorded by the differential scanning calorimeter is called the DSC curve. It uses the rate at which the sample absorbs or releases heat, that is, the heat flow rate dH / dt (unit: millijoules / second) as the vertical coordinate, and the temperature T or time t as the horizontal coordinate. It can measure a variety of thermodynamic and kinetic parameters, such as specific heat capacity, reaction heat, transition heat, phase diagram, reaction rate, crystallization rate, polymer crystallinity, sample purity, etc. In the embodiment of the present application, crucibles containing alloy powders with different component contents and a blank control crucible are prepared. This method is used to observe the thermal response of the sample and the control crucible, record the melting point, and obtain the binary phase diagram of the alloy, such as Figure 2 shown.
[0059] from Figure 2 It can be seen that when different contents of Cd element are doped at the B position of the lead-based perovskite CsPbBr3 material, the obtained alloy material exhibits different types of space group states. Only when the doping content of the Cd element at the B position is in the range of 18% to 28%, can the obtained alloy material be in a 221 space group solid solution at room temperature (0 to 30°C), which is suitable as an optoelectronic material for the preparation of products such as energy spectrum CT and area array imaging detectors.
[0060] The cubic all-inorganic lead-based perovskite material CsPb prepared in Example 1 0.72 Cd 0.28 Br3 was analyzed using XRD diffractometer (Shimadzu XRD-6100).
[0061] Figure 3 CsPb 0.72 Cd 0.28XRD test results of Br3 alloy crystal from top to bottom. Figure 4 The standard XRD cards corresponding to the three crystal space groups of 221, 194 and 62 are compared. Figure 3 and Figure 4 , it can be concluded that CsPb 0.72 Cd 0.28 The XRD results of the Br3 alloy material and the 221 phase are basically consistent (the shape and angle are highly consistent), indicating that the CsPb prepared in the embodiment of the present application 0.72 Cd 0.28 The Br3 alloy material exhibits a 221 cubic phase.
[0062] Example 1 prepared by Bridgman furnace CsPb 0.72 Cd 0.28 The size of the Br3 alloy was measured to be up to 12 cm in diameter and 10 cm in length.
[0063] For CsPb prepared by Bridgman furnace in Example 1 0.72 Cd 0.28 The attenuation performance of the Br3 alloy material was tested, and the specific steps were as follows: the grown Bridgman crystal was cut and polished to obtain an alloy wafer with a diameter of 12 mm and a thickness of 2 to 3 mm; electrodes were evaporated on the polished wafer using a thermal evaporation process to evaporate Au electrodes on one side and Bi electrodes on the other side to complete the preparation of the device; the prepared device was connected to an electrometer test bench to collect electrical signals in real time, where counts represents the relative size of the electrical signal. After the signal is stable in the dark state (without lighting), the light source is quickly switched on and off to obtain the attenuation curve of the device.
[0064] Figure 5 CsPb 0.72 Cd 0.28 The attenuation performance test results of the Br3 alloy material show that the signal is very small when there is no light, and the light signal increases rapidly when the light is turned on, and the response speed is extremely fast. After the light source is turned off, the signal slowly decays to the dark state value, indicating that the cubic phase all-inorganic lead-based perovskite CsPb prepared in the embodiment of the present application 0.72 Cd 0.28 Br3 alloy material has long attenuation life and fast response.
[0065] The CsPb prepared in Example 1 0.72 Cd 0.28The Br3 alloy material was subjected to IV testing, and the specific steps were as follows: the grown Bridgman crystal was cut and polished to obtain alloy wafers with a diameter of 12 mm and a thickness of 2 to 3 mm; electrodes were evaporated on the polished wafers using a thermal evaporation process to evaporate Au electrodes on one side and Bi electrodes on the other side to complete the preparation of the device; the device was connected to an electrometer test bench, voltage was applied to the device, the current value was collected, the IV curve was obtained, and the resistivity was calculated.
[0066] Figure 6 This is the IV test result. It can be seen from the figure that the resistivity of the alloy material can be as high as 3.3×10 9 Ω*cm, showing excellent electrical properties.
[0067] The CsPb prepared in Example 1 0.72 Cd 0.28 The Br3 alloy material was tested for IT, and the specific steps were as follows: the grown Bridgman crystal was cut and polished to obtain alloy wafers with a diameter of 12 mm and a thickness of 2 to 3 mm; the polished wafers were evaporated with electrodes, using a thermal evaporation process to evaporate Au electrodes on one side and Bi electrodes on the other side to complete the preparation of the device; the device was connected to the electrometer test bench, and the light was turned on and off repeatedly, and the electrical signal was collected to obtain the curve of the change of the current over time, and the stability of the optical signal, the size of the optical signal, and the light-dark ratio (the ratio of the electrical signal in the light state to the electrical signal in the dark state) were observed.
[0068] Figure 7 This is the It test result. It can be seen from the figure that the alloy material has a large light response and good stability.
[0069] In summary, the new material CsPb provided in this application 0.72 Cd 0.28 Br3 belongs to the cubic phase all-inorganic lead-based perovskite, and its structure is pure 221. The cubic phase has more obvious advantages, which are manifested in: high symmetry. The cubic symmetry enables the cubic phase to play an important role in crystallography and is widely used in the preparation and application of materials; simple structure. The structure of the cubic phase is simple and clear, with a high degree of regularity, which is suitable for the preparation of high-quality single crystals, and its research in crystallographic theory is relatively easy; strong stability. The physical properties of the cubic phase are stable, and it is more stable under high temperature and high pressure conditions.
[0070] The present application is described in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the present application and its core ideas. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.
Claims
1. A cubic all-inorganic lead-based perovskite material, characterized in that: The B position of the lead-based perovskite material CsPbBr3 is doped with Cd, and its chemical formula is CsPb m Cd 1-m Br3, wherein 0.7<m<0.
82.
2. The cubic all-inorganic lead-based perovskite material according to claim 1, characterized in that: Its chemical formula is CsPb m Cd 1-m Br3, where 0.72≤m≤0.
76.
3. The cubic all-inorganic lead-based perovskite material according to claim 1, characterized in that: Its chemical formula is CsPb 0.72 Cd 0.28 Br3.
4. A method for preparing a cubic all-inorganic lead-based perovskite material, characterized in that: include: Take the raw material CsPbBr3 and the raw material CsCdBr3, grind them into powder respectively; The powdered raw material CsPbBr3 and the raw material CsCdBr3 are uniformly mixed to obtain a mixed raw material; The mixed raw materials are placed at 600-700°C for heat preservation; The mixed raw materials are then cooled to room temperature to obtain raw material powder of single crystal alloy; the single crystal alloy raw material powder is placed in a heating furnace for single crystal growth to obtain a cubic phase all-inorganic lead-based perovskite material.
5. The preparation method according to claim 4, characterized in that: The molar mixing ratio of the raw material CsPbBr3 and the raw material CsCdBr3 is 0.7-0.82:0.18-0.
3.
6. The preparation method according to claim 5, characterized in that: The molar mixing ratio of the raw material CsPbBr3 and the raw material CsCdBr3 is 0.72:0.
28.
7. The preparation method according to claim 4, characterized in that: The mixed raw materials are heat-treated at 600-700°C for more than 12 hours.
8. The preparation method according to claim 4, characterized in that: The heating furnace is a Bridgman furnace, which is provided with five temperature zones SV1 to SV5 arranged in sequence, wherein the set temperatures of the five temperature zones are: SV1: 540°C, SV2: 540°C, SV3: 580°C, SV4: 410°C, SV5: 450°C; the alloy raw material powder is pulled in the Bridgman furnace along the direction of the SV1 to SV5 temperature zones.
9. The preparation method according to claim 8, characterized in that: The alloy raw material powder is pulled in the Bridgman furnace along the direction of the SV1 to SV5 temperature zones at a speed of 0.3 mm / h.
10. Use of the cubic all-inorganic lead-based perovskite material according to any one of claims 1 to 3 and / or the preparation method according to any one of claims 4 to 9 in the preparation of energy spectrum CT and area array imaging detectors.