Photosensitive resin composition, solder resist dry film, photosensitive laminate, solder resist pattern, and semiconductor package substrate

By introducing epoxy-based glass polymer prepolymer into the photosensitive resin composition, and using dynamic covalent bond exchange reaction, the problems of thermal expansion coefficient and development performance of the photosensitive resin composition on the IC carrier plate are solved, and the problem of the photosensitive resin composition is realized Low thermal expansion coefficient and good development performance avoid cracking and warping, and meet the needs of refined and high-density of IC carrier plates.

CN119002179AActive Publication Date: 2024-11-22HANGZHOU FIRST ELECTRONIC MATERIAL CO LTD

Patent Information

Application Number
CN202411153979.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The prior art is difficult to take into account the heat resistance, thermal expansion coefficient and development performance of the photosensitive resin composition, resulting in cracking, warping and wrinkling problems on the IC carrier plate, and cannot meet the needs of fineness and high density.

Method used

Using a photosensitive resin composition containing alkali-soluble resin, photopolymerized monomer, epoxy resin, epoxy-based glass polymer prepolymer and curing agent, the thermal expansion coefficient is reduced through the exchange reaction of dynamic covalent bonds, and the thermal expansion coefficient is guaranteed. While heat resistance and development performance, cracking and warping are avoided.

Benefits of technology

The photosensitive resin composition is achieved with low thermal expansion coefficient and good development performance, avoiding cracking, warping and wrinkling, meeting the requirements of the IC carrier plate to refine and high density, while maintaining heat resistance and hardness performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005004403380000021
    Figure BDA0005004403380000021
  • Figure BDA0005004403380000061
    Figure BDA0005004403380000061
  • Figure BDA0005004403380000171
    Figure BDA0005004403380000171
Patent Text Reader

Abstract

The invention provides a photosensitive resin composition, a solder resist dry film, a photosensitive laminate, a solder resist pattern and a semiconductor package substrate, and relates to the technical field of high polymer materials. The photosensitive resin composition is prepared from the following components in parts by mass: 100 to 120 parts of alkali-soluble resin, 5 to 25 parts of photopolymerization monomer, 1 to 7 parts of photoinitiator, 10 to 30 parts of epoxy resin, 3 to 15 parts of epoxy group glass macromolecular prepolymer, and 1 to 5 parts of curing agent and accelerant thereof. By limiting the mass parts of the specific components, the thermal expansion coefficient can be reduced and the problems of cracking, warping, wrinkling and the like can be avoided while the heat resistance, the hardness, the scratch resistance, the acid and alkali resistance, the solvent resistance, the cold and hot impact resistance, the developing performance and the like of the photosensitive resin composition are ensured, so that the requirements of refinement and high density of the IC support plate are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a photosensitive resin composition, a solder resist dry film, a photosensitive laminate, a solder resist pattern and a semiconductor package carrier. Background Art

[0002] In printed circuit boards used in electronic devices, a solder mask is usually provided in areas other than connection holes on a substrate having a circuit pattern in order to prevent the conductors of the circuit from being exposed and corroded and solder from adhering to unnecessary locations and causing short circuits. Currently, photosensitive resin compositions are widely used as solder mask materials.

[0003] With the development of miniaturization of electronic products, related components are also tending to be miniaturized, precise, high-density and highly integrated, and semiconductor packaging (IC) substrates are gradually receiving widespread attention. Compared with traditional printed circuit boards (PCBs), IC substrates also have more stringent performance requirements for photosensitive resin compositions, including heat resistance, thermal expansion coefficient, hardness, scratch resistance, acid and alkali resistance, solvent resistance, and resistance to cold and hot shocks. Among them, good heat resistance, hardness, acid and alkali resistance, solvent resistance and other properties require the photosensitive resin composition to have a rigid structure, that is, the photosensitive resin composition has a high glass transition temperature (Tg), but it also leads to a high thermal expansion coefficient. If the thermal expansion coefficient is high, the photosensitive resin composition will shrink during the light and heat curing process and easily wrinkle and warp. In addition, since the subsequent processing adopts the chemical gold plating process, the photosensitive resin composition is also required to have excellent gold resistance (i.e., corrosion resistance at high temperatures) to avoid the loss of product appearance and performance due to bubbling, discoloration or shedding of the photosensitive resin composition. At the same time, the needs of refinement and high density also require the photosensitive resin composition to have good development performance.

[0004] At present, most of the methods improve heat resistance by grafting rigid segments onto the components of the photosensitive resin composition. For example, patent document CN116768728A discloses a method for preparing high-performance photosensitive solder resist ink by using a naphthalene-type chain-extended modified epoxy resin, wherein a small molecule naphthalene-type epoxy compound is chain-extended by a difunctional acid chain extender, and then the chain is sequentially reacted with an acrylic modifier and an unsaturated acid anhydride. Although the invention prepares a new type of photocurable solder resist ink having a high glass transition temperature, strong toughness, low dielectric constant, and resistance to DC voltage breakdown, the patent does not provide a specific thermal expansion coefficient, and according to the structure of the epoxy compound, it can be foreseen that the photosensitive resin composition has a relatively high thermal expansion coefficient and is not suitable for use in IC substrates. Alternatively, inorganic fillers are introduced into the photosensitive resin composition to reduce the thermal expansion coefficient. For example, patent document CN108350107B discloses a photocurable and heat-curable resin composition and a solder resist dry film. The thermal expansion coefficient is reduced by introducing a flaky inorganic filler with a modulus of 90 GPa to 120 GPa into the composition system. However, the requirements for the inorganic filler are high, and the whiteness needs to be limited to more than 90%. The particle size is close to the nanometer level, which increases the cost. The nanometer-level inorganic filler is difficult to disperse in the photosensitive resin system, and the system is prone to uneven dispersion and incompatibility. It will also affect the subsequent development performance. Some technologies help improve the dispersion effect by modifying the inorganic filler or adding a dispersant, but it will increase the cost. Alternatively, the thermal expansion coefficient is reduced by introducing a flexible segment on the alkali-soluble resin or the thermosetting resin in the photosensitive resin composition to improve the wrinkling and warping problems. For example, patent document CN115793389A discloses a solder resist dry film with a low thermal expansion coefficient and its application, which uses a high-elastic polymer to reduce the thermal expansion coefficient to improve cracking under high temperature stress. However, the patent has a low content of photosensitive acrylate and a high content of thermosetting epoxy resin. Although it can reduce the thermal expansion coefficient while ensuring heat resistance, it will lead to a decrease in development performance and cannot meet the refinement requirements of IC substrates.

[0005] In summary, the heat resistance is improved by grafting rigid segments on the components of the photosensitive resin composition through chemical modification, but the addition of rigid segments will affect the thermal expansion coefficient, that is, it will cause the photosensitive resin composition to have a microscopic decrease in molecular distance and a macroscopic shrinkage in volume during light and heat curing. The rapid polymerization rate and incomplete conversion of double bonds can easily cause stress concentration in the photosensitive resin, resulting in product cracking, warping and wrinkling, affecting the performance and appearance of the final product; the thermal expansion coefficient is reduced by introducing flexible segments into the components of the photosensitive resin composition, and the wrinkling and warping problems are improved, but the heat resistance and other properties will be lost to a certain extent; the method of reducing the thermal expansion coefficient by adding inorganic fillers, although the method is simple and low-cost, will cause problems of uneven dispersion and incompatibility of the system, and will also affect the subsequent development performance. Although some technologies avoid the problems of uneven dispersion and incompatibility by modifying the inorganic fillers, it will increase the cost.

[0006] Therefore, how to improve the heat resistance, thermal expansion coefficient and development performance of the photosensitive resin composition so that it can meet the requirements of refinement and high density of IC substrates is a technical problem that needs to be solved urgently in this field. Summary of the invention

[0007] The main purpose of the present invention is to provide a photosensitive resin composition, a solder resist dry film, a photosensitive laminate, a solder resist pattern and a semiconductor packaging carrier, so as to solve the technical problem in the prior art that it is difficult to improve the heat resistance, thermal expansion coefficient and development performance of the photosensitive resin composition at the same time, so as to meet the requirements of refinement and high density of IC carriers.

[0008] In order to achieve the above-mentioned object, according to the first aspect of the present invention, a photosensitive resin composition is provided, which comprises, by weight, 100 to 120 parts of an alkali-soluble resin, 5 to 25 parts of a photopolymerizable monomer, 1 to 7 parts of a photoinitiator, 10 to 30 parts of an epoxy resin, 3 to 15 parts of an epoxy-based glass polymer prepolymer, and 1 to 5 parts of a curing agent and an accelerator thereof.

[0009] Further, the epoxy-based glass polymer prepolymer is 5 to 10 parts by weight; and / or, the epoxy-based glass polymer prepolymer is a prepolymer having a dynamic cross-linked network structure formed by the reaction of a glycidyl compound and a carboxylic acid compound, and has an intramolecular hydrogen bond structure formed by the association of β-hydroxyl and ester groups as shown in Formula 1

[0010]

[0011] Further, the glycidyl compound has a cyclic structure containing at least four atoms, and the glycidyl compound also contains at least two epoxy groups; preferably, the glycidyl compound is selected from at least one of bisphenol A diglycidyl ether, magnolol glycidyl ether, resorcinol diglycidyl ether, bisphenol F diglycidyl ether, cardanol glycidyl ether, terephthalic acid diglycidyl ester, tetrahydrophthalic acid diglycidyl ester, hexahydrophthalic acid diglycidyl ester, isocyanuric acid triglycidyl ester, 1,2-cyclohexanedicarboxylic acid diglycidyl ester, and 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester.

[0012] Furthermore, the carboxylic acid compound contains at least two carboxyl groups, and the ortho-group of at least one carboxyl group is a hydroxyl group; preferably, the carboxylic acid compound is selected from at least one of 2-hydroxysuccinic acid and 2,3-hydroxysuccinic acid.

[0013] Furthermore, the mass ratio of the epoxy resin to the epoxy-based glass polymer prepolymer is (1 to 5): 1; and / or, the epoxy resin is 15 to 25 parts by mass; and / or, the epoxy resin contains at least two functional groups and has a cyclic structure; preferably, the epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, hydrogenated bisphenol A epoxy resin, phenolic epoxy resin, alicyclic epoxy resin, hydantoin epoxy resin, and imide epoxy resin.

[0014] Furthermore, the alkali-soluble resin is an epoxy acrylic resin containing a carboxyl group; preferably, the alkali-soluble resin is an epoxy acrylic resin containing a carboxyl group and having a rigid chemical structure, preferably, the alkali-soluble resin includes an epoxy acrylic resin containing a polycyclic structure on the main chain or side chain; preferably, the alkali-soluble resin is selected from at least one of bisphenol A epoxy acrylic resin, alicyclic epoxy acrylic resin, and phenolic epoxy acrylic resin.

[0015] Further, the photopolymerizable monomer is 7 to 15 parts by weight; and / or, the photopolymerizable monomer comprises a monofunctional acrylate and a multifunctional acrylate; preferably, the monofunctional acrylate has a cyclic structure; further preferably, the monofunctional acrylate is selected from at least one of tetrahydrofuran acrylate, 2-phenoxyethyl acrylate, cycloaliphatic acrylate, (4) ethoxylated nonylphenol acrylate, isobornyl acrylate, trimethylolpropane formal acrylate, alkoxylated phenol acrylate, alkoxylated tetrahydrofuran acrylate, and alkoxylated nonylphenol acrylate; preferably, the multifunctional acrylate comprises at least one of 2 to 6 functional groups. acrylate; further preferably, the multifunctional acrylate is selected from at least one of pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, ethoxylated pentaerythritol tetraacrylate, dipentaerythritol acrylate, trimethylolpropane acrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, (3) ethoxylated trimethylolpropane triacrylate, pentaerythritol triacrylate, ethoxylated trimethylolpropane triacrylate, (3) propoxylated trimethylolpropane triacrylate, and (6) ethoxylated trimethylolpropane triacrylate; preferably, the mass ratio of the monofunctional acrylate to the multifunctional acrylate is (0.3-0.5):1.

[0016] Further, in terms of mass fractions, the photoinitiator is 2 to 4 parts, and the curing agent and its accelerator are 1 to 3 parts; and / or the photoinitiator includes a free radical photoinitiator and / or a cationic photoinitiator; preferably, the free radical photoinitiator is selected from 2,4,6-trimethylbenzoyldiphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, 2-isopropylthioxanthone, 1-hydroxycyclohexylphenyl ketone, benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, tetramethyl Michler's ketone, tetraethyl Michler's ketone, 2-chlorothioxanthone, 1-chloro-4-propoxythioxanthone, At least one of anthrone, 2,4-diethylthioxanthone, benzoin dimethyl ether, 2-hydroxy-methylphenylpropane-1-one, ethyl 4-(N,N-dimethylamino)benzoate, and 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone; the cationic photoinitiator is selected from triphenylsulfonium hexafluorophosphate, 4-phenylthiophenyl diphenylsulfonium salt, 4-dodecyloxyphenyl diphenylsulfonium hexafluoroantimonate, bis[(4-diphenylsulfonium)benzene] sulfide-bis-hexafluorophosphate, 4-phenylthiophenyl diphenylsulfonium salt, (4-hydroxyphenyl)methyl (benzyl) hexasulfonium fluorophosphate, 4-acetoxyphenyl dimethylsulfonium hexafluoroantimonate, diphenyl and / or the curing agent comprises at least one of an amine curing agent, a boron amine salt curing agent, a boron amine complex curing agent, an acid anhydride curing agent, a linear phenolic resin curing agent, a polyester resin curing agent, a polysulfide rubber curing agent, and an imidazole curing agent; and / or the accelerator comprises at least one of an electrophilic accelerator, a nucleophilic accelerator, and a metal carboxylate accelerator; preferably, the curing agent is selected from 2-methylimidazole, 2-ethylimidazole, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl disulfide, 3-aminobenzylamine, m-phenylenediamine, 3-amino-5-mercapto-1,2,4-triazole, 4-amino-3-hydrazino-5-mercapto-1,2, At least one of 4-triazole, 1,3-bis(2,4,6-trimethylphenyl)imidazole chloride, 1-tritylimidazole, 4-imidazole-1-phenylpropiotone, 1-ethyl-3-methylimidazole tetrafluoroborate, 1-ethylimidazole, 1-allylimidazole, 2,4,5-triphenylimidazole, melamine, melamine phosphate, melamine phosphate, trichloromelamine, hexamethylol melamine, 1,8-diazabicyclo[5,4,0]dodec-7-ene, 4-cyanobenzylamine, 4,4'-diaminodiphenyl sulfone, 1-ethyl-3-methylimidazolium dicyanamide, 1-butyl-3-methylimidazolium dicyanamide, adipic acid dihydrazide, sebacic acid dihydrazide, and triphenylphosphine.

[0017] According to a second aspect of the present invention, a solder resist dry film is provided. The solder resist dry film is obtained by mixing and drying the above-mentioned photosensitive resin composition.

[0018] According to a third aspect of the present invention, there is provided a photosensitive laminate, comprising a supporting layer, a photosensitive layer and a protective layer which are stacked, wherein the photosensitive layer is the above-mentioned solder resist dry film.

[0019] According to a fourth aspect of the present invention, a solder resist pattern is provided. The solder resist pattern is formed by sequentially exposing, developing and curing the above-mentioned solder resist dry film.

[0020] According to a fifth aspect of the present invention, a semiconductor package carrier is provided, comprising a solder resist pattern, wherein the solder resist pattern is obtained by mixing and curing the photosensitive resin composition of the first aspect, or the solder resist pattern is the solder resist pattern described in the fourth aspect.

[0021] The implementation of the present invention has at least the following beneficial effects:

[0022] The photosensitive resin composition provided by the present invention cooperates with each other in that, on the one hand, by introducing an epoxy-based glass polymer prepolymer to interact with other components, a three-dimensional cross-linked network formed by the composition system has dynamic covalent bonds. Under external stimulation (such as light or heat) of a curing process (such as photocuring or thermal curing), the dynamic covalent bonds can be exchanged, and the topological structure of the three-dimensional cross-linked structure is rearranged, that is, the covalent bonds are broken and reorganized in the photosensitive resin composition system, so that the distance between molecules is expanded, the mobility of the chain segments is improved, thereby releasing local stress and reducing the thermal expansion coefficient. , avoiding cracking, wrinkling and warping caused by volume shrinkage and stress concentration. At the same time, the exchange reaction of dynamic covalent bonds only changes the crosslinking points, but does not reduce the number of crosslinking points, thereby avoiding the loss of crosslinking degree and crosslinking density, and ensuring the heat resistance, hardness, scratch resistance, acid and alkali resistance, solvent resistance, cold and hot shock resistance and other properties of the photosensitive resin composition; on the other hand, the epoxy-based glass polymer prepolymer is used as a heat-curing component in the composition system, and adding a small mass fraction can achieve the maximum performance, ensuring that the photosensitive resin composition has good alkali developability and high resolution. In this way, by limiting the mass fraction of specific components, the components interact with each other, while ensuring the heat resistance, hardness, scratch resistance, acid and alkali resistance, solvent resistance, cold and hot shock resistance, and development performance of the photosensitive resin composition, it can also reduce the thermal expansion coefficient and avoid cracking, warping and wrinkling. Problems such as wrinkling can be avoided, so that it can meet the requirements of refinement and high density of IC carriers. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the embodiment of the present invention will be clearly and completely described below in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all the embodiments. Based on the embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] As described in the background art, it is difficult to improve the heat resistance, thermal expansion coefficient and developing performance of the photosensitive resin composition in the prior art. In order to solve the above technical problems, the first aspect of the present invention provides a photosensitive resin composition, which comprises, by weight, 100 to 120 parts of an alkali-soluble resin, 5 to 25 parts of a photopolymerizable monomer, 1 to 7 parts of a photoinitiator, 10 to 30 parts of an epoxy resin, 3 to 15 parts of an epoxy-based glass polymer prepolymer, and 1 to 5 parts of a curing agent and its accelerator.

[0025] The photosensitive resin composition of the present invention can be used as a solder resist material on a semiconductor package (IC) substrate. In a specific implementation process, the components need to be mixed and then cured to form a solder resist pattern.

[0026] In the present invention, epoxy-based glass polymer prepolymer refers to a glass-like polymer material having epoxy groups. Among them, by introducing epoxy-based glass polymer prepolymer to interact with other components to form dynamic covalent bonds, the three-dimensional cross-linked network formed by the composite system has dynamic covalent bonds, and the dynamic covalent bonds can undergo an exchange reaction of dynamic covalent bonds under external stimulation (such as light, heat) of a curing process (such as photocuring, thermal curing, etc.), so that the topological structure of the three-dimensional cross-linked network is rearranged. Specifically, the epoxy-based glass polymer prepolymer can interact with other components (such as alkali-soluble resins, epoxy resins, curing agents, etc.) to generate dynamic covalent bonds, and under the photosensitive resin During the curing process of the composition, a dynamic covalent bond exchange reaction occurs. The breaking and recombination of the covalent bonds expands the distance between molecules and improves the mobility of the chain segments, thereby releasing local stress and reducing the thermal expansion coefficient, avoiding cracking, wrinkling and warping caused by volume shrinkage and stress concentration. At the same time, the dynamic covalent bond exchange reaction only changes the cross-linking points, but does not reduce the number of cross-linking points, thereby avoiding the loss of cross-linking degree and cross-linking density, and ensuring the heat resistance, hardness, scratch resistance, acid and alkali resistance, solvent resistance, and resistance to cold and hot shocks of the photosensitive resin composition.

[0027] In addition, the epoxy-based glass polymer prepolymer is used as a heat-curing component in the composition system. Adding a small mass fraction can achieve maximum performance and ensure that the photosensitive resin composition has good alkali developability and high resolution. In this way, by limiting the mass fraction of a specific component, the components cooperate with each other, while ensuring the heat resistance, hardness, scratch resistance, acid and alkali resistance, solvent resistance, cold and hot shock resistance, and development performance of the photosensitive resin composition, it can also reduce the thermal expansion coefficient and avoid problems such as cracking, warping and wrinkling, so that it can meet the needs of refinement and high density of IC carriers.

[0028] In the present invention, the dynamic covalent bond can be an ester structure. Specifically, the epoxy group in the epoxy-based glass polymer prepolymer and / or the epoxy group in the epoxy resin reacts with the carboxylic acid group of the alkali-soluble resin and / or the anhydride group of the curing agent to form an ester structure. At this time, the ester structure acts as a dynamic covalent bond and undergoes an ester exchange reaction during the curing process. That is, the dynamic covalent bond exchange reaction during the curing process is based on the dynamic exchange between the ester group and the hydroxyl group. In this way, not only can the performance of the dynamic covalent bond be maximized, but the operation is also simple and easy to implement, which helps to reduce costs.

[0029] In some preferred embodiments, the epoxy-based glass polymer prepolymer is 5 to 10 parts by weight.

[0030] In some embodiments, the epoxy-based glass polymer prepolymer is a prepolymer having a dynamic cross-linked network structure formed by the reaction of a glycidyl compound and a carboxylic acid compound, and has an intramolecular hydrogen bond structure formed by the association of β-hydroxyl groups and ester groups as shown in Formula 1.

[0031]

[0032] In this way, the epoxy-based glass polymer prepolymer contains an intramolecular hydrogen bond hexacyclic structure. Compared with the intermolecular hydrogen bond, the intramolecular hydrogen bond hexacyclic structure has greater strength and a closer action distance, so that the epoxy-based glass polymer prepolymer containing the intramolecular hydrogen bond hexacyclic structure has excellent rigidity, and thus the photosensitive resin composition has good heat resistance, hardness, scratch resistance, acid and alkali resistance, solvent resistance, and resistance to cold and hot shocks.

[0033] The present invention does not limit the specific preparation parameters of the epoxy-based glass polymer prepolymer, and it can be prepared by conventional methods in the art. For example, a glycidyl compound and a carboxylic acid compound are mixed in a certain molar ratio, reacted at a certain reaction temperature, and after the reaction is completed, the reaction product is washed with deionized water, dried with anhydrous sodium sulfate, and finally placed in a vacuum oven to dry to obtain an epoxy-based glass polymer prepolymer. In some embodiments, the molar ratio of the glycidyl compound to the carboxylic acid compound is (2 to 5): 1, the reaction time is 0.5 to 1.5 hours, the reaction temperature is 80 to 120°C, the drying temperature is 50 to 70°C, and the drying time is 10 to 14 hours. By limiting the specific type and addition amount of the reaction raw materials, it is helpful to obtain an epoxy-based glass polymer prepolymer that meets the above requirements. In addition, by limiting the reaction conditions, it is helpful to regulate the molecular weight and degree of polymerization of the prepolymer within an appropriate range.

[0034] In some embodiments, the glycidyl compound has a cyclic structure containing at least four atoms, and the glycidyl compound also contains at least two epoxy groups. In this way, the cyclic structure can enhance the rigidity of the epoxy-based glass polymer prepolymer, and further improve the heat resistance, hardness, scratch resistance, acid and alkali resistance, solvent resistance, and resistance to cold and hot shock of the photosensitive resin composition; in addition, the epoxy groups in the epoxy-based glass polymer prepolymer are mainly derived from the glycidyl compound. By limiting the number of epoxy groups in the glycidyl compound, the number of epoxy groups in the epoxy-based glass polymer prepolymer is essentially limited, which helps to provide more epoxy groups for reaction to achieve the formation of ester structure, that is, to ensure the formation of sufficient dynamic covalent bonds, thereby achieving the purpose of reducing the thermal expansion coefficient.

[0035] In some preferred embodiments, the glycidyl compound is selected from at least one of bisphenol A diglycidyl ether, resorcinol diglycidyl ether, bisphenol F diglycidyl ether, magnolol glycidyl ether, cardanol glycidyl ether, terephthalic acid diglycidyl ester, tetrahydrophthalic acid diglycidyl ester, hexahydrophthalic acid diglycidyl ester, isocyanuric acid triglycidyl ester, 1,2-cyclohexanedicarboxylic acid diglycidyl ester, and 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester.

[0036] In some embodiments, the carboxylic acid compound contains at least two carboxyl groups, and the ortho-group of at least one carboxyl group is a hydroxyl group. In this way, it is helpful to prepare an epoxy-based glass polymer prepolymer having a structure of Formula 1, that is, to form an intramolecular hydrogen bond six-membered ring structure, thereby taking into account the improvement of the heat resistance and developing performance of the photosensitive resin composition and the reduction of the thermal expansion coefficient. In addition, multiple epoxy groups in the glycidyl compound can interact with multiple carboxyl groups in the carboxylic acid compound, which can increase the number of cross-linking points of the cross-linking reaction and generate a network cross-linked polymer with a large cross-linking density.

[0037] Specifically, in some preferred embodiments, the carboxylic acid compound is selected from at least one of 2-hydroxysuccinic acid and 2,3-hydroxysuccinic acid.

[0038] In some embodiments, the mass ratio of the epoxy resin to the epoxy-based glass polymer prepolymer is (1-5):1, such as 1:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 5:1 or any two thereof. By limiting the mass ratio of the epoxy resin to the epoxy-based glass polymer prepolymer to the above range, it is beneficial to further balance the reduction of the thermal expansion coefficient and the guarantee of heat resistance.

[0039] In some preferred embodiments, the epoxy resin is 15 to 25 parts by weight. Further limiting the mass fraction of the epoxy resin helps to further improve the comprehensive performance of the photosensitive resin composition.

[0040] In some embodiments, the epoxy resin comprises at least two functional groups and has a cyclic structure. Specifically, in some preferred embodiments, the epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, hydrogenated bisphenol A epoxy resin, novolac epoxy resin, alicyclic epoxy resin, hydantoin epoxy resin, and imide epoxy resin. For example, epoxy resins derived from Japan DIC are preferred, and specifically may include naphthalene ring type multifunctional epoxy HP-4710, HP-4032D, HP-9500, HP-6000, HP-7241, HP-7250, HP-6000L, HP-5000, HP-4770, EXA-9900, or dicyclopentadiene type multifunctional epoxy HP-7200H, HP-7200HHH, or bisphenol A or bisphenol F type epoxy EXA-830CRP, EXA-830LVP, EXA-835LV, EXA-850CRP, or phenolic epoxy resin N-730A, and may also be at least one of NC-3000, NC-3000H, and XD-1000 derived from Chemical Medicine Chemical (Wuxi) Co., Ltd.

[0041] In some embodiments, the alkali-soluble resin is an epoxy acrylic resin containing a carboxyl group; preferably, the alkali-soluble resin is an epoxy acrylic resin containing a carboxyl group and having a rigid chemical structure, and preferably, the alkali-soluble resin includes an epoxy acrylic resin containing a polycyclic structure on the main chain or side chain. By limiting the type of the alkali-soluble resin to be selected within the above range, it is helpful to further improve the photosensitivity and developing ability of the photosensitive resin composition.

[0042] Specifically, the alkali-soluble resin can be selected from at least one of bisphenol A epoxy acrylic resin, alicyclic epoxy acrylic resin, and phenolic epoxy acrylic resin. Among them, the alkali-soluble resin is preferably derived from epoxy acrylic resin of Nippon Chemical, which can be R-115W, R-190W, KEA-11, EAM-2160W, EAM-5060W, EAM-5080W, CCR-1159HW, CCR-1169HW, CCR-1171HW, CCR-1173HW, CCR-4959HW, CCR-4969HW, WH-205 and other models; it can also be HC166, B325, L1057M, Q857, Q612 from Mitsui Chemicals of Japan. , Q850, QC300G, Q890; it can also be anhydride modified o-cresol epoxy acrylic resin from Shanghai Showa, such as PR300CP, PR3000, PR400 and other models, or bisphenol A epoxy modified acrylic resin (PRV series); it can also be GF-105, GF-104HM, GF-106R, GF-105F-1, GF-105GM, GF-108, GF-159, GF-130, GF-148, GF-211LX, GF-068 and other models from Guangzhou Starley.

[0043] In some embodiments, the photopolymerizable monomer is 7 to 15 parts by weight. Specifically, the photopolymerizable monomer includes a monofunctional acrylate and a multifunctional acrylate. That is, the photopolymerizable monomer is compounded from a monofunctional acrylate and a multifunctional acrylate, and specifically can be compounded from at least one monofunctional acrylate and at least two multifunctional acrylates.

[0044] In the present invention, the monofunctional acrylate has a cyclic structure; more preferably, the monofunctional acrylate is selected from at least one of tetrahydrofuran acrylate, 2-phenoxyethyl acrylate, cycloaliphatic acrylate, (4) ethoxylated nonylphenol acrylate, isobornyl acrylate, trimethylolpropane formal acrylate, alkoxylated phenol acrylate, alkoxylated tetrahydrofuran acrylate, and alkoxylated nonylphenol acrylate; preferably, the multifunctional acrylate includes acrylates with a functionality of 2 to 6; further .... Preferably, the multifunctional acrylate is selected from at least one of pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, ethoxylated pentaerythritol tetraacrylate, dipentaerythritol acrylate, trimethylolpropane acrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, (3) ethoxylated trimethylolpropane triacrylate, pentaerythritol triacrylate, ethoxylated trimethylolpropane triacrylate, (3) propoxylated trimethylolpropane triacrylate, and (6) ethoxylated trimethylolpropane triacrylate.

[0045] Preferably, the mass ratio of the monofunctional acrylate to the multifunctional acrylate is (0.3-0.5):1, for example, 0.3:1, 0.4:1, 0.5:1 or a range consisting of any two thereof.

[0046] In some embodiments, the photoinitiator is 2 to 4 parts by weight, and the curing agent and its accelerator are 1 to 3 parts by weight; and / or the photoinitiator includes a free radical photoinitiator and / or a cationic photoinitiator; preferably, the free radical photoinitiator is selected from 2,4,6-trimethylbenzoyldiphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, 2-isopropylthioxanthone, 1-hydroxycyclohexylphenyl ketone, benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, tetramethyl Michler's ketone, tetraethyl Michler's ketone, 2-chlorothioxanthone, 1-chloro-4-propoxy At least one of 2-(4-(2-hydroxyethoxy)phenyl)-1-propanone, ... and / or the curing agent comprises at least one of an amine curing agent, a boron amine salt curing agent, a boron amine complex curing agent, an acid anhydride curing agent, a linear phenolic resin curing agent, a polyester resin curing agent, a polysulfide rubber curing agent, and an imidazole curing agent; and / or the accelerator comprises at least one of an electrophilic accelerator, a nucleophilic accelerator, and a metal carboxylate accelerator; preferably, the curing agent is selected from 2-methylimidazole, 2-ethylimidazole, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl disulfide, 3-aminobenzylamine, m-phenylenediamine, 3-amino-5-mercapto-1,2,4-triazole, 4-amino-3-hydrazino-5-mercapto-1,2 , 4-triazole, 1,3-bis(2,4,6-trimethylphenyl)imidazole chloride, 1-tritylimidazole, 4-imidazole-1-phenylpropiotone, 1-ethyl-3-methylimidazole tetrafluoroborate, 1-ethylimidazole, 1-allylimidazole, 2,4,5-triphenylimidazole, melamine, melamine phosphate, melamine phosphate, trichloromelamine, hexamethylol melamine, 1,8-diazabicyclo[5,4,0]dodec-7-ene, 4-cyanobenzylamine, 4,4'-diaminodiphenyl sulfone, 1-ethyl-3-methylimidazolium dicyanamide, 1-butyl-3-methylimidazolium dicyanamide, adipic acid dihydrazide, sebacic acid dihydrazide, and at least one of triphenylphosphine.

[0047] In some embodiments, the photosensitive resin composition further comprises 15 to 40 parts of filler, 2 to 10 parts of auxiliary agent and 30 parts of solvent, preferably, the filler is 20 to 35 parts; preferably, the auxiliary agent is 2 to 7 parts; and / or, the auxiliary agent comprises a colorant, a defoamer, an antioxidant and a leveling agent; preferably, the filler is an inorganic filler; further preferably, the inorganic filler is selected from at least one of silicon dioxide, titanium dioxide, barium sulfate, calcium carbonate, aluminum hydroxide, kaolin, talc, titanium oxide, aluminum oxide, silicon nitride and aluminum nitride; preferably, the colorant is at least one of a pigment, a dye, and a pigment; species; further preferably, the colorant is selected from at least one of carbon black, indigo blue, indigo green, toluidine red, chrome yellow and titanium white; preferably, the defoaming agent is selected from at least one of emulsion polysiloxane, polyether-modified silicone, high carbon alcohol and polyether; preferably, the antioxidant is selected from at least one of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 2,6-di-tert-butyl-4-methylphenol, catechol and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxyphenyl) isocyanate; preferably, the leveling agent is selected from at least one of modified polysiloxane and long-chain resin.

[0048] The addition of solvent helps to promote the full mixing of the components of the photosensitive resin composition. The solvent can be any conventional solvent used in the art, preferably γ-butyrolactone.

[0049] The second aspect of the present invention provides a solder resist dry film, which is obtained by mixing and drying the above-mentioned photosensitive resin composition. The solder resist dry film formed by the above-mentioned photosensitive resin composition has excellent heat resistance, developing performance and low thermal expansion coefficient, and is not prone to cracking, warping and wrinkling. In addition, the solder resist dry film formed by the above-mentioned photosensitive resin composition also has excellent hardness, HAST, acid resistance, alkali resistance and solvent resistance, and has good alkali developability and high analytical performance. The solder resist dry film made of the above-mentioned photosensitive resin composition is suitable for the packaging field, can meet the requirements of refinement and high density of semiconductor packaging carriers, is conducive to the formation of specific solder resist patterns, and can ensure the performance and appearance of the final product.

[0050] A third aspect of the present invention provides a photosensitive laminate, comprising a support layer, a photosensitive layer and a protective layer which are stacked, wherein the photosensitive layer is the above-mentioned solder resist dry film.

[0051] In the specific implementation process of the present invention, the above-mentioned photosensitive resin composition can be mixed and directly coated on the support layer, and after drying, a photosensitive layer is formed, and then a protective layer is attached to the photosensitive layer to finally obtain a photosensitive laminate. Among them, the protective layer is used to protect and prevent the performance of the photosensitive layer from being reduced. In the specific use process, the protective layer can be removed to attach the photosensitive layer to the component to be processed, and the support layer can be removed to cover the surface of the component to be processed. The component to be processed can be a conventional electronic component in the art.

[0052] The fourth aspect of the present invention provides a solder resist pattern, which is formed by the above-mentioned solder resist dry film after exposure, development and curing. In the specific implementation process of the present invention, the solder resist dry film is covered on the component to be processed, and then the corresponding solder resist pattern can be obtained after exposure, development and curing. Since the solder resist dry film formed by the above-mentioned photosensitive resin composition has excellent heat resistance, development performance and low thermal expansion coefficient, the solder resist pattern is more complete and is not prone to cracking, wrinkling and warping. In addition, the photosensitive resin composition formed also has excellent hardness, HAST, acid resistance, alkali resistance and solvent resistance, and has good alkali developability and high analytical performance, which ensures the strength, stability and non-flaking property of the solder resist pattern.

[0053] A fifth aspect of the present invention provides a semiconductor package carrier, characterized in that it includes a solder resist pattern, which is obtained by mixing and curing the photosensitive resin composition of the first aspect, or the solder resist pattern is the solder resist pattern of the fourth aspect.

[0054] Due to the inclusion of the above-mentioned photosensitive resin composition, the solder resist pattern has excellent heat resistance, developing performance and low thermal expansion coefficient, and is not prone to cracking, warping and wrinkling. In addition, it has excellent hardness, HAST, acid resistance, alkali resistance and solvent resistance, and can meet the requirements of refinement and high density of semiconductor packaging carriers, thereby ensuring the performance and appearance of semiconductor packaging carriers.

[0055] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0056] Example 1

[0057] 1. Preparation of epoxy-based glass polymer prepolymer A-1

[0058] Add 2-hydroxybutanedioic acid (13.4 g, 0.1 mol) into a three-necked flask, and add bisphenol A diglycidyl ether (136 g, 0.4 mol) into the three-necked flask, and react at 110°C for 1 hour. After the reaction, wash the product with deionized water, dry it with anhydrous sodium sulfate, and finally place it in a vacuum oven at 60°C and dry it for 12 hours to obtain epoxy glass polymer prepolymer A-1.

[0059] 2. Preparation of solder mask dry film

[0060] In terms of mass fractions, alkali-soluble resin, inorganic filler, epoxy-based glass polymer prepolymer and additives are added to a solvent and mixed evenly, and ground by a sand mill to a particle size of less than 10 μm, and then photopolymerization monomer, photoinitiator, epoxy resin and curing agent are added in sequence and mixed evenly to obtain a photosensitive resin composition; the photosensitive resin composition is evenly coated on a PET support film by a coater, and placed in an oven at 85°C for 30 minutes to obtain a solder resist dry film with a thickness of 25 μm.

[0061] The specific information of the above components is as follows:

[0062] The alkali-soluble resin is an anhydride-modified o-cresol-formaldehyde epoxy acrylic resin, and its mass fraction is 110 parts;

[0063] The photopolymerizable monomers are 3 parts by mass of isobornyl acrylate and 7 parts by mass of pentaerythritol tetraacrylate;

[0064] The photoinitiator is 1 part by mass of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1 part by mass of 1-hydroxycyclohexylphenyl ketone and 1 part by mass of 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone;

[0065] The inorganic filler is 20 parts by mass of barium sulfate and 12 parts by mass of silicon dioxide;

[0066] The epoxy resin is 20 parts by weight of bisphenol A epoxy resin;

[0067] The mass fraction of epoxy-based glass polymer prepolymer A-1 is 6 parts;

[0068] The curing agent is 1 part by mass of 4,4'-diaminodiphenyl sulfone, 0.5 parts by mass of 2-ethyl-4-methylimidazole and 0.5 parts by mass of 3-amino-5-mercapto-1,2,4-triazole;

[0069] The auxiliary agent is 1.5 parts by mass of carbon black, 1 part by mass of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 0.5 parts by mass of leveling agent polyether-modified polydimethylsiloxane, and 0.5 parts by mass of defoaming agent octamethylcyclotetrasiloxane;

[0070] The solvent was 30 parts by mass of γ-butyrolactone.

[0071] Example 2

[0072] The difference from Example 1 is that when preparing the epoxy-based glass polymer prepolymer, 2-hydroxysuccinic acid (13.4 g, 0.1 mol) is replaced with 2,3-dihydroxysuccinic acid (15 g, 0.1 mol), and other conditions remain unchanged, to obtain the epoxy-based glass polymer prepolymer A-2 of this example;

[0073] When preparing the solder resist dry film, the epoxy-based glass polymer prepolymer A-1 is replaced with the epoxy-based glass polymer prepolymer A-2 of this embodiment to obtain the solder resist dry film of this embodiment.

[0074] Example 3

[0075] The difference from Example 1 is that when preparing the epoxy-based glass polymer prepolymer, bisphenol A diglycidyl ether (136 g, 0.4 mol) is replaced with magnolol glycidyl ether (152 g, 0.4 mol), and other conditions remain unchanged, to obtain the epoxy-based glass polymer prepolymer A-3 of this example;

[0076] The synthesis of magnolol glycidyl ether includes the following steps: magnolol (106.4g, 0.4mol), epichlorohydrin (148g, 1.6mol) and tetrabutylammonium bromide (7.6g, 3%) are added to a three-necked round-bottom flask in sequence and stirred at 80°C for 3h. Then, sodium hydroxide (32g, 0.8mol) with a mass fraction of 50% is added dropwise to the reactor using a constant pressure dropping funnel. Stir at room temperature for 5h. After the reaction is completed, the filtrate is poured into a separatory funnel, washed with deionized water, then dried with anhydrous sodium sulfate, and finally placed in a vacuum oven at 80°C for 12h to obtain magnolol glycidyl ether;

[0077] When preparing the solder resist dry film, the epoxy-based glass polymer prepolymer A-1 is replaced with the epoxy-based glass polymer prepolymer A-3 of this embodiment to obtain the solder resist dry film of this embodiment.

[0078] Example 4

[0079] The difference from Example 1 is that when preparing the epoxy-based glass polymer prepolymer, 2-hydroxysuccinic acid (13.4 g, 0.1 mol) is replaced with succinic acid (11.8 g, 0.3 mol), and other conditions remain unchanged, to obtain the epoxy-based glass polymer prepolymer B-1 of this example;

[0080] When preparing the solder resist dry film, the epoxy-based glass polymer prepolymer A-1 is replaced with the epoxy-based glass polymer prepolymer B-1 of this embodiment to obtain the solder resist dry film of this embodiment.

[0081] Example 5

[0082] The difference from Example 1 is that when preparing the epoxy-based glass polymer prepolymer, bisphenol A diglycidyl ether (136 g, 0.4 mol) is replaced with polyethylene glycol diglycidyl ether (52 g, 0.4 mol), and other conditions remain unchanged, to obtain the epoxy-based glass polymer prepolymer B-2 of this example;

[0083] When preparing the solder resist dry film, the epoxy-based glass polymer prepolymer A-1 is replaced with the epoxy-based glass polymer prepolymer B-2 of this embodiment to obtain the solder resist dry film of this embodiment.

[0084] Example 6

[0085] The difference from Example 1 is that the mass fraction of epoxy resin is 23 parts, and the mass fraction of epoxy-based glass polymer prepolymer is 5 parts.

[0086] Example 7

[0087] The difference from Example 1 is that the mass fraction of epoxy resin is 17 parts, and the mass fraction of epoxy-based glass polymer prepolymer is 9 parts.

[0088] Example 8

[0089] The difference from Example 1 is that the mass fraction of the alkali-soluble resin is 100 parts.

[0090] Example 9

[0091] The difference from Example 1 is that the mass fraction of the alkali-soluble resin is 120 parts.

[0092] Example 10

[0093] The difference from Example 1 is that the photopolymerizable monomers are 1 part by mass of isobornyl acrylate and 4 parts by mass of pentaerythritol tetraacrylate.

[0094] Embodiment 11

[0095] The difference from Example 1 is that the photopolymerizable monomers are 2 parts by mass of isobornyl acrylate (produced by Sartomer, trade name SR506EGNS) and 5 parts by mass of pentaerythritol tetraacrylate (produced by Sartomer, trade name SR295NS).

[0096] Example 12

[0097] The difference from Example 1 is that the photopolymerizable monomers are 5 parts by mass of isobornyl acrylate and 10 parts by mass of pentaerythritol tetraacrylate.

[0098] Embodiment 13

[0099] The difference from Example 1 is that the photopolymerizable monomers are 10 parts by mass of isobornyl acrylate and 15 parts by mass of pentaerythritol tetraacrylate.

[0100] Embodiment 14

[0101] The difference from Example 1 is that the photoinitiator is 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide.

[0102] Embodiment 15

[0103] The difference from Example 1 is that the photoinitiator is 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 1 part of 1-hydroxycyclohexylphenyl ketone.

[0104] Example 16

[0105] The difference from Example 1 is that the photoinitiator is 2 parts of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1 part of 1-hydroxycyclohexylphenyl ketone and 1 part of 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone.

[0106] Embodiment 17

[0107] The difference from Example 1 is that the photoinitiator is 2 parts of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2 parts of 1-hydroxycyclohexylphenyl ketone and 3 parts of 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone.

[0108] Embodiment 18

[0109] The difference from Example 1 is that the mass fraction of epoxy resin is 10 parts.

[0110] Embodiment 19

[0111] The difference from Example 1 is that the mass fraction of epoxy resin is 30 parts.

[0112] Embodiment 20

[0113] The difference from Example 1 is that the mass fraction of the epoxy glass polymer prepolymer is 3 parts.

[0114] Embodiment 21

[0115] The difference from Example 1 is that the mass fraction of the epoxy glass polymer prepolymer is 10 parts.

[0116] Embodiment 22

[0117] The difference from Example 1 is that the mass fraction of the epoxy glass polymer prepolymer is 15 parts.

[0118] Embodiment 23

[0119] The difference from Example 1 is that the curing agent is 1 part of 4,4'-diaminodiphenyl sulfone.

[0120] Embodiment 24

[0121] The difference from Example 1 is that the curing agent is 1 part of 4,4'-diaminodiphenyl sulfone, 1 part of 2-ethyl-4-methylimidazole and 1 part of 3-amino-5-mercapto-1,2,4-triazole.

[0122] Embodiment 25

[0123] The difference from Example 1 is that the curing agent is 2 parts of 4,4'-diaminodiphenyl sulfone, 2 parts of 2-ethyl-4-methylimidazole and 1 part of 3-amino-5-mercapto-1,2,4-triazole.

[0124] Embodiment 26

[0125] The difference from Example 1 is that no inorganic filler is added to the photosensitive resin composition.

[0126] Embodiment 27

[0127] The difference from Example 1 is that the inorganic filler is 10 parts of barium sulfate and 5 parts of silicon dioxide.

[0128] Embodiment 28

[0129] The difference from Example 1 is that the inorganic filler is 20 parts of barium sulfate and 20 parts of silicon dioxide.

[0130] Embodiment 29

[0131] The difference from Example 1 is that no auxiliary agent is added to the photosensitive resin composition.

[0132] Embodiment 30

[0133] The difference from Example 1 is that the auxiliary agents are 0.5 parts of carbon black, 0.5 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 0.5 parts of leveling agent polyether-modified polydimethylsiloxane, and 0.5 parts of defoaming agent octamethylcyclotetrasiloxane.

[0134] Embodiment 31

[0135] The difference from Example 1 is that the auxiliary agent is 2.5 parts of carbon black, 2.5 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2.5 parts of leveling agent polyether-modified polydimethylsiloxane, and 2.5 parts of defoaming agent octamethylcyclotetrasiloxane.

[0136] Comparative Example 1

[0137] The difference from Example 1 is that no epoxy-based glass polymer prepolymer is added to the photosensitive resin composition.

[0138] Comparative Example 2

[0139] The difference from Example 1 is that the mass fraction of the epoxy-based glass polymer prepolymer is 2 parts.

[0140] Comparative Example 3

[0141] The difference from Example 1 is that the mass fraction of the epoxy-based glass polymer prepolymer is 20 parts.

[0142] Comparative Example 4

[0143] The difference from Example 1 is that no epoxy resin is added to the photosensitive resin composition.

[0144] Comparative Example 5

[0145] The difference from Example 1 is that the mass fraction of epoxy resin is 5 parts.

[0146] Comparative Example 6

[0147] The difference from Example 1 is that the mass fraction of epoxy resin is 10 parts.

[0148] Comparative Example 7

[0149] The difference from Example 1 is that the mass fraction of the alkali-soluble resin is 90 parts.

[0150] Comparative Example 8

[0151] The difference from Example 1 is that the mass fraction of the alkali-soluble resin is 130 parts.

[0152] Test example

[0153] (1) Sensitivity test

[0154] The above-mentioned solder mask dry film was attached to the commercial copper clad laminate by a vacuum laminator. The pressure in the vacuum section was 6kgf, the vacuum time was 20s, the pressing time was 30s, and the temperature was 65°C; the pressure in the leveling section was 6kgf, the leveling time was 50s, and the temperature was 85°C. After the attachment was completed, it was exposed and developed on the ST21 step exposure scale. The lowest energy that was not developed and completely exposed on the ST8 step was recorded as the sensitivity energy of the formula.

[0155] (2) L / S (line width and line spacing), side erosion and minimum window opening test

[0156] The above solder resist dry film is attached to the commercial copper clad laminate using a vacuum laminating machine. The pressure of the vacuum section is 6kgf, the vacuum time is 20s, the pressing time is 30s, and the temperature is 65℃; the pressure of the leveling section is 6kgf, the leveling time is 50s, and the temperature is 85℃. After the attachment is completed, it is exposed at ST8 / 21 sensitivity energy through a standard test mask film. After thermal curing, L / S and side etching are observed under a metallographic microscope through slicing, and the minimum window can be directly observed under a metallographic microscope. The optimal L / S and minimum window can be achieved when the line width, line spacing and window diameter can be fully presented and the error between them and the standard mask film is within ±5%. At this time, the size of the side etching is measured and recorded to observe whether the side etching is within ±5% of the standard mask film. The test results are graded as follows: Level 1: error within ±5%; Level 2: error outside ±5% and within ±10%; Level 3: error outside ±10%.

[0157] (3) Surface flatness test after thermal curing

[0158] The above-mentioned solder resist dry film was attached to the commercial copper clad laminate using a vacuum laminating machine, the pressure of the vacuum section was 6kgf, the vacuum time was 20s, the pressing time was 30s, and the temperature was 65°C; the pressure of the leveling section was 6kgf, the leveling time was 50s, and the temperature was 85°C. After the attachment was completed, the commercial copper clad laminate with the solder resist dry film was exposed under a high-pressure mercury lamp exposure machine, and the PET support film was peeled off and exposed with appropriate energy. After exposure, it was placed at room temperature for 30min and then developed at 30°C for 30s with an alkaline developer (1wt% sodium carbonate aqueous solution). After development, it was rinsed with water for 30s to remove the residual developer on the surface of the solder resist dry film, and then the copper clad laminate with the solder resist dry film was post-cured in an oven at 150°C for 1h. Observe whether the solder resist dry film on the copper clad laminate is cracked, wrinkled, and warped under a microscope. The test results are graded as follows: Level 1: The surface is flat, without wrinkles, cracks or warping; Level 2: The surface has wrinkles, cracks or warping.

[0159] (4) Tg (glass transition temperature) and CTE (coefficient of thermal expansion) tests

[0160] The above-mentioned solder resist dry film was attached to the commercial copper clad laminate using a vacuum laminating machine. The pressure of the vacuum section was 6kgf, the vacuum time was 20s, the pressing time was 30s, and the temperature was 65°C; the pressure of the leveling section was 6kgf, the leveling time was 50s, and the temperature was 85°C. After the attachment was completed, the whole board was exposed using ST8 / 21 sensitivity energy. After exposure, it was placed at room temperature for 30min and then developed at 30°C for 30s by an alkaline developer (1wt% sodium carbonate aqueous solution). After development, it was rinsed with water for 30s to remove the residual developer on the surface of the solder resist dry film, and then the copper clad laminate with the solder resist dry film was post-cured in an oven at 150°C for 1h. Then, after cutting it into 5mm wide and 25mm long with a cutting knife, the PET support film of the solder resist dry film product was peeled off to obtain a photosensitive resin composition cured product for thermal expansion coefficient evaluation. The thermal expansion coefficient in the tensile mode was determined using a TMA device (TMAQ400, Shenzhen Shante Technology). The tensile load is 0.1N, the span (distance between chucks) is 15mm, and the heating rate is 10℃ / min. First, install the sample on the device, heat it from room temperature (25℃) to 160℃, and leave it for 15 minutes. Then, cool it to -60℃, and measure it again under the condition of heating from -60℃ to 250℃ at a heating rate of 10℃ / min. Mark the inflection point seen in the range from 25℃ to 200℃ as Tg, and record the temperature at this time. CTE uses the slope of the tangent of the curve obtained at a temperature below Tg. The test results are graded as follows: Level 1: less than 50ppm / ℃; Level 2: 50~60ppm / ℃; Level 3: 60~70ppm / ℃; Level 4: more than 70ppm / ℃.

[0161] (5) HAST test

[0162] The above-mentioned solder resist dry film was attached to the commercial copper clad laminate using a vacuum laminator, with a pressure of 6 kgf in the vacuum section, a vacuum time of 20 s, a pressing time of 30 s, and a temperature of 65°C; the pressure in the leveling section was 6 kgf, the leveling time was 50 s, and the temperature was 85°C. After the attachment was completed, the entire board was exposed using ST8 / 21 sensitivity energy. After exposure, it was placed at room temperature for 30 minutes and then developed at 30°C for 30 seconds using an alkaline developer (1 wt% sodium carbonate aqueous solution). After development, it was rinsed with water for 30 seconds to remove the residual developer on the surface of the solder resist dry film. The copper clad laminate with the solder resist dry film was then post-cured in an oven at 150°C for 1 hour to obtain a test sample after HAST treatment. The resistivity of the dry film product before and after HAST treatment was tested with a resistance meter, and then the test sample was moved to the HAST chamber (PC-422R8D, Hirayama Manufacturing Co., Ltd.), and placed at 121°C and 100% humidity for 120 hours. The resistivity after HAST treatment was tested again, and the presence of bubble peeling and other phenomena was observed, and the resistivity changes before and after HAST were compared. The test results are graded as follows: Level 1: No bubble peeling or other phenomena, or the resistivity changes within ±10%; Level 2: No bubble peeling or other phenomena, or the resistivity changes within ±30%; Level 3: The dry film has a small amount of bubbling, peeling, or even falling off; Level 4: There are a lot of bubbles or falling off, or the resistivity changes>50%.

[0163] (6) Acid resistance test

[0164] The test sample was prepared by the same preparation method as in the HAST test. The test sample was immersed in a 10 vol% H2SO4 aqueous solution at 30°C for 30 minutes, and then rinsed with clean water and dried. Then a peeling test was performed using 3M tape. Acid resistance was evaluated according to the following standards. The test results were graded as follows: Level 1: The dry film had no bubbling, peeling, or even shedding; Level 2: The dry film had a small amount of bubbling, no peeling, and no shedding; Level 3: The dry film had a small amount of bubbling, peeling, or even shedding; Level 4: The dry film had a large amount of shedding.

[0165] (7) Alkali resistance test

[0166] The test samples were prepared by the same preparation method as in the HAST test. The test samples were immersed in a 10 vol% NaOH aqueous solution at 30°C for 30 minutes, and then rinsed with clean water and dried. Then the peeling test was performed with 3M tape. The alkali resistance was evaluated according to the following standards. The test results were graded as follows: Level 1: The dry film had no bubbling, peeling, or even shedding; Level 2: The dry film had a small amount of bubbling, no peeling, and no shedding; Level 3: The dry film had a small amount of bubbling, peeling, or even shedding; Level 4: The dry film had a large amount of shedding.

[0167] (8)Solvent resistance test

[0168] The test samples were prepared using the same preparation method as in the HAST test. The test samples were immersed in propylene glycol methyl ether acetate solvent at 30°C for 30 minutes, and then taken out and dried for peeling test using 3M tape. The solvent resistance was evaluated according to the following standards. The test results were graded as follows: Level 1: The dry film had no bubbling, peeling, or even shedding; Level 2: The dry film had a small amount of bubbling, no peeling, and no shedding; Level 3: The dry film had a small amount of bubbling, peeling, or even shedding; Level 4: The dry film had a large amount of shedding.

[0169] (9) Heat resistance test

[0170] Refer to IPC-TM650.2.6.8 standard. After the solder mask dry film is immersed in rosin flux for 30 seconds, it is vertically immersed in a tin furnace at a temperature of 288°C for 10 seconds, and repeated 3 times. Observe whether the surface is bubbling, discolored, or floating, and observe whether the dry film falls off by peeling off the 3M tape, and evaluate the changes in appearance based on the following criteria. The test results are graded as follows: Level 1: The dry film has no bubbling, peeling, or even falling off; Level 2: The dry film has a small amount of bubbling, no peeling, and no falling off; Level 3: The dry film has a small amount of bubbling, peeling, or even falling off; Level 4: The dry film has a large amount of falling off.

[0171] (10) Hardness test

[0172] Refer to the GB / T 6739-2006 test standard "Determination of film hardness by pencil method for paints and varnishes". Prepare the test samples using the same preparation method as in the HAST test, and perform hardness tests using pencils of different hardness.

[0173] The composition ratios of the solder resist dry films in the embodiments and comparative examples can be referred to Table 1, in parts by mass. The solder resist dry films obtained in the embodiments and comparative examples were subjected to the above-mentioned performance tests, and the performance test results are shown in Tables 2 and 3.

[0174] Table 1

[0175]

[0176]

[0177]

[0178] Table 2

[0179]

[0180]

[0181] Table 3

[0182]

[0183]

[0184] From the test results of the above embodiments and comparative examples, it can be seen that the photosensitive resin composition provided by the present invention can effectively reduce the CTE of the solder resist dry film, and significantly improve the heat resistance, hardness, HAST, acid resistance, alkali resistance and solvent resistance, which can meet the needs of IC substrates, and has good alkali developability and high analytical performance. In addition, the addition of epoxy-based glass polymer prepolymer can avoid cracking, warping and wrinkling of the solder resist dry film after light and heat curing, making its comprehensive performance better.

[0185] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A photosensitive resin composition, characterized in that The photosensitive resin composition comprises, by weight, 100 to 120 parts of alkali-soluble resin, 5 to 25 parts of photopolymerizable monomers, 1 to 7 parts of photoinitiators, 10 to 30 parts of epoxy resins, 3 to 15 parts of epoxy-based glass polymer prepolymers, and 1 to 5 parts of curing agents and accelerators thereof.

2. The photosensitive resin composition according to claim 1, characterized in that The epoxy-based glass polymer prepolymer is 5 to 10 parts by mass; and / or the epoxy-based glass polymer prepolymer is a prepolymer having a dynamic cross-linked network structure formed by the reaction of a glycidyl compound and a carboxylic acid compound, and has an intramolecular hydrogen bond structure formed by the association of a β-hydroxyl group and an ester group as shown in Formula 1:

3. The photosensitive resin composition according to claim 2, characterized in that: The glycidyl compound has a cyclic structure containing at least four atoms, and the glycidyl compound also contains at least two epoxy groups; preferably, the glycidyl compound is selected from at least one of bisphenol A diglycidyl ether, magnolol glycidyl ether, resorcinol diglycidyl ether, bisphenol F diglycidyl ether, cardanol glycidyl ether, terephthalic acid diglycidyl ester, tetrahydrophthalic acid diglycidyl ester, hexahydrophthalic acid diglycidyl ester, isocyanuric acid triglycidyl ester, 1,2-cyclohexanedicarboxylic acid diglycidyl ester, and 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester.

4. The photosensitive resin composition according to claim 2 or 3, characterized in that: The carboxylic acid compound contains at least two carboxyl groups, and the adjacent group of at least one carboxyl group is a hydroxyl group; preferably, the carboxylic acid compound is selected from at least one of 2-hydroxysuccinic acid and 2,3-hydroxysuccinic acid.

5. The photosensitive resin composition according to any one of claims 1 to 3, characterized in that: The mass ratio of the epoxy resin to the epoxy-based glass polymer prepolymer is (1-5):1; and / or, in terms of mass fractions, the epoxy resin is 15-25 parts; and / or, the epoxy resin contains at least two functional groups and has a cyclic structure; preferably, the epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, hydrogenated bisphenol A epoxy resin, phenolic epoxy resin, alicyclic epoxy resin, hydantoin epoxy resin, and imide epoxy resin.

6. The photosensitive resin composition according to any one of claims 1 to 3, characterized in that: The alkali-soluble resin is an epoxy acrylic resin containing a carboxyl group; preferably, the alkali-soluble resin is an epoxy acrylic resin containing a carboxyl group and having a rigid chemical structure; preferably, the alkali-soluble resin includes an epoxy acrylic resin containing a polycyclic structure on the main chain or the side chain; preferably, the alkali-soluble resin is selected from at least one of bisphenol A epoxy acrylic resin, alicyclic epoxy acrylic resin, and phenolic epoxy acrylic resin; and / or, the photopolymerizable monomer is 7 to 15 parts by mass; and / or, the photopolymerizable monomer includes a monofunctional acrylate and a polyfunctional acrylate; preferably, the monofunctional acrylate has a cyclic structure; further preferably, the monofunctional acrylate is selected from tetrahydrofuran acrylate, 2-phenoxyethyl acrylate, cycloaliphatic acrylate, (4) ethoxylated nonylphenol acrylate, isobornyl acrylate, tris(2-hydroxyethyl)acrylate, At least one of hydroxymethylpropane formal acrylate, alkoxylated phenol acrylate, alkoxylated tetrahydrofuran acrylate, and alkoxylated nonylphenol acrylate; preferably, the multifunctional acrylate includes acrylates with a functionality of 2 to 6; further preferably, the multifunctional acrylate is selected from at least one of pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, ethoxylated pentaerythritol tetraacrylate, dipentaerythritol acrylate, trimethylolpropane acrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, (3) ethoxylated trimethylolpropane triacrylate, pentaerythritol triacrylate, ethoxylated trimethylolpropane triacrylate, (3) propoxylated trimethylolpropane triacrylate, and (6) ethoxylated trimethylolpropane triacrylate; preferably, the mass ratio of the monofunctional acrylate to the multifunctional acrylate is (0.3 to 0.5): 1; and / or, in terms of mass fractions, the photoinitiator is 2 to 4 parts, and the curing agent and its accelerator are 1 to 3 parts; and / or, the photoinitiator includes a free radical photoinitiator and / or a cationic photoinitiator; preferably, the free radical photoinitiator is selected from 2,4,6-trimethylbenzoyldiphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, 2-isopropylthioxanthone, 1-hydroxycyclohexylphenyl ketone, benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, tetramethyl Michler's ketone, tetraethyl Michler's ketone, 2-chlorothioxanthone, 1-chloro- At least one of 4-propoxythioxanthone, 2,4-diethylthioxanthone, benzoin dimethyl ether, 2-hydroxy-methylphenylpropane-1-one, ethyl 4-(N,N-dimethylamino)benzoate, and 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone; the cationic photoinitiator is selected from triphenylsulfonium hexafluorophosphate, 4-phenylthiophenyl diphenylsulfonium salt, 4-dodecyloxyphenyl diphenylsulfonium hexafluoroantimonate, bis[(4-diphenylsulfonium)benzene] sulfide-bis-hexafluorophosphate, 4-phenylthiophenyl diphenylsulfonium salt, (4-hydroxyphenyl)methyl (benzyl) hexasulfonium fluorophosphate, 4-acetoxyphenyl dimethylsulfonium hexafluoroantimonate. salt, diphenyliodonium hexafluorophosphate; and / or, the curing agent includes at least one of an amine curing agent, a boron amine salt curing agent, a boron amine complex curing agent, an acid anhydride curing agent, a linear phenolic resin curing agent, a polyester resin curing agent, a polysulfide rubber curing agent, and an imidazole curing agent; and / or, the accelerator includes at least one of an electrophilic accelerator, a nucleophilic accelerator, and a metal carboxylate accelerator; preferably, the curing agent is selected from 2-methylimidazole, 2-ethylimidazole, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl disulfide, 3-aminobenzylamine, m-phenylenediamine, 3-amino-5-mercapto-1,2,4-triazole, 4-amino-3-hydrazino-5-mercapto -1,2,4-triazole, 1,3-bis(2,4,6-trimethylphenyl)imidazole chloride, 1-tritylimidazole, 4-imidazole-1-phenylpropiotone, 1-ethyl-3-methylimidazole tetrafluoroborate, 1-ethylimidazole, 1-allylimidazole, 2,4,5-triphenylimidazole, melamine, melamine phosphate, melamine phosphate, trichloromelamine, hexamethylol melamine, 1,8-diazabicyclo[5,4,0]dodec-7-ene, 4-cyanobenzylamine, 4,4'-diaminodiphenyl sulfone, 1-ethyl-3-methylimidazolium dicyanamide, 1-butyl-3-methylimidazolium dicyanamide, adipic acid dihydrazide, sebacic acid dihydrazide, at least one of triphenylphosphine. .

7. A solder resist dry film, characterized in that: The solder resist dry film is obtained by mixing and drying the photosensitive resin composition according to any one of claims 1 to 6.

8. A photosensitive laminate, characterized in that: It comprises a supporting layer, a photosensitive layer and a protective layer which are stacked, and the photosensitive layer is the solder resist dry film according to claim 7.

9. A solder resist pattern, characterized in that: The solder resist pattern is formed by sequentially exposing, developing and curing the solder resist dry film according to claim 7.

10. A semiconductor package carrier, characterized in that: The invention comprises a solder resist pattern, wherein the solder resist pattern is obtained by mixing and curing the photosensitive resin composition according to any one of claims 1 to 6, or the solder resist pattern is the solder resist pattern according to claim 9.

Citation Information

Patent Citations

  • Cyclic carbonate group-terminated polyurethane prepolymer and preparation method and application thereof

    CN112011029A

  • Photosensitive resin composition, solder resist dry film, solder resist layer and printed circuit board

    CN118363265A

Cited By

  • Self-repairing invisible car cover and preparation method thereof

    CN119592246A

  • Photosensitive dry film and preparation method and application thereof

    CN119916642A

  • Photosensitive dry film, method for preparing the same, and use thereof

    CN119916642B

  • Developing photoresist-removing alkali-soluble photoresist and preparation method thereof

    CN120255278A

  • A method for developing a photoresist which is alkali-soluble after removal of a photoresist

    CN120255278B