Fabric flame-retardant anti-ultraviolet organic silicon finishing agent and preparation method thereof
By preparing a combination of flame-retardant modified silicone oil, UV absorber, and surfactant, the problem of fabric finishing agents being unable to simultaneously impart flame retardancy and UV resistance was solved, thus achieving a multi-functional performance improvement for fabrics.
Patent Information
- Application Number
- CN202411038519.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing fabric finishing agents cannot simultaneously impart flame retardant and UV-resistant properties to fabrics, and the application scope of silicone finishing agents is limited.
A flame-retardant and UV-resistant silicone finishing agent for fabrics was prepared by combining flame-retardant modified silicone oil with UV absorbers and cationic-nonionic surfactants through a specific chemical reaction. DOPO was used as the flame-retardant structural unit, chitosan-titanium dioxide was used as the UV absorber, and a stable silicone finishing agent system was formed through polyurethane.
It improves the flame retardant and UV resistance properties of fabrics, and the finishing agent has good durability and certain antibacterial properties.
Smart Images

Figure BDA0004971761100000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of fabric treatment, in particular to a flame retardant and anti-ultraviolet organosilicon finishing agent for fabric and a preparation method thereof. Background Art
[0002] With the progress of society and the improvement of living standards, people's requirements for textiles for clothing are getting higher and higher. Finishing textiles with textile auxiliaries can effectively improve the performance of fabrics in various aspects. At present, the finishing of such fabrics is mostly to improve the hydrophilicity and softness of the fabrics. However, other special properties such as flame retardancy or UV resistance are not given to the fabrics. At present, the finishing agents mainly include polyether finishing agents, silicone finishing agents, etc. Among them, silicone finishing agents can well improve the softness and feel of fabrics because they are widely used. In order to further broaden the scope of application of silicone finishing agents, this application aims to prepare finishing agents with flame retardancy and UV resistance. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present invention designs an organic silicone oil modified by a flame retardant group, and combines an ultraviolet absorber and a surfactant to prepare an organic silicone finishing agent with flame retardancy and UV resistance.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] A flame retardant and anti-ultraviolet organosilicon finishing agent for fabrics, comprising the following components: 70 to 85 parts of flame retardant modified organosilicon oil, 5 to 15 parts of ultraviolet absorber and 15 to 30 parts of cationic-nonionic surfactant;
[0006] The preparation process of the flame retardant modified silicone oil is as follows:
[0007] S1-1, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and formaldehyde are refluxed at 90-140° C. to prepare DOPO-OH;
[0008] S1-2, dissolving ethyl dichlorophosphate in DMF and placing in an ice-water bath under nitrogen protection, adding triethylamine and stirring evenly, then slowly dropping DOPO-OH solvent in DMF into the reaction system, and continuing to stir for 2-4 hours after the addition is completed;
[0009] S1-3, dissolving the side chain hydroxy silicone oil in DMF, and slowly adding it dropwise to the reaction system in step 2), and continuing stirring for 2-4 hours after the addition is completed; and removing the low-boiling substances by distillation under reduced pressure to obtain the product;
[0010] The ultraviolet absorber is modified chitosan-titanium dioxide, and the preparation process is as follows:
[0011] S2-1, dissolving chitosan in a 1 wt % acetic acid solution and stirring to form a colloidal solution, adding a certain amount of titanium dioxide powder and stirring to disperse uniformly to obtain a mixed reaction system;
[0012] S2-2. Add ammonium persulfate initiator to the mixed reaction system, dissolve the reactive benzotriazole derivative in THF and then add it dropwise to the mixed reaction system, raise the temperature to 70-80°C, and stir the reaction for 3 hours; after cooling, adjust the pH to neutral, evaporate the mixed system to remove part of the solvent, dehydrate it in methanol, filter it, dry it, and grind it to obtain.
[0013] Furthermore, the preparation process of the cationic-nonionic surfactant is as follows:
[0014] A polyurethane prepolymer is prepared using polyoxypropylene glycol (PPG) and isophorone diisocyanate (IPDI) as starting materials, organic tin as a catalyst, and N-methyldiethanolamine (MDEA) as a chain extender; the polyurethane prepolymer is then capped with polyethylene glycol (PEG), the temperature is raised to 110° C., γ-chloropropylmethyldimethoxysilane is added dropwise, and after cooling, water is added to emulsify the mixture to a solid content of 30-40%.
[0015] Furthermore, the molecular weight of the polyoxypropylene glycol is 1000-2000; the molecular weight of the polyethylene glycol is 400-600.
[0016] Furthermore, the mass ratio of polyoxypropylene glycol, isophorone diisocyanate, organic tin catalyst, N-methyldiethanolamine and polyethylene glycol is 15-25:10-15:0.01-0.02:3-10:1-2.
[0017] Furthermore, the mass ratio of the titanium dioxide powder to chitosan is 0.5 to 2:1.
[0018] Furthermore, the mass ratio of the reactive benzotriazole derivative to chitosan is 4 to 8:1.
[0019] The second object of the present invention is to provide a method for preparing the flame retardant and anti-ultraviolet silicone finishing agent for fabrics as described above, comprising the following steps:
[0020] Ultrasonic dispersion of measured ultraviolet absorber in deionized water, then slowly adding it into cationic-nonionic surfactant during stirring, forming a stable dispersion, and evenly mixing it with flame retardant modified silicone oil, adjusting the solid content between 30-40%, thus obtaining the product.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention uses 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) flame retardant monomer as a flame retardant structural unit and grafts it with side chain hydroxy silicone oil through chlorine substitution reaction to obtain modified silicone oil. Due to the presence of the flame retardant structural unit, the modified silicone oil has good flame retardancy.
[0023] 2. The present application adopts a new type of reactive benzotriazole ultraviolet absorber developed by Nornameo, which has strong absorption of ultraviolet rays with a wavelength between 300-385nm, high absorption efficiency and good stability. At the same time, it can undergo free radical polymerization due to its methacrylate structure. The present application utilizes this monomer to carry out a grafting reaction on the surface of chitosan. When titanium dioxide is dispersed in a chitosan colloidal solution, a reactive benzotriazole derivative undergoes a grafting polymerization reaction on the surface of chitosan to wrap the titanium dioxide therein, so that the finally obtained ultraviolet absorber has a good and stable absorption effect over a wide range, and can also give the fabric a certain antibacterial property.
[0024] 3. With polyurethane as the main chain unit, the cationic structural unit is introduced through N-methyldiethanolamine, and then a cation containing a siloxane structure is formed with γ-chloropropylmethyldimethoxysilane. The obtained surfactant can assist in the dispersion of the ultraviolet absorber. At the same time, due to the interaction between the siloxane structure and the silicone oil, the three work together to form a stable silicone finishing agent. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0027] Example 1: A flame retardant and UV-resistant silicone finishing agent for fabrics,
[0028] The invention comprises the following components: 70 parts of flame retardant modified silicone oil, 5 parts of ultraviolet absorber and 15 parts of cationic-nonionic surfactant;
[0029] The preparation process of the flame retardant modified silicone oil is as follows:
[0030] S1-1, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and formaldehyde were refluxed at 90-140°C to prepare DOPO-OH
[0031] S1-2, dissolve ethyl dichlorophosphate in DMF and place in an ice-water bath under nitrogen protection, add triethylamine and stir evenly, then slowly drop DOPO-OH solvent in DMF into the reaction system, continue stirring for 2-4 hours after the dropwise addition is completed, and obtain the intermediate product
[0032] S1-3, dissolve the side chain hydroxy silicone oil (viscosity 1000) in DMF, and slowly add it dropwise to the reaction system in step 2), and continue stirring for 2-4h after the addition is completed; remove the low boiling point by distillation under reduced pressure to obtain R is silicone oil.
[0033] The ultraviolet absorber is modified chitosan-titanium dioxide, and the preparation process is as follows:
[0034] S2-1, dissolving 1 part of chitosan in 1 wt% acetic acid solution and stirring to form a colloidal solution, adding 1 part of titanium dioxide powder and stirring to disperse uniformly to obtain a mixed reaction system;
[0035] S2-2, add ammonium persulfate initiator to the mixed reaction system, and mix 4 parts of reactive benzotriazole derivatives Dissolve in THF and then add dropwise into the mixed reaction system, heat to 70-80°C, and stir to react for 3 hours; after cooling, adjust the pH to neutral, evaporate the mixed system to remove part of the solvent, dehydrate in methanol, filter, dry, and grind to obtain.
[0036] The preparation process of the cationic-nonionic surfactant is as follows:
[0037] Place 15 parts of PPG-1000 in a reaction bottle for vacuum dehydration, then add 10 parts of IPDI and 0.01 parts of organic tin catalyst at room temperature, introduce nitrogen protection, heat to 80°C, and react with stirring for 3 hours; cool to below 50°C, add 5 parts of MDEA and acetone, heat to 80°C, and react with stirring for 1 hour; cool to below 50°C, add PEG-500, heat to 70°C, and react with stirring for 3 hours; heat to 110°C, add dropwise 7.5 parts of γ-chloropropylmethyldimethoxysilane, and react with stirring for 3 hours; when cooled to below 50°C, add excess glacial acetic acid for neutralization, and after cooling, add water to emulsify to a solid content of 30%.
[0038] Ultrasonic dispersion of measured ultraviolet absorber in deionized water, then slowly adding it into cationic-nonionic surfactant during stirring, forming a stable dispersion, and then mixing it evenly with flame retardant modified silicone oil, adjusting the solid content to 30%, to obtain the product.
[0039] Example 2: A flame retardant and UV-resistant silicone finishing agent for fabrics,
[0040] The invention comprises the following components: 80 parts of flame retardant modified silicone oil, 10 parts of ultraviolet absorber and 22 parts of cationic-nonionic surfactant;
[0041] The preparation process of the flame retardant modified silicone oil is as follows:
[0042] S1-1, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and formaldehyde are refluxed at 90-140° C. to prepare DOPO-OH;
[0043] S1-2, dissolving ethyl dichlorophosphate in DMF and placing in an ice-water bath under nitrogen protection, adding triethylamine and stirring evenly, then slowly dropping DOPO-OH solvent in DMF into the reaction system, and continuing to stir for 2-4 hours after the addition is completed to obtain an intermediate product;
[0044] S1-3, dissolving the side chain hydroxy silicone oil (viscosity 1000) in DMF, and slowly dropping it into the reaction system of step 2), and continuing stirring for 2-4 hours after the dropping is completed; and removing the low boiling point by distillation under reduced pressure to obtain the product.
[0045] The ultraviolet absorber is modified chitosan-titanium dioxide, and the preparation process is as follows:
[0046] S2-1, dissolving 1 part of chitosan in 1 wt% acetic acid solution and stirring to form a colloidal solution, adding 1.5 parts of titanium dioxide powder and stirring to disperse uniformly to obtain a mixed reaction system;
[0047] S2-2. Add ammonium persulfate initiator to the mixed reaction system, dissolve 5 parts of reactive benzotriazole derivatives in THF and then add dropwise to the mixed reaction system, raise the temperature to 70-80°C, and stir to react for 3 hours; after cooling, adjust the pH to neutral, evaporate the mixed system to remove part of the solvent, dehydrate it in methanol, filter it, dry it, and grind it to obtain.
[0048] The preparation process of the cationic-nonionic surfactant is as follows:
[0049] Place 15 parts of PPG-1000 in a reaction bottle for vacuum dehydration, then add 10 parts of IPDI and 0.01 parts of organic tin catalyst at room temperature, introduce nitrogen protection, heat to 80°C, and react with stirring for 3 hours; cool to below 50°C, add 5 parts of MDEA and acetone, heat to 80°C, and react with stirring for 1 hour; cool to below 50°C, add PEG-500, heat to 70°C, and react with stirring for 3 hours; heat to 110°C, add dropwise 7.5 parts of γ-chloropropylmethyldimethoxysilane, and react with stirring for 3 hours; when cooled to below 50°C, add excess glacial acetic acid for neutralization, and after cooling, add water to emulsify to a solid content of 30%.
[0050] Ultrasonic dispersion of measured ultraviolet absorber in deionized water, then slowly adding it into cationic-nonionic surfactant during stirring, forming a stable dispersion, and then mixing it evenly with flame retardant modified silicone oil, adjusting the solid content to 30%, to obtain the product.
[0051] Embodiment 3: A flame retardant and UV-resistant silicone finishing agent for fabrics,
[0052] The invention comprises the following components: 85 parts of flame retardant modified silicone oil, 15 parts of ultraviolet absorber and 30 parts of cationic-nonionic surfactant;
[0053] The preparation process of the flame retardant modified silicone oil is as follows:
[0054] S1-1, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and formaldehyde are refluxed at 90-140° C. to prepare DOPO-OH;
[0055] S1-2, dissolving ethyl dichlorophosphate in DMF and placing in an ice-water bath under nitrogen protection, adding triethylamine and stirring evenly, then slowly dropping DOPO-OH solvent in DMF into the reaction system, and continuing to stir for 2-4 hours after the addition is completed to obtain an intermediate product;
[0056] S1-3, dissolving the side chain hydroxy silicone oil (viscosity 1000) in DMF, and slowly dropping it into the reaction system of step 2), and continuing stirring for 2-4 hours after the dropping is completed; and removing the low boiling point by distillation under reduced pressure to obtain the product.
[0057] The ultraviolet absorber is modified chitosan-titanium dioxide, and the preparation process is as follows:
[0058] S2-1, dissolving 1 part of chitosan in 1 wt% acetic acid solution and stirring to form a colloidal solution, adding 2 parts of titanium dioxide powder and stirring to disperse uniformly to obtain a mixed reaction system;
[0059] S2-2. Add ammonium persulfate initiator to the mixed reaction system, dissolve 6 parts of reactive benzotriazole derivatives in THF and then add dropwise to the mixed reaction system, raise the temperature to 70-80°C, and stir to react for 3 hours; after cooling, adjust the pH to neutral, evaporate the mixed system to remove part of the solvent, dehydrate it in methanol, filter it, dry it, and grind it to obtain.
[0060] The preparation process of the cationic-nonionic surfactant is as follows:
[0061] Place 15 parts of PPG-1000 in a reaction bottle for vacuum dehydration, then add 10 parts of IPDI and 0.01 parts of organic tin catalyst at room temperature, introduce nitrogen protection, heat to 80°C, and react with stirring for 3 hours; cool to below 50°C, add 5 parts of MDEA and acetone, heat to 80°C, and react with stirring for 1 hour; cool to below 50°C, add PEG-500, heat to 70°C, and react with stirring for 3 hours; heat to 110°C, add dropwise 7.5 parts of γ-chloropropylmethyldimethoxysilane, and react with stirring for 3 hours; when cooled to below 50°C, add excess glacial acetic acid for neutralization, and after cooling, add water to emulsify to a solid content of 30%.
[0062] Ultrasonic dispersion of measured ultraviolet absorber in deionized water, then slowly adding it into cationic-nonionic surfactant during stirring, forming a stable dispersion, and then mixing it evenly with flame retardant modified silicone oil, adjusting the solid content to 30%, to obtain the product.
[0063] Comparative Example 1:
[0064] The composition includes the following components: 85 parts of flame retardant modified silicone oil and 15 parts of ultraviolet absorber;
[0065] The preparation process of the flame retardant modified silicone oil is as follows:
[0066] S1-1, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and formaldehyde are refluxed at 90-140° C. to prepare DOPO-OH;
[0067] S1-2, dissolving ethyl dichlorophosphate in DMF and placing in an ice-water bath under nitrogen protection, adding triethylamine and stirring evenly, then slowly dropping DOPO-OH solvent in DMF into the reaction system, and continuing to stir for 2-4 hours after the addition is completed to obtain an intermediate product;
[0068] S1-3, dissolving the side chain hydroxy silicone oil (viscosity 1000) in DMF, and slowly dropping it into the reaction system of step 2), and continuing stirring for 2-4 hours after the dropping is completed; and removing the low boiling point by distillation under reduced pressure to obtain the product.
[0069] The ultraviolet absorber is modified chitosan-titanium dioxide, and the preparation process is as follows:
[0070] S2-1, dissolving 1 part of chitosan in 1 wt% acetic acid solution and stirring to form a colloidal solution, adding 2 parts of titanium dioxide powder and stirring to disperse uniformly to obtain a mixed reaction system;
[0071] S2-2. Add ammonium persulfate initiator to the mixed reaction system, dissolve 6 parts of reactive benzotriazole derivatives in THF and then add dropwise to the mixed reaction system, raise the temperature to 70-80°C, and stir to react for 3 hours; after cooling, adjust the pH to neutral, evaporate the mixed system to remove part of the solvent, dehydrate it in methanol, filter it, dry it, and grind it to obtain.
[0072] The measured ultraviolet absorber is ultrasonically dispersed in deionized water, and then evenly mixed with the flame retardant modified organic silicone oil, and the solid content is adjusted to 30% to obtain the product.
[0073] Comparative Example 2:
[0074] The invention comprises the following components: 85 parts of flame retardant modified silicone oil, 15 parts of ultraviolet absorber and 30 parts of cationic-nonionic surfactant;
[0075] The preparation process of the flame retardant modified silicone oil is as follows:
[0076] S1-1, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and formaldehyde are refluxed at 90-140° C. to prepare DOPO-OH;
[0077] S1-2, dissolving ethyl dichlorophosphate in DMF and placing in an ice-water bath under nitrogen protection, adding triethylamine and stirring evenly, then slowly dropping DOPO-OH solvent in DMF into the reaction system, and continuing to stir for 2-4 hours after the addition is completed to obtain an intermediate product;
[0078] S1-3, dissolving the side chain hydroxy silicone oil (viscosity 1000) in DMF, and slowly dropping it into the reaction system of step 2), and continuing stirring for 2-4 hours after the dropping is completed; and removing the low boiling point by distillation under reduced pressure to obtain the product.
[0079] The ultraviolet absorber is chitosan-titanium dioxide, and the preparation process is as follows:
[0080] S2-1, dissolving 1 part of chitosan in 1 wt% acetic acid solution and stirring to form a colloidal solution, adding 2 parts of titanium dioxide powder and stirring to disperse evenly, and degassing and solidifying the mixed solution to obtain a UV absorber;
[0081] The preparation process of the cationic-nonionic surfactant is as follows:
[0082] Place 15 parts of PPG-1000 in a reaction bottle for vacuum dehydration, then add 10 parts of IPDI and 0.01 parts of organic tin catalyst at room temperature, introduce nitrogen protection, heat to 80°C, and react with stirring for 3 hours; cool to below 50°C, add 5 parts of MDEA and acetone, heat to 80°C, and react with stirring for 1 hour; cool to below 50°C, add PEG-500, heat to 70°C, and react with stirring for 3 hours; heat to 110°C, add dropwise 7.5 parts of γ-chloropropylmethyldimethoxysilane, and react with stirring for 3 hours; when cooled to below 50°C, add excess glacial acetic acid for neutralization, and after cooling, add water to emulsify to a solid content of 30%.
[0083] Ultrasonic dispersion of measured ultraviolet absorber in deionized water, then slowly adding it into cationic-nonionic surfactant during stirring, forming a stable dispersion, and then mixing it evenly with flame retardant modified silicone oil, adjusting the solid content to 30%, to obtain the product.
[0084] Finishing process:
[0085] Cotton fabric → impregnation (two impregnations and two impregnations, the residual rate is 80%) → pre-baking (90°C, 60s) → baking (140-170°C, 60-180s).
[0086] Refer to GB / T18830-2002 to test the anti-ultraviolet performance of the finished fabric;
[0087] The flame retardant properties of the finished cotton fabrics were tested according to GB / T 5455-2014; the results are recorded in Table 1.
[0088] Table 1
[0089]
[0090] It can be seen from the above table that the present application prepares a flame retardant and UV-proof finishing agent by the mutual coordination of three flame retardant modified silicone oils, UV absorbers and surfactants. The flame retardant and UV-proof properties of the finished fabric are improved, and the durability is good.
[0091] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A flame retardant and anti-ultraviolet silicone finishing agent for fabrics, characterized in that: The invention comprises the following components: 70 to 85 parts of flame retardant modified organic silicone oil, 5 to 15 parts of ultraviolet absorber and 15 to 30 parts of cationic-nonionic surfactant; The preparation process of the flame retardant modified silicone oil is as follows: S1-1, DOPO-OH is prepared by reflux reaction of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and formaldehyde at 90-140°C; S1-2, dissolving ethyl dichlorophosphate in DMF and placing in an ice-water bath under nitrogen protection, adding triethylamine and stirring evenly, then slowly dropping DOPO-OH solvent in DMF into the reaction system, and continuing to stir for 2-4 hours after the addition is completed; S1-3, dissolving the side chain hydroxy silicone oil in DMF, and slowly adding it dropwise to the reaction system in step 2), and continuing stirring for 2-4 hours after the addition is completed; and removing the low-boiling substances by distillation under reduced pressure to obtain the product; The ultraviolet absorber is modified chitosan-titanium dioxide, and the preparation process is as follows: S2-1, dissolving chitosan in a 1 wt% acetic acid solution and stirring to form a colloidal solution, adding a certain amount of titanium dioxide powder and stirring to disperse uniformly to obtain a mixed reaction system; S2-2. Add ammonium persulfate initiator to the mixed reaction system, dissolve the reactive benzotriazole derivative in THF and then add it dropwise to the mixed reaction system, raise the temperature to 70-80°C, and stir the reaction for 3 hours; after cooling, adjust the pH to neutral, evaporate the mixed system to remove part of the solvent, dehydrate it in methanol, filter it, dry it, and grind it to obtain.
2. The flame retardant and anti-ultraviolet silicone finishing agent for fabrics according to claim 1, characterized in that: The preparation process of the cationic-nonionic surfactant is as follows: The polyurethane prepolymer is prepared with polyoxypropylene glycol and isophorone diisocyanate as starting materials, organic tin as catalyst and N-methyldiethanolamine as chain extender; the polyurethane prepolymer is then capped with polyethylene glycol, the temperature is raised to 110°C, γ-chloropropylmethyldimethoxysilane is added dropwise, and after cooling, water is added to emulsify the mixture to a solid content of 30-40%.
3. The flame retardant and anti-ultraviolet silicone finishing agent for fabrics according to claim 2, characterized in that: The molecular weight of the polyoxypropylene glycol is 1000-2000; the molecular weight of the polyethylene glycol is 400-600.
4. The flame retardant and anti-ultraviolet silicone finishing agent for fabrics according to claim 2, characterized in that: The mass ratio of polyoxypropylene glycol, isophorone diisocyanate, organic tin catalyst, N-methyldiethanolamine and polyethylene glycol is 15-25:10-15:0.01-0.02:3-10:1-2.
5. The flame retardant and anti-ultraviolet silicone finishing agent for fabrics according to claim 1, characterized in that: The mass ratio of the titanium dioxide powder to chitosan is 0.5-2:
1.
6. The flame retardant and anti-ultraviolet silicone finishing agent for fabrics according to claim 1, characterized in that: The mass ratio of the reactive benzotriazole derivative to chitosan is 4-8:
1.
7. A method for preparing the flame retardant and anti-ultraviolet silicone finishing agent for fabrics as claimed in any one of claims 1 to 6, characterized in that: The steps include: Ultrasonic dispersion of measured ultraviolet absorber in deionized water, then slowly adding it into cationic-nonionic surfactant during stirring, forming a stable dispersion, and evenly mixing it with flame retardant modified silicone oil, adjusting the solid content between 30-40%, thus obtaining the product.
Citation Information
Cited By
Antibacterial waterproof material as well as preparation method and application thereof
CN120776584A