Modified positive electrode material and preparation method and application thereof

By using inert metal and low-priced anionic elements in the positive electrode material of sodium ion battery, the problem of irreversible phase change in the material during charge and discharge is solved, and the electrochemical performance and structural stability are significantly improved.

CN119008913APending Publication Date: 2024-11-22LANGFANG GREEN IND TECH CENT +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411315712.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing sodium ion battery positive electrode materials are prone to irreversible phase change during charging and discharging, resulting in structural instability and affecting electrochemical performance.

Method used

The sodium-based positive electrode material matrix containing transition metal elements is multi-site doping and substituting the matrix of transition metal elements by inert metal elements. Through the interaction between the doping elements and the matrix elements, irreversible phase change is suppressed and the stability of the material structure is improved. .

Benefits of technology

The electrochemical performance of the positive electrode material is significantly improved, including reversible capacity, cycling performance and rate performance, ensuring the stability of the material over a wide voltage range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008913A_ABST
    Figure CN119008913A_ABST
Patent Text Reader

Abstract

The invention relates to a modified positive electrode material and a preparation method and application thereof, the modified positive electrode material comprises a sodium-based positive electrode material matrix and a doping element doped in the sodium-based positive electrode material matrix, the sodium-based positive electrode material matrix comprises a layered oxide containing transition metal elements, the doping elements comprise inert metal elements and low-valence anion elements; the inert metal element comprises any one or a combination of at least two of Li, K, Ca, Cr, Mg, Ti, Zn, Al or Ag, and the low-valence anion element comprises any one or a combination of at least two of F, Cl or S. According to the invention, inert metal elements and low-valence anion elements are adopted to jointly perform multi-site doping substitution on a sodium-based positive electrode material matrix, and interaction between doping elements and matrix elements is utilized to jointly inhibit irreversible phase change in the modified positive electrode material and improve the stability of the material structure; therefore, the electrochemical performance of the material is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a modified positive electrode material and a preparation method and application thereof. Background Art

[0002] In recent years, with the continuous mining of lithium, the price of lithium-ion batteries has continued to rise, and the energy market has faced a new round of development trends. Research on sodium-ion batteries has been put back on the agenda. Sodium is abundant in the earth's crust and has great cost advantages. In addition, sodium-ion batteries also have advantages such as a large operating temperature range, good low-temperature adaptability, and higher safety.

[0003] The selection of appropriate cathode materials is the key to determining the capacity and rate performance of sodium-ion batteries. Currently, the three mainstream cathode materials for sodium-ion batteries on the market include transition metal oxides, Prussian blue analogs, and polyanion materials. a MeO2, Me = Fe, Ni, Co, Mn and their combinations), is a triangular prism crystal composed of alternating transition metal layers and alkali metal layers. Its open two-dimensional sodium ion diffusion channel and low Na + The diffusion energy barrier enables it to have a high sodium ion insertion and extraction speed. In addition, this type of positive electrode material also has the advantages of high reversible specific capacity, high energy density, high rate performance, easy technology conversion and high average working potential. Similar to O3-type layered transition metal oxide materials, due to the larger radius of Na + Migration will cause the slip of the oxygen layer, and the P2-type layered structure will also undergo an irreversible phase change under high pressure, resulting in low electrochemical stability of the material; in addition, due to the change in the concentration of sodium ions during the charge and discharge process, Na + / Hole structure rearrangement, resulting in superlattice phase, causing phase structure transformation. This leads to unsatisfactory performance of P2-type layered structure materials in terms of working voltage and structural stability in practical applications and electrochemical tests.

[0004] At present, by implementing strategies such as multi-element doping and substitution, not only can the capacity performance of the material be improved, but also the occurrence of phase change phenomena can be effectively curbed, the cycle stability of the material can be improved, and the activity of anion redox reactions can be stimulated, thereby greatly broadening the voltage operation window of the positive electrode material.

[0005] CN117613255A discloses a layered oxide positive electrode material, a sodium ion battery and a preparation method. The chemical formula of the layered oxide positive electrode material is Na x M y Me zO₂, where 0.8 ≤ x ≤ 1.1, M is selected from one or more elements of Group IA and Group IIA elements, 0 ≤ y ≤ 1, Me is selected from one or more metal elements, and 0 < z ≤ 1. Through a certain element doping, this technical solution can effectively improve the structural stability of the layered oxide cathode material, and increase the reversible capacity and cycle life.

[0006] CN115224254A discloses a Cu, Zn and Mg co-doped layered oxide sodium-ion battery cathode material, its preparation method and application. The chemical formula of the sodium-ion battery cathode material is Na 0.66+2z Ni 0.33-x-y Cu x Zn y Mn 0.67- z Mg z O₂, where 0 < x ≤ 0.1, 0 < y ≤ 0.05, 0 < z ≤ 0.2. Through the cation co-doping strategy, this technical solution enables the cathode material to remain in the P2-phase structure even at a relatively high sodium content, having a high capacity, average discharge voltage, energy density, and good cycle stability.

[0007] CN116259743A discloses a titanium-doped sodium-ion battery cathode layered oxide material, its preparation method and application. The general chemical formula of the titanium-doped sodium-ion battery cathode layered oxide material is Na x Ni (1-y) / 2 Mn (1-y) / 2 Ti y O₂, where 0.7 ≤ x < 1, 0.01 ≤ y < 0.3. By doping tetravalent titanium into NaNi 0.5 Mn 0.5 O₂ and increasing the content of Mn 3+ , Ti 4+ expands the spacing of the sodium layer, inhibits the occurrence of irreversible phase transformation, and improves the structural stability of the material.

[0008] Although the above solutions are modified by element doping, improving the structural stability of the layered oxide cathode material and increasing the reversible capacity and cycle life of the cathode material, with the progress of the charge and discharge process, the element doping at a single Me site will face the problem that the doped element detaches from the original doping site, resulting in interlayer structure slip and Na + / vacancy ordered arrangement, causing irreversible phase transformation of the material structure. The cycle stability of sodium-ion batteries needs to be further improved.

[0009] Therefore, developing a cathode material that can inhibit the irreversible phase transformation inside the material and stabilize the material structure through the synergistic effect between elements, thereby improving the electrochemical performance of the cathode material, has become an urgent technical problem to be solved currently. Summary of the invention

[0010] In order to solve the above technical problems, the purpose of the present invention is to provide a modified positive electrode material and its preparation method and application. The present invention adopts inert metal elements and low-valent anion elements to perform multi-site doping substitution on the matrix of sodium-based positive electrode materials containing transition metal elements, and utilizes the interaction between the doping elements and the matrix elements to jointly inhibit the irreversible phase change inside the modified positive electrode material and improve the stability of the material structure, thereby significantly improving the electrochemical performance of the material.

[0011] To achieve this object, the present invention adopts the following technical solutions:

[0012] In a first aspect, the present invention provides a modified positive electrode material, the modified positive electrode material comprising a sodium-based positive electrode material matrix and a doping element doped in the sodium-based positive electrode material matrix, the sodium-based positive electrode material matrix comprising a layered oxide containing a transition metal element, the doping element comprising an inert metal element and a low-valent anion element;

[0013] The inert metal element includes any one of Li, K, Ca, Cr, Mg, Ti, Zn, Al or Ag or a combination of at least two thereof, and the low-valent anion element includes any one of F, Cl or S or a combination of at least two thereof.

[0014] The modified positive electrode material provided by the present invention in situ dopes inert metal elements and low-valent anion elements into a sodium-based positive electrode material matrix containing transition metal oxides, introduces electrochemically inert metal elements such as Li, K, Ca, Cr, Mg, Ti, Zn, Al or Ag, and can be doped into the sodium layer and / or transition metal layer of the sodium-based positive electrode material matrix due to its suitable ionic radius, effectively maintains the interlayer spacing in the matrix, and further promotes the reversible migration of the inert doping element L between the transition metal layer and the sodium layer in the matrix, thereby inhibiting the O between adjacent oxygen layers. 2- -O 2- Electrostatic repulsion is used to suppress the irreversible phase transition of the sodium-based cathode material matrix and the Na + / The formation of an ordered vacancy structure stabilizes the structure of the modified positive electrode material, thereby improving the reversible capacity, cycle performance and rate performance of the positive electrode material.

[0015] Among the inert metal doping elements introduced into the modified positive electrode material of the present invention, large-sized K, Ca or Ag have a higher diffusion barrier, and their mobility remains unchanged during the charge and discharge process, which is riveted to the Na in the positive electrode material matrix. + site, can contribute more Na + vacancies, reducing the strength of the Na-O bond and Na + / Vacancy formation energy, favoring more Na+ delithiation and maintain the cation content in the sodium layer, thereby improving the rate performance of the modified cathode material; and inert metal elements with small ionic radius can replace the transition metal elements in the transition metal layer of the sodium-based cathode material matrix, which can effectively inhibit the + ordering of Na

[0016] / vacancies and charge ordering, thereby inhibiting the slip of the transition metal layer, preventing phase transformation of the cathode material, and improving the structural stability of the cathode material. At the same time, the low-valent anion elements in the doping elements can partially replace O in the sodium-based cathode material matrix, promoting oxygen to participate in the redox reaction, thereby increasing the average valence state of the oxygen layer, and being able to expand the interlayer spacing and reduce the band gap, thereby accelerating the charge transfer kinetics; and there is a strong interaction between the transition metal elements and the introduced low-valent anion elements with strong electronegativity, which can inhibit the dissolution of the transition metal elements in the discharged state and promote the reversible conversion of the low-valent transition metal elements to the high-valent transition metal elements in the charged state, having a higher oxygen vacancy formation energy, effectively inhibiting the irreversible oxygen evolution, thereby increasing the + diffusion rate of Na and inhibiting the lattice distortion caused by the Jahn-Teller effect. This continuous cation presence and increased anion valence state together alleviate the increase in O 2- -O 2- repulsion during the sodium extraction process, enabling the cathode material to maintain a stable pure-phase structure within a wide voltage range.

[0017] In the present invention, an inert metal element and a low-valent anion element are used to perform multi-site substitution on the sodium-based cathode material matrix containing transition metal elements, and the interaction between the doping elements and the elements in the matrix elements is utilized to jointly inhibit the irreversible phase transformation inside the modified cathode material and improve the structural stability of the material, thereby further enhancing the electrochemical performance of the material.

[0018] Preferably, the chemical general formula of the modified cathode material is Na a-x N x Me 1-y L y O 2-z Q z , 0 < a ≤ 1, 0 ≤ x < 1, x < a, 0 ≤ y < 1, 0 < z < 2, x and y are not both 0, Me is a transition metal element, N, L, and Q are doping elements, wherein the doping element N and the doping element L are the inert metal elements, and the doping element Q is the low-valent anion element.

[0019] Specifically, in the present invention, a can be 0.01, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.5, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95 or 1.00, etc.; x can be 0, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.5, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, y can be 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.5, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95 or 0.99, etc., and z can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 1.99, etc.

[0020] In the modified positive electrode material provided by the present invention, the doping element N partially replaces the sodium site in the sodium-based positive electrode material matrix, the doping element L partially replaces the transition metal element site in the sodium-based positive electrode material matrix, and the doping element Q partially replaces the oxygen site in the sodium-based positive electrode material matrix.

[0021] Preferably, the doping element N and the doping element L are different inert metal elements.

[0022] Preferably, the modified positive electrode material is a P2 type layered structure.

[0023] Preferably, 0.5 <a≤1,0<x≤0.5,0<y≤0.5,0<z≤0.5。

[0024] In the modified positive electrode material provided by the present invention, it is further preferred to simultaneously replace the Na site, Me site and O site of the sodium-based positive electrode material matrix with doping elements N, L and Q. Through the synergistic effect of the three doping elements on the multiple sites of the matrix material, the interaction between the doping elements and the matrix elements is fully utilized, thereby forming a modified positive electrode material with no phase change characteristics, and obtaining a more stable layered structure, so that the capacity performance, cycle performance and thermal stability of the battery using the modified positive electrode material are more significantly improved.

[0025] Meanwhile, the modified cathode material of the present invention is further preferably of the P2-type structure (a ≤ 0.7). Compared with the modified cathode material of the O3-type configuration (0.7 < a ≤ 1), the present invention dopes in the cathode material of the P2-type structure. The P2-type material has less Na content, and Na + The migration path is the open trigonal prism position, which has a larger diffusion space and a low diffusion energy barrier. Therefore, doping large-sized elements at the Na sites of the P2-type layered oxide material can better maintain the Na layer spacing without affecting Na + migration, which is beneficial to more Na + insertion and extraction, and inhibits the inherent P2-O2 phase transition of the P2-type layered oxide material caused by the O 2- -O 2- electrostatic repulsion in the over-sodium extraction state, making the material exhibit higher reversible capacity and rate performance.

[0026] Preferably, 0.5 < a ≤ 1, 0.01 ≤ x ≤ 0.2, 0.01 ≤ y ≤ 0.2, 0.01 ≤ z ≤ 0.2.

[0027] The present invention further optimizes the doping content of each doping element. Excessive doping elements will destroy the stable crystal structure of the material itself, and the optimized lattice parameters will be excessively changed. At the same time, excessive doping elements will interfere with the diffusion path of sodium ions, affect the insertion and extraction channels of sodium ions, cause their transmission to be blocked, and are more likely to undergo structural collapse during charge and discharge, showing poor electrochemical performance.

[0028] Preferably, in the modified cathode material, the molar ratio of the doping element N, the doping element L, and the doping element Q is (4 - 6):(9 - 12):(7 - 9), where the selection range of the doping element N is "4 - 6", such as 4, 4.5, 5, 5.5, or 6, etc.; the selection range of the doping element L is "9 - 12", such as 9, 9.5, 10, 10.5, 11, 11.5, or 12, etc.; the selection range of the doping element Q is "7 - 9", such as 7, 7.5, 8, 8.5, or 9, etc.

[0029] Preferably, the transition metal element Me includes any one or at least two combinations of Ni, Mn, Fe, Co, or V, further preferably Ni and / or Mn, and further preferably Ni and Mn.

[0030] Preferably, when the transition metal element Me includes Ni and Mn, the molar ratio of Ni to Mn is (0.1-0.4):(0.5-0.8), wherein the range of Ni can be selected from "0.1-0.4", such as 0.1, 0.11, 0.13, 0.15, 0.17, 0.19, 0.21, 0.23, 0.25, 0.27, 0.29, 0.31, 0.33, 0. 35, 0.37, 0.39 or 0.4, etc., Mn can be selected in the range of "0.5-0.8", for example, 0.5, 0.51, 0.53, 0.55, 0.57, 0.59, 0.61, 0.63, 0.65, 0.67, 0.69, 0.71, 0.73, 0.75, 0.77, 0.79 or 0.8, etc., preferably (0.2-0.3):(0.6-0.7).

[0031] Preferably, the doping element N includes any one of K, Ca or Ag or a combination of at least two thereof, preferably K.

[0032] The modified positive electrode material provided by the present invention further optimizes the type of doping elements in the sodium layer and uses K to replace the sodium position. + (152 μm) has a six-coordinate crystallographic ionic radius and is smaller than Na + Larger ionic radius and same valence, will not replace too much Na + , which can be riveted to the modified positive electrode material layered structure of Na + site, and the K element has a large ionic radius, which can effectively widen the interlayer spacing, thereby inhibiting the occurrence of irreversible phase change of the modified positive electrode material and stabilizing the structure of the positive electrode material; in addition, K + The presence of can also make the doping element L exist stably in the transition metal Me layer, and improve the reversibility of the migration of the doping element L between the transition metal Me layer and the Na layer.

[0033] Preferably, the doping element L includes any one of Li, Zn, Mg, Cr, Al or Ti, or a combination of at least two thereof, preferably Li.

[0034] The modified positive electrode material provided by the present invention further optimizes the type of doping elements at the transition metal layer site, uses Li to replace the transition metal site, and has a smaller ion radius ratio between Li and the transition metal element, which not only effectively suppresses the Na + / Vacancy ordering and charge ordering, as well as promoting relatively reversible migration behavior between the transition metal layer and the Na layer under high pressure, inhibiting the slip of the transition metal layer, resulting in the material's phase-change-free characteristics and improving the stability of the structure. In addition, Li +The presence of can also induce some anions to participate in the redox reaction, activate the anions in the matrix material for redox, and increase the initial sodium content of the material.

[0035] Preferably, the doping element Q includes F.

[0036] The modified positive electrode material provided by the present invention further optimizes the type of doping elements at the oxygen layer site, and adopts F to replace the oxygen site. F can not only dope at the O site to increase the average oxidation state in the O layer, change the crystal structure, electronic structure and ion transport performance of the electrode, but also - Ionic radius and O 2- Similar, oxidation state higher than O 2- , which can enhance the reversibility of anion reactions and inhibit oxygen evolution, improving the structural stability and electrochemical properties of the material.

[0037] In a second aspect, the present invention provides a method for preparing the modified positive electrode material as described in the first aspect, the preparation method comprising:

[0038] In situ mixing a sodium source, a transition metal Me source and a dopant containing a doping element to obtain the modified positive electrode material; the doping element includes an inert metal element and a low-valent anion element;

[0039] The inert metal element includes any one of Li, K, Ca, Cr, Mg, Ti, Zn, Al or Ag or a combination of at least two thereof, and the low-valent anion element includes any one of F, Cl or S or a combination of at least two thereof.

[0040] The preparation method provided by the present invention is simple to operate, has a short process, and is evenly mixed, and is easy to evenly and quantitatively incorporate some trace elements to achieve uniform doping at the molecular level of the matrix positive electrode material, thereby effectively inhibiting the reversible phase change inside the material and improving the stability of the material structure, thereby obtaining a modified positive electrode material with excellent performance. The preparation method has strong repeatability and is suitable for industrial large-scale production.

[0041] Preferably, the in-situ mixing method includes any one of a sol-gel method, a solid phase reaction method or a co-precipitation method, preferably a sol-gel method.

[0042] The present invention preferably adopts the sol-gel method to prepare the modified positive electrode material, which can adjust the content of each doping element and regulate the composition of the positive electrode material to achieve the best performance.

[0043] Preferably, the sol-gel method for preparing the modified positive electrode material comprises the following steps:

[0044] A sodium source, a transition metal Me source, a dopant containing a doping element and a solvent are subjected to a first mixing to obtain a mixed solution. Then, the mixed solution is subjected to a second mixing with a complexing agent accompanied by heating to obtain a wet gel. After drying the wet gel, it is calcined to obtain the modified cathode material.

[0045] In the present invention, it is possible to first mix the complexing agent and the solvent to prepare a complexing agent solution, and then perform a second mixing of the complexing agent solution with the mixed solution.

[0046] Preferably, the dopant containing an inert metal element includes an N source and / or an L source.

[0047] Preferably, the dopant containing a low-valence anion element includes a Q source.

[0048] Preferably, the molar ratio of the sodium element in the sodium source to the transition metal element Me in the transition metal Me source is (0.03 - 1.1):(0 - 1), and does not include 0. Among them, the selection range of the sodium element is "0.03 - 1.1", such as 0.03, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0 or 1.1, etc. The selection range of the transition metal element is "0 - 1, and does not include 0", for example, 0.01, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1.0, etc., and is preferably (0.53 - 0.8):1.

[0049] In the present invention, during the process of preparing the modified cathode material, an excessive amount of sodium source needs to be added to compensate for the sodium loss during the subsequent high-temperature calcination process.

[0050] Preferably, in the first mixing process, the molar ratio of the transition metal element Me, the doping element N, the doping element L, and the doping element Q in the transition metal Me source, the N source, the L source, and the Q source is (1 - y):x:y:z, 0 ≤ x < 1, 0 ≤ y < 1, 0 < z < 2, x and y are not both 0, preferably 0 < x ≤ 0.5, 0 < y ≤ 0.5, 0 < z ≤ 0.5, and further preferably 0.01 ≤ x ≤ 0.2, 0.01 ≤ y ≤ 0.2, 0.01 ≤ z ≤ 0.2.

[0051] Specifically, in the present invention, x can be 0, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.5, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95 or 0.99, etc.; y can be 0, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0. 35, 0.40, 0.45, 0.5, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95 or 0.99, etc., and z can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 1.99, etc.

[0052] Preferably, in the first mixing process, the molar ratio of the doping element N, the doping element L and the doping element Q in the N source, the L source and the Q source is (4-6):(9-12):(7-9), wherein the selection range of the doping element N is "4-6", for example, 4, 4.5, 5, 5.5 or 6, etc., the selection range of the doping element L is "9-12", for example, 9, 9.5, 10, 10.5, 11, 11.5 or 12, etc., and the selection range of the doping element Q is "7-9", for example, 7, 7.5, 8, 8.5 or 9, etc.

[0053] Preferably, the ratio of the molar amount of the complexing agent to the total molar amount of all transition metal elements in the mixed solution is (0.5-5):1, for example, 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1 or 5:1, etc., preferably (0.8-1.2):1.

[0054] In the present invention, the “all transition metal elements” refers to the sum of the transition metal elements Me in the transition metal layer in the sodium-based positive electrode material matrix and the transition metal elements in the doping elements.

[0055] The present invention further optimizes the ratio of the molar amount of the complexing agent in the preparation process to the total molar amount of the transition metal elements in the mixed solution to optimize the amount of the complexing agent added, thereby ensuring the integrity and stability of the gel network, making the structure of the obtained modified positive electrode material stable, and improving the uniformity of the crystal structure and the particle size of the material, thereby improving the electrochemical performance of the material.

[0056] Preferably, the sodium source includes any one of sodium acetate, sodium fluoride, sodium carbonate, sodium nitrate or sodium hydroxide, or a combination of at least two thereof.

[0057] Preferably, the transition metal Me source includes any one of acetate, chloride, nitrate, sulfate or oxide containing the transition metal element Me, preferably acetate containing the transition metal element Me.

[0058] Preferably, the transition metal Me source includes any one of a nickel source, a manganese source, an iron source, a cobalt source or a vanadium source, or a combination of at least two thereof, more preferably a nickel source and / or a manganese source, and more preferably a nickel source and a manganese source.

[0059] Preferably, the molar ratio of the nickel element in the nickel source to the manganese element in the manganese source is (0.1-0.4):(0.5-0.8), wherein the nickel element can be selected in the range of "0.1-0.4", for example, 0.1, 0.11, 0.13, 0.15, 0.17, 0.19, 0.21, 0.23, 0.25, 0.27, 0.29, 0.31, 0.33, 0.35, 0. 37, 0.39 or 0.4, etc., and the manganese element can be selected in the range of "0.5-0.8", for example 0.5, 0.51, 0.53, 0.55, 0.57, 0.59, 0.61, 0.63, 0.65, 0.67, 0.69, 0.71, 0.73, 0.75, 0.77, 0.79 or 0.8, etc., preferably (0.2-0.3):(0.6-0.7).

[0060] Preferably, the nickel source includes any one of nickel acetate, nickel chloride, nickel nitrate, nickel sulfate or nickel oxide, or a combination of at least two thereof, preferably nickel acetate.

[0061] Preferably, the manganese source includes any one of manganese acetate, manganese chloride, manganese nitrate, manganese sulfate or manganese dioxide, or a combination of at least two thereof, preferably manganese acetate.

[0062] Preferably, the N source includes any one of acetate, chloride, nitrate, carbonate or hydroxide containing the doping element N, preferably acetate containing the doping element N.

[0063] Preferably, the N source includes any one of a potassium source, a calcium source or a silver source, or a combination of at least two of them, preferably a potassium source.

[0064] Preferably, the potassium source includes any one of potassium acetate, potassium chloride, potassium nitrate, potassium carbonate or potassium hydroxide, or a combination of at least two thereof, preferably potassium acetate.

[0065] Preferably, the L source includes any one of acetate, chloride, nitrate, carbonate or hydroxide containing the doping element L, preferably acetate containing the doping element L.

[0066] Preferably, the L source includes any one of a lithium source, a zinc source, a magnesium source, a chromium source, an aluminum source or a titanium source, or a combination of at least two thereof, preferably a lithium source.

[0067] Preferably, the lithium source includes any one of lithium acetate, lithium chloride, lithium nitrate, lithium carbonate or lithium hydroxide, or a combination of at least two thereof, preferably lithium acetate.

[0068] Preferably, the Q source includes any one of a sodium salt, an ammonium salt, a potassium salt or an acid containing the doping element Q, and is preferably a sodium source containing the doping element Q.

[0069] Preferably, the Q source includes any one of a fluorine source, a chlorine source or a sulfur source, or a combination of at least two of them, preferably a fluorine source.

[0070] Preferably, the fluorine source includes any one of sodium fluoride, ammonium fluoride, ammonium bifluoride, ammonium trifluoroacetate, potassium fluoride or hydrofluoric acid, or a combination of at least two thereof, preferably sodium fluoride.

[0071] In the present invention, sodium fluoride is further preferred, which can be used as a fluorine source to provide the doping element fluorine, and can also be used as a sodium source to provide the sodium element.

[0072] Preferably, the complexing agent is any one of citric acid, ethylene glycol or ethylenediaminetetraacetic acid (EDTA) or a combination of at least two thereof, more preferably citric acid.

[0073] Preferably, the rotation speeds of the first mixing and the second mixing are independently selected from 200-500 rpm, such as 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm or 500 rpm, etc., preferably 300-400 rpm.

[0074] Preferably, the heating temperature is 60-100°C, such as 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C, etc., preferably 75-85°C.

[0075] Preferably, the drying temperature is 120-180°C, such as 120°C, 130°C, 140°C, 150°C, 160°C, 170°C or 180°C, etc., preferably 140-160°C.

[0076] Preferably, the drying time is 4-10 h, such as 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h, etc., preferably 5-7 h.

[0077] Preferably, the calcination includes a first calcination stage and a second calcination stage.

[0078] Preferably, the heating rates of the first calcination stage and the second calcination stage are independently selected from 1-10°C / min, such as 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, etc., preferably 4-6°C / min.

[0079] Preferably, the temperature of the first calcination stage is 300-600°C, such as 300°C, 350°C, 400°C, 450°C, 500°C, 550°C or 600°C, etc., preferably 400-500°C.

[0080] Preferably, the time of the first calcination stage is 4-8 h, such as 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h or 8 h, etc., preferably 5-7 h.

[0081] Preferably, the temperature of the second calcination stage is 700-1100°C, such as 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C or 1100°C, etc., preferably 850-950°C.

[0082] Preferably, the second calcination stage lasts for 10-20 h, such as 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h or 20 h, etc., preferably 14-16 h.

[0083] Preferably, the calcination atmosphere is any one of air atmosphere, oxygen atmosphere or argon atmosphere, preferably air atmosphere.

[0084] In a third aspect, the present invention provides a sodium ion battery, comprising a positive electrode plate, an electrolyte, a separator and a negative electrode plate, wherein the positive electrode plate comprises the modified positive electrode material described in the first aspect.

[0085] The modified positive electrode material is used in the positive electrode plate of the sodium ion battery provided by the present invention, inert metal elements and low-valent anion elements are introduced into the positive electrode material of the sodium ion battery, and multi-site doping and substitution are performed on the positive electrode material matrix together, so as to suppress the irreversible phase change inside the positive electrode material and improve the structural stability of the positive electrode material, thereby further improving the capacity performance, cycle stability and rate performance of the sodium ion battery.

[0086] Preferably, the electrolyte comprises sodium salt, an organic solvent and an additive.

[0087] Preferably, the diaphragm comprises a glass fiber diaphragm.

[0088] Preferably, the sodium ion battery is prepared by the following preparation method, which comprises:

[0089] In a button-type battery shell, a positive electrode sheet, a separator and a negative electrode sheet are stacked in sequence and an electrolyte is added to obtain the sodium ion battery.

[0090] Preferably, the diameter of the negative electrode plate is 12-14 mm, such as 12 mm, 13 mm or 14 mm.

[0091] Preferably, the diameter of the diaphragm is 16-18 mm, such as 16 mm, 17 mm or 18 mm.

[0092] Preferably, the diameter of the positive electrode plate is 10-12 mm, such as 10 mm, 11 mm or 13 mm.

[0093] In a fourth aspect, the present invention provides a power device, wherein the power device comprises the modified positive electrode material as described in the first aspect, or the power device comprises the sodium ion battery as described in the third aspect.

[0094] Compared with the prior art, the present invention has at least the following beneficial effects:

[0095] (1) The modified positive electrode material provided by the present invention in situ dopes inert metal elements and low-valent anion elements into a sodium-based positive electrode material matrix containing transition metal oxides. The introduction of inert metal doping elements can stabilize the Na layer in the matrix material and inhibit the slip of the transition metal layer in the matrix material. Under high pressure conditions, it can exhibit relatively reversible migration behavior between the transition metal layer and the Na layer in the sodium-based positive electrode material matrix, stabilize the structure of the material, and inhibit the occurrence of irreversible phase changes within the material. At the same time, the introduced low-valent anion elements partially replace the O in the sodium-based positive electrode material matrix, promote oxygen to participate in the redox reaction, thereby increasing the average valence state of the oxygen layer, expanding the interlayer spacing and reducing the band gap, thereby accelerating the charge transfer kinetics; and the strong electronegative low-valent anion elements used have a strong interaction with the transition metal elements, inhibiting the dissolution of the transition metal elements, increasing the oxygen vacancy formation energy, and reducing the irreversible oxygen evolution in the material, thereby improving the Na + The diffusion rate can be reduced and the lattice distortion caused by the Jahn-Teller effect can be suppressed.

[0096] (2) In the modified positive electrode material provided by the present invention, it is further preferred to partially replace the sodium sites in the sodium-based positive electrode material matrix with the doping element N, partially replace the transition metal element sites with the doping element L, and partially replace the oxygen sites with the doping element Q. Through the synergistic effect of the three doping elements on the multiple sites of the matrix material, the interaction between the doping elements and the matrix elements is fully utilized, thereby forming a modified positive electrode material with no phase change characteristics, and obtaining a more stable layered structure, so that the electrochemical performance of the modified positive electrode material is more significantly improved.

[0097] (3) The preparation method provided by the present invention is simple to operate, has a short process, and is evenly mixed, and is easy to evenly and quantitatively incorporate some trace elements to achieve uniform doping at the molecular level of the matrix positive electrode material, thereby effectively inhibiting the reversible phase change inside the material and improving the stability of the material structure, thereby obtaining a modified positive electrode material with excellent performance. The preparation method has strong repeatability and is suitable for industrial large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0098] Figure 1 This is a schematic diagram of the structure of the modified positive electrode material provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0099] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0100] Example 1

[0101] This embodiment provides a modified positive electrode material of a P2-type layered structure, including a sodium-based positive electrode material matrix and a doping element doped in the sodium-based positive electrode material matrix, wherein the sodium-based positive electrode material matrix is ​​a layered structure containing a transition metal oxide, and the chemical formula of the modified positive electrode material is Na 0.62 K 0.05 Ni 0.23 Li 0.1 Mn 0.67 O 1.93 F 0.07 , K element is doped to replace the sodium site of the matrix material, Li element is doped to replace the transition metal site of the matrix material, and F element is doped to replace the oxygen site of the matrix material. The molar ratio of the doping elements K, Li and F is 5:10:7.

[0102] This embodiment also provides a method for preparing the modified positive electrode material, which comprises the following steps:

[0103] (1) dissolving anhydrous sodium acetate (CH3COONa), anhydrous potassium acetate (CH3COOK), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), anhydrous lithium acetate (CH3COOLi), manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) and sodium fluoride (NaF) (Na in excess to compensate for Na loss during calcination) in a molar ratio of 0.60:0.05:0.23:0.1:0.67:0.07 in 50 ml of deionized water, stirring magnetically at a rotation speed of 400 rpm for 30 min, and mixing uniformly to obtain a mixed solution;

[0104] (2) dissolving anhydrous citric acid in 50 ml of deionized water, stirring magnetically at a speed of 400 rpm for 30 min, and mixing uniformly to obtain a citric acid solution. The mixed solution obtained in step (1) is mixed with the citric acid solution, wherein the ratio of the molar amount of anhydrous citric acid to the total molar amount of all transition metal elements in the mixed solution obtained in step (1) is 1:1. The mixture is heated in a water bath at 80° C. and stirred magnetically at a speed of 350 rpm for 4 h until a wet gel is formed. The wet gel is dried in an oven at 150° C. for 6 h to obtain a solid phase product.

[0105] (3) After the solid phase product obtained in step (1) is fully ground, it is incubated at 5°C min in air atmosphere. -1 The first calcination stage was carried out at 450 °C for 6 h, and then at 5 °C min -1 The second calcination stage was carried out at 900 °C for 15 h and then cooled to room temperature to obtain Na 0.62 K 0.05 Ni 0.23 Li 0.1 Mn 0.67 O 1.93 F 0.07 Modified positive electrode material.

[0106] Example 2

[0107] This embodiment provides a modified positive electrode material of a P2-type layered structure, including a sodium-based positive electrode material matrix and a doping element doped in the sodium-based positive electrode material matrix, wherein the sodium-based positive electrode material matrix is ​​a layered structure containing a transition metal oxide, and the chemical formula of the modified positive electrode material is Na 0.63 K 0.04 Ni 0.21 Li 0.12 Mn 0.67 O 1.91 F 0.09, K element is doped to replace the Na site of the matrix material, Li element is doped to replace the transition metal site of the matrix material, and F element is doped to replace the transition metal site of the matrix material. The molar ratio of the doping elements K, Li and F is 4:12:9.

[0108] This embodiment also provides a method for preparing the modified positive electrode material, which comprises the following steps:

[0109] (1) dissolving anhydrous sodium acetate (CH3COONa), anhydrous potassium acetate (CH3COOK), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), anhydrous lithium acetate (CH3COOLi), manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) and sodium fluoride (NaF) (Na in excess to compensate for Na loss during calcination) in a molar ratio of 0.59:0.04:0.21:0.12:0.67:0.09 in 50 ml of deionized water, stirring the mixture with a magnetic stirrer at a rotation speed of 300 rpm for 50 min, and mixing the mixture uniformly to obtain a mixed solution;

[0110] (2) dissolving anhydrous citric acid in 50 ml of deionized water, stirring magnetically at a speed of 400 rpm for 30 min, and mixing uniformly to obtain a citric acid solution. The mixed solution obtained in step (1) is mixed with the citric acid solution, wherein the ratio of the molar amount of anhydrous citric acid to the total molar amount of all transition metal elements in the mixed solution obtained in step (1) is 0.8:1. The mixture is heated in a water bath at 75° C. and stirred magnetically at a speed of 300 rpm for 4 h until a wet gel is formed. The wet gel is dried in an oven at 140° C. for 7 h to obtain a solid phase product.

[0111] (3) After the solid phase product obtained in step (1) is fully ground, it is incubated at 4°C min in air atmosphere. -1 The first calcination stage was carried out at 400 °C for 7 h, and then at 4 °C min -1 The second calcination stage was carried out at 850 °C for 16 h and then cooled to room temperature to obtain Na 0.63 K 0.04 Ni 0.21 Li 0.12 Mn 0.67 O 1.91 F 0.09 Modified positive electrode material.

[0112] Example 3

[0113] This embodiment provides a modified positive electrode material of a P2-type layered structure, including a sodium-based positive electrode material matrix and a doping element doped in the sodium-based positive electrode material matrix, wherein the sodium-based positive electrode material matrix is ​​a layered structure containing a transition metal oxide, and the chemical formula of the modified positive electrode material is Na0.61 K 0.06 Ni 0.24 Li 0.09 Mn 0.67 O 1.92 F 0.08 , K element is doped to replace the sodium site of the matrix material, Li element is doped to replace the transition metal site of the matrix material, and F element is doped to replace the oxygen site of the matrix material. The molar ratio of the doping elements K, Li and F is 6:9:8.

[0114] This embodiment also provides a method for preparing the modified positive electrode material, which comprises the following steps:

[0115] (1) dissolving anhydrous sodium acetate (CH3COONa), anhydrous potassium acetate (CH3COOK), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), anhydrous lithium acetate (CH3COOLi), manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) and sodium fluoride (NaF) (Na in excess to compensate for Na loss during calcination) in a molar ratio of 0.58:0.06:0.24:0.09:0.67:0.08 in 50 ml of deionized water, stirring magnetically at a rotation speed of 400 rpm for 30 min, and mixing uniformly to obtain a mixed solution;

[0116] (2) dissolving anhydrous citric acid in 50 ml of deionized water, stirring magnetically at a speed of 400 rpm for 30 min, and mixing uniformly to obtain a citric acid solution. The mixed solution obtained in step (1) is mixed with the citric acid solution, wherein the ratio of the molar amount of anhydrous citric acid to the total molar amount of all transition metal elements in the mixed solution obtained in step (1) is 1.2:1. The mixture is heated in a water bath at 85° C. and stirred magnetically at a speed of 400 rpm for 4 h until a wet gel is formed. The wet gel is dried in an oven at 160° C. for 5 h to obtain a solid phase product.

[0117] (3) After the solid phase product obtained in step (1) is fully ground, it is incubated at 6°C min in air atmosphere. -1 The first calcination stage was carried out at 500 °C for 5 h, and then at 6 °C min -1 The second calcination stage was carried out at 950°C for 14 h and then cooled to room temperature to obtain Na 0.61 K 0.06 Ni 0.24 Li 0.09 Mn 0.67 O 1.92 F 0.08 Modified positive electrode material.

[0118] Example 4

[0119] The difference between this embodiment and embodiment 1 is that the chemical formula of the modified positive electrode material provided in this embodiment is Na 0.67 Ni 0.23 Li 0.1 Mn 0.67 O 1.93 F 0.07 , the molar ratio of doping elements Li to F is 10:7. Accordingly, in the preparation method of this embodiment, anhydrous sodium acetate (CH3COONa), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), anhydrous lithium acetate (CH3COOLi), manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) and sodium fluoride (NaF) (Na is excessive to compensate for the loss of Na during calcination) in a molar ratio of 0.65:0.23:0.1:0.67:0.07 are dissolved in 50 ml of deionized water. The rest is the same as in Example 1.

[0120] Example 5

[0121] The difference between this embodiment and embodiment 1 is that the chemical formula of the modified positive electrode material provided in this embodiment is Na 0.62 K 0.05 Ni 0.33 Mn 0.67 O 1.93 F 0.07 , the molar ratio of doping element K to F is 5:7. Accordingly, in the preparation method of this embodiment, anhydrous sodium acetate (CH3COONa), anhydrous potassium acetate (CH3COOK), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) and sodium fluoride (NaF) (Na is excessive to compensate for the loss of Na during calcination) in a molar ratio of 0.60:0.05:0.33:0.67:0.07 are dissolved in 50 ml of deionized water. The rest is the same as in Example 1.

[0122] Example 6

[0123] The difference between this embodiment and embodiment 1 is that the chemical formula of the modified positive electrode material provided in this embodiment is Na 0.62 Ca 0.05 Ni 0.23 Li 0.1 Mn 0.67 O 1.93 F 0.07, the molar ratio of doping elements Ca, Li and F is 5:10:7. Accordingly, in the preparation method of this embodiment, anhydrous sodium acetate (CH3COONa), calcium acetate monohydrate (Ca(CH3COO)2·H2O), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), anhydrous lithium acetate (CH3COOLi), manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) and sodium fluoride (NaF) (Na is excessive to compensate for the loss of Na during calcination) in a molar ratio of 0.60:0.05:0.23:0.1:0.67:0.07 are dissolved in 50 ml of deionized water. The rest is the same as in Example 1.

[0124] Example 7

[0125] The difference between this embodiment and embodiment 1 is that the chemical formula of the modified positive electrode material provided in this embodiment is Na 0.62 K 0.05 Ni 0.23 Mg 0.1 Mn 0.67 O 1.93 F 0.07 , the molar ratio of doping elements K, Mg and F is 5:10:7. Accordingly, in the preparation method of this embodiment, anhydrous sodium acetate (CH3COONa), anhydrous potassium acetate (CH3COOK), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), magnesium acetate tetrahydrate (Mg(CH3COO)2·4H2O), manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) and sodium fluoride (NaF) (Na is excessive to compensate for the loss of Na during calcination) in a molar ratio of 0.60:0.05:0.23:0.1:0.67:0.07 are dissolved in 50 ml of deionized water. The rest is the same as in Example 1.

[0126] Example 8

[0127] The difference between this embodiment and embodiment 1 is that the chemical formula of the modified positive electrode material provided in this embodiment is Na 0.62 K 0.05 Ni 0.23 Li 0.1 Mn 0.67 O 1.93 Cl 0.07, the molar ratio of doping elements K, Li and Cl is 5:10:7. Accordingly, in the preparation method of this embodiment, anhydrous sodium acetate (CH3COONa), anhydrous potassium acetate (CH3COOK), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), anhydrous lithium acetate (CH3COOLi), manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) and sodium chloride (NaCl) (Na is excessive to compensate for the loss of Na during calcination) in a molar ratio of 0.60:0.05:0.23:0.1:0.67:0.07 are dissolved in 50 ml of deionized water. The rest is the same as in Example 1.

[0128] Example 9

[0129] The difference between this embodiment and embodiment 1 is that the chemical formula of the modified positive electrode material provided in this embodiment is Na 0.1 2K 0.5 Ni 0.1 Li 0.5 Mn 0.4 O 1.5 F 0.5, The molar ratio of doping elements K, Li and F is 50:50:50. The rest is the same as in Example 1.

[0130] Example 10

[0131] The difference between this embodiment and embodiment 1 is that: the preparation method of the modified positive electrode material provided in this embodiment is to dissolve sodium nitrate (NaNO3), potassium nitrate (KNO3), nickel nitrate (Ni(NO3)2), lithium nitrate (LiNO3), manganese nitrate (Mn(NO3)2) and sodium fluoride (NaF) (Na is excessive to compensate for the loss of Na during calcination) in a molar ratio of 0.60:0.05:0.23:0.1:0.67:0.07 in 50 ml of deionized water. The rest is the same as in embodiment 1.

[0132] Embodiment 11

[0133] The difference between this embodiment and embodiment 1 is that: the preparation method of the modified positive electrode material provided in this embodiment is to dissolve sodium chloride (NaCl), potassium chloride (KCl), nickel chloride (NiCl2), lithium chloride (LiCl), manganese chloride (MnCl2) and sodium fluoride (NaF) (Na is excessive to compensate for the loss of Na during calcination) in a molar ratio of 0.60:0.05:0.23:0.1:0.67:0.07 in 50 ml of deionized water. The rest is the same as in embodiment 1.

[0134] Example 12

[0135] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the calcination atmosphere is an argon atmosphere. The rest is the same as embodiment 1.

[0136] Example 13

[0137] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the calcination atmosphere is an oxygen atmosphere. The rest is the same as embodiment 1.

[0138] Embodiment 14

[0139] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the temperature of the first calcination stage is 300° C. The rest is the same as embodiment 1.

[0140] Embodiment 15

[0141] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the temperature of the first calcination stage is 600° C. The rest is the same as embodiment 1.

[0142] Example 16

[0143] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the temperature of the second calcination stage is 700° C. The rest is the same as embodiment 1.

[0144] Embodiment 17

[0145] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the temperature of the second calcination stage is 1100° C. The rest is the same as embodiment 1.

[0146] Embodiment 18

[0147] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the time of the second calcination stage is 10 hours. The rest is the same as embodiment 1.

[0148] Embodiment 19

[0149] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the time of the second calcination stage is 20 hours. The rest is the same as embodiment 1.

[0150] Embodiment 20

[0151] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the ratio of the molar amount of anhydrous citric acid to the total molar amount of the transition metal elements in the mixed solution is 0.5:1. The rest is the same as embodiment 1.

[0152] Embodiment 21

[0153] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the ratio of the molar amount of anhydrous citric acid to the total molar amount of the transition metal elements in the mixed solution is 1.5:1. The rest is the same as embodiment 1.

[0154] Embodiment 22

[0155] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified positive electrode material provided in this embodiment, the mixed solution is not prepared first, but anhydrous citric acid is directly mixed with the raw material and the solvent. The rest is the same as embodiment 1.

[0156] Comparative Example 1

[0157] The difference between this comparative example and Example 1 is that the chemical formula of the modified positive electrode material provided in this comparative example is Na 0.62 K 0.05 Ni 0.23 Li 0.1 Mn 0.67 O2, the molar ratio of doping element K to Li is 5:10. Accordingly, in the preparation method of this comparative example, anhydrous sodium acetate (CH3COONa) (Na is excessive to compensate for the loss of Na during calcination), anhydrous potassium acetate (CH3COOK), tetrahydrated nickel acetate (Ni(CH3COO)2·4H2O), anhydrous lithium acetate (CH3COOLi), and tetrahydrated manganese acetate (Mn(CH3COO)2·4H2O) with molar amounts of 0.67:0.05:0.23:0.1:0.67 are dissolved in 50 ml of deionized water. The rest is the same as Example 1.

[0158] Comparative Example 2

[0159] The difference between this comparative example and Example 1 is that the chemical formula of the modified positive electrode material provided in this comparative example is Na 0.62 K 0.05 Ni 0.33 Mn 0.67O2. Accordingly, in the preparation method of this comparative example, anhydrous sodium acetate (CH3COONa) (Na is excessive to compensate for the Na loss during calcination), anhydrous potassium acetate (CH3COOK), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), and manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) with molar weights of 0.67:0.05:0.33:0.67 are dissolved in 50 ml of deionized water. The rest is the same as in Example 1.

[0160] Comparative Example 3

[0161] The difference between this comparative example and Example 1 is that the chemical formula of the modified positive electrode material provided in this comparative example is Na 0.67 Ni 0.23 Li 0.1 Mn 0.67 O2. Accordingly, in the preparation method of this comparative example, anhydrous sodium acetate (CH3COONa) (Na is excessive to compensate for the Na loss during calcination), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), anhydrous lithium acetate (CH3COOLi), and manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) with molar weights of 0.72:0.23:0.1:0.67 are dissolved in 50 ml of deionized water. The rest is the same as in Example 1.

[0162] Comparative Example 4

[0163] The difference between this comparative example and Example 1 is that the chemical formula of the modified positive electrode material provided in this comparative example is Na 0.67 Ni 0.33 Mn 0.67 O 1.93 F 0.07 Accordingly, in the preparation method of this comparative example, anhydrous sodium acetate (CH3COONa), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) and sodium fluoride (NaF) (Na is excessive to compensate for the loss of Na during calcination) with molar weights of 0.65:0.33:0.67:0.07 were dissolved in 50 ml of deionized water. The rest was the same as in Example 1.

[0164] Comparative Example 5

[0165] The difference between this comparative example and Example 1 is that the chemical formula of the modified positive electrode material provided in this comparative example is Na 0.67 Ni 0.33 Mn 0.67O2. Accordingly, in the preparation method of this comparative example, anhydrous sodium acetate (CH3COONa) (Na is excessive to compensate for the Na loss during calcination), nickel acetate tetrahydrate (Ni(CH3COO)2·4H2O), and manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) are dissolved in 50 ml of deionized water according to a stoichiometric ratio of 0.72:0.33:0.67. The rest is the same as Example 1.

[0166] Application Example 1-22 and Comparative Application Example 1-5

[0167] The modified positive electrode material or positive electrode material provided in the above embodiments and comparative examples is used as the positive electrode active material of the positive electrode plate, and is stacked with the separator and the negative electrode plate layer into the electrolyte and placed in a 2032 button battery shell to assemble a button sodium ion battery. The specific components are as follows:

[0168] (1) Positive electrode sheet: The modified positive electrode material or positive electrode material obtained in the above embodiments and comparative examples is used as a positive electrode active material, and is uniformly mixed with polyvinylidene fluoride (PVDF) and superconducting carbon black in a mass ratio of 7:2:1, and N-methylpyrrolidone (NMP) is added to prepare a positive electrode slurry, which is uniformly coated on an aluminum foil, dried in a forced air dryer at 60° C. for 2 h, and then transferred to a vacuum dryer at 120° C. and dried for 12 h to obtain a positive electrode sheet with a diameter of 11 mm;

[0169] (2) Negative electrode: A metal sodium sheet is used as the negative electrode with a diameter of 13 mm;

[0170] (3) Diaphragm: Glass fiber diaphragm with a diameter of 17 mm;

[0171] (4) Electrolyte: 1 M NaClO4 was dissolved in propylene carbonate (PC), and 5 wt% fluoroethylene carbonate (FEC) was added as an additive.

[0172] The button-type sodium ion batteries provided in the above-mentioned application examples 1-22 and comparative application examples 1-5 were subjected to charge and discharge tests, and constant current charge and discharge were performed at a voltage range of 2.0-4.4V and a current density of 1C. The battery's first cycle discharge capacity and the discharge capacity after 300 cycles were tested, and the capacity retention rate was calculated.

[0173] The specific test results are shown in Table 1-5.

[0174] Table 1

[0175]

[0176]

[0177] Table 2

[0178]

[0179] Table 3

[0180]

[0181] Table 4

[0182]

[0183] Table 5

[0184]

[0185] From Tables 1 to 5, we can see that:

[0186] (1) It can be seen from Application Examples 1 to 3 that the present invention uses inert metal elements and low-valent anion elements to perform multi-site doping substitution on the sodium-based positive electrode material matrix containing transition metal elements, and utilizes the interaction between the doping elements and the matrix elements to jointly inhibit the irreversible phase change inside the modified positive electrode material and improve the stability of the material structure, thereby significantly improving the electrochemical performance of the material.

[0187] Depend on Figure 1 As shown, it can be seen that the doping elements K, Li, and F in the modified positive electrode material provided in Example 1 are respectively located at the Na site, Me site, and O site of the matrix material, and together maintain the interlayer spacing of the material.

[0188] (2) It can be seen from Application Examples 1 and 4-5 that if the modified positive electrode material of the present invention does not contain the doping element K, due to the lack of substitution of elements with large ionic radius at the Na site, the interlayer spacing of the alkali metal layer is small, which limits the Na + The insertion / extraction speed of the obtained material is poor, and the cycle performance is poor. If the doping element Li is not contained, due to the lack of doping of transition metal sites, the element types of the transition metal layer in the matrix material are small, and as the charge and discharge process proceeds, Na + / vacancy ordered structure, resulting in Na + The structure is rearranged under spatial interaction to form a superlattice structure, which restricts the Na + Moreover, due to the lack of Li-F bonds, the material will undergo irreversible phase transition under high pressure, resulting in poor battery cycling stability.

[0189] (3) It can be seen from Application Examples 1 and 6-8 that if Ca is used to replace Na sites in the modified positive electrode material of the present invention, although a larger interlayer spacing of the alkali metal layers can be provided by utilizing the steric effect, due to the Ca 2+ The higher ion valence reduces the overall capacity of the material and makes the substitution position of heterovalent metal ions more difficult to control.2+ Although replacing transition metal sites can also suppress the occurrence of irreversible phase transitions under high pressure, the use of Li + It can show relatively reversible migration behavior between the transition metal layer and the Na layer, inhibit the slip of the transition metal layer, and induce some anions to participate in the redox reaction, thereby increasing the initial sodium content of the material. 2+ The initial capacity of the replacement transition metal site is low, and the degree of improvement on the material stability is limited; if Cl is used to replace the O site, although the conductivity of the material can be improved, the material has better rate performance, but compared with F doping, the Cl-doped material still has Mn 2+ Dissolution in the discharge state and lattice distortion caused by the Jahn-Teller effect. In addition, Cl-containing compounds are corrosive and may react with other elements in the electrode, thus affecting the electrochemical properties of the material.

[0190] (4) It can be seen from Application Examples 1 and 9 that if the proportion of the doping content in the positive electrode material of the present invention is too high, the excessive doping elements will destroy the stable crystal structure of the material itself, and the optimized lattice parameters will be excessively changed. At the same time, the excessive doping elements will interfere with the diffusion path of sodium ions, affecting the embedding and extraction channels of sodium ions, thereby hindering their transmission. It is more likely to cause structural collapse during the charge and discharge process, showing poor electrochemical performance.

[0191] (5) It can be seen from Application Examples 1 and 10-11 that when the present invention uses the sol-gel method to prepare the positive electrode material, the acetate system has a stronger complexing ability than the nitrate system and the chloride system. The obtained positive electrode material has better crystallinity, more uniform material composition, and exhibits better electrochemical performance. In addition, compared with nitrate and chloride, acetate is less toxic and less polluting to the environment.

[0192] (6) It can be seen from Application Examples 1 and 12-13 that in the preparation method of the modified positive electrode material provided by the present invention, although O vacancies can be created in an argon atmosphere, Mn 3+ / Mn 4+ The redox potential of the positive electrode material is increased to stimulate its electrochemical activity, but the oxygen-deficient environment inhibits the redox activity of the anions, resulting in capacity loss; the positive electrode material can be fully oxidized in an oxygen atmosphere, but excessive oxygen supply will cause the transition metal Me ions of the matrix material to be over-oxidized to a high valence state and cause microcracks in the material. Under this effect, the positive electrode material calcined in an argon atmosphere and an oxygen atmosphere showed slightly inferior performance to that of the material in an air atmosphere, which shows that an appropriate amount of oxygen can be provided in an air atmosphere to promote the change of the oxidation state of the transition metal ions, thereby improving the cycle performance and cycle stability of the battery.

[0193] (7) It can be seen from Application Examples 1 and 14-15 that if the temperature of the first calcination stage of the present invention is too low, the thermal decomposition transformation of the solid phase product obtained in the preparation process cannot be maximized, the adsorbed water and crystallization water are not fully removed, the citric acid and acetate are not completely decomposed, and the doping elements cannot be fully diffused and evenly distributed, thereby affecting the electrochemical properties of the material; if the temperature of the first calcination stage is too high, it will cause excessive thermal decomposition of the solid phase product in the preparation process, trigger unnecessary chemical reactions, produce impurity phases, and also cause a certain element loss of the doping elements, affecting the electrochemical properties of the material.

[0194] (8) It can be seen from Application Examples 1 and 16-17 that if the temperature of the second calcination stage is too low, the crystallization of the modified positive electrode material obtained is not perfect, the distance between particles is large, and Na + The diffusion path is long, which affects the kinetic properties of the material and is prone to generate impurities, which is not conducive to the formation of a pure phase structure. The material exhibits a low initial capacity and poor cycle stability. If the temperature of the second calcination stage is too high, the inter-particle spacing of the modified material obtained is too small, and particles are prone to agglomeration, resulting in poor electrochemical performance of the modified positive electrode material.

[0195] (9) It can be seen from Application Examples 1 and 18-19 that if the second calcination stage of the present invention is too short, the crystallinity of the sample particles is poor, the capacity of the positive electrode material is low, and the structural stability is poor; if the second calcination stage is too long, it will lead to serious agglomeration, resulting in Na + During the embedding and de-embedding process, the structure collapses, the capacity decays rapidly, and the cycle performance deteriorates.

[0196] (10) It can be seen from Application Examples 1 and 20-21 that if the citric acid content of the present invention is too low, the gel network will be unstable and incomplete, resulting in a loose structure of the modified positive electrode material and poor cycle stability; if the citric acid content is too high, the gel network will be too dense, so that the crystal growth of the modified positive electrode material is restricted, and it is difficult to form a uniform crystal structure during the subsequent heat treatment process, resulting in uneven particle size and increased grain boundaries. At the same time, the pore structure of the material is overfilled, affecting the Na + The storage sites and migration channels of the materials affect the capacity and rate performance.

[0197] (11) It can be seen from Application Examples 1 and 22 that the present invention does not evenly stir the salt solution before mixing it with citric acid, which will lead to uneven mixing during the material preparation process and fail to fully exert the effect of doping to improve the performance of the material.

[0198] (12) By comparing Application Example 1 with Comparative Application Example 1, it can be seen that if the modified positive electrode material in the present invention does not contain the doping element F, there is no strong interaction between Mn and F with strong electronegativity.2+ Dissolution occurs in the discharge state, accompanied by lattice distortion caused by the Jahn-Teller effect and irreversible oxygen evolution, resulting in low Na + diffusion rate and structural stability.

[0199] (13) By comparing Application Example 1 with Comparative Application Examples 2-4, it can be seen that the doping of a single element can often only improve the electrochemical performance of the material in a certain dimension. Due to the lack of synergistic effects between elements, the modified positive electrode material still undergoes irreversible phase changes, and its structural stability is poor, resulting in poor performance of the assembled battery.

[0200] (14) By comparing Application Example 1 with Comparative Application Example 5, it can be seen that if the layered transition metal oxide matrix of the present invention is not doped and modified, an irreversible phase change will occur during the charge and discharge process. + The content of Na + In addition, the material faces the problem of lattice distortion caused by transition metal dissolution and Jahn-Teller effect during the cycle, which makes the material exhibit poor electrochemical performance.

[0201] In summary, the modified positive electrode material provided by the present invention in situ dopes inert metal elements and low-valent anion elements into a sodium-based positive electrode material matrix containing transition metal oxides. The introduction of inert metal doping elements can stabilize the Na layer in the matrix material and inhibit the slip of the transition metal layer in the matrix material. Under high pressure conditions, it can exhibit relatively reversible migration behavior between the transition metal layer and the Na layer of the matrix material, stabilize the structure of the material, and inhibit the occurrence of irreversible phase changes inside the material. At the same time, the introduced low-valent anion elements partially replace the O in the matrix of the sodium-based positive electrode material, promote oxygen to participate in the redox reaction, thereby increasing the average valence state of the oxygen layer, expanding the interlayer spacing and reducing the band gap, thereby accelerating the charge transfer kinetics; and, the strong electronegative low-valent anion elements used have a strong interaction with the transition metal elements in the matrix, inhibiting the dissolution of the transition metal elements, increasing the oxygen vacancy formation energy, and reducing the irreversible oxygen evolution in the material, thereby improving Na + The diffusion rate can be reduced and the lattice distortion caused by the Jahn-Teller effect can be suppressed.

[0202] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A modified positive electrode material, characterized in that: The modified positive electrode material comprises a sodium-based positive electrode material matrix and a doping element doped in the sodium-based positive electrode material matrix, wherein the sodium-based positive electrode material matrix comprises a layered oxide containing a transition metal element, and the doping element comprises an inert metal element and a low-valent anion element; The inert metal element includes any one of Li, K, Ca, Cr, Mg, Ti, Zn, Al or Ag or a combination of at least two thereof, and the low-valent anion element includes any one of F, Cl or S or a combination of at least two thereof.

2. The modified positive electrode material according to claim 1, characterized in that The chemical general formula of the modified cathode material is Na a-x N x Me 1-y L y O 2-z Q z , where 0 < a ≤ 1, 0 ≤ x < 1, x < a, 0 ≤ y < 1, 0 < z < 2, x and y are not simultaneously 0, Me is a transition metal element, N, L, and Q are doping elements, among which, doping element N and doping element L are the inert metal elements, and doping element Q is the low-valence anion element; Preferably, the modified positive electrode material is a P2 type layered structure; Preferably, 0.5 <a≤0.7,0<x≤0.5,0<y≤0.5,0<z≤0.5; Preferably, 0.5 <a≤0.7,0.01≤x≤0.2,0.01≤y≤0.2,0.01≤z≤0.2; Preferably, in the modified positive electrode material, the molar ratio of the doping element N, the doping element L and the doping element Q is (4-6):(9-12):(7-9).

3. The modified positive electrode material according to claim 2, characterized in that: The transition metal element Me includes any one or a combination of at least two of Ni, Mn, Fe, Co or V, preferably Ni and / or Mn, more preferably Ni and Mn; Preferably, when the transition metal element Me includes Ni and Mn, the molar ratio of Ni to Mn is (0.1-0.4):(0.5-0.8), preferably (0.2-0.3):(0.6-0.7); Preferably, the doping element N includes any one of K, Ca or Ag or a combination of at least two thereof, preferably K; Preferably, the doping element L includes any one or a combination of at least two of Li, Zn, Mg, Cr, Al or Ti, preferably Li; Preferably, the doping element Q includes F.

4. A method for preparing a modified positive electrode material according to any one of claims 1 to 3, characterized in that: The preparation method comprises: In-situ mixing of a sodium source, a transition metal Me source and a dopant containing a doping element to obtain the modified positive electrode material; the doping element comprises an inert metal element and a low-valent anion element; The inert metal element includes any one of Li, K, Ca, Cr, Mg, Ti, Zn, Al or Ag or a combination of at least two thereof, and the low-valent anion element includes any one of F, Cl or S or a combination of at least two thereof.

5. The preparation method according to claim 4, characterized in that: The in-situ mixing method includes any one of a sol-gel method, a solid phase reaction method or a co-precipitation method, preferably a sol-gel method; Preferably, the sol-gel method for preparing the modified positive electrode material comprises the following steps: A sodium source, a transition metal Me source, a dopant containing a doping element and a solvent are first mixed to obtain a mixed solution, and then the mixed solution is second mixed with a complexing agent and heated to obtain a wet gel, and the wet gel is dried and calcined to obtain the modified positive electrode material.

6. The preparation method according to claim 4 or 5, characterized in that: The dopant containing the inert metal element includes an N source and / or an L source; Preferably, the dopant containing a low-valent anion element comprises a Q source; Preferably, the molar ratio of sodium element in the sodium source to transition metal element Me in the transition metal Me source is (0.03 - 1.1):(0 - 1), and does not include 0, preferably (0.53 - 0.8):1; Preferably, in the first mixing process, the molar ratio of transition metal element Me, doping element N, doping element L, and doping element Q in the transition metal Me source, N source, L source, and Q source is (1 - y):x:y:z, 0 ≤ x < 1, 0 ≤ y < 1, 0 < z < 2, x and y are not both 0, preferably 0 < x ≤ 0.5, 0 < y ≤ 0.5, 0 < z ≤ 0.5, further preferably 0.01 ≤ x ≤ 0.2, 0.01 ≤ y ≤ 0.2, 0.01 ≤ z ≤ 0.2; Preferably, the molar ratio of doping element N, doping element L, and doping element Q in the N source, L source, and Q source is (4 - 6):(9 - 12):(7 - 9); Preferably, the molar amount ratio of the complexing agent to the total molar amount of all transition metal elements in the mixed solution is (0.5 - 5):1, preferably (0.8 - 1.2):

1.

7. The preparation method according to claim 6, characterized in that: The sodium source includes any one or a combination of at least two of sodium acetate, sodium fluoride, sodium carbonate, sodium nitrate, or sodium hydroxide; Preferably, the transition metal Me source includes any one of acetate, chloride, nitrate, sulfate, or oxide containing transition metal element Me, preferably acetate; Preferably, the transition metal Me source includes any one or a combination of at least two of nickel source, manganese source, iron source, cobalt source, or vanadium source, further preferably nickel source and / or manganese source, further preferably nickel source and manganese source; Preferably, the molar ratio of nickel element in the nickel source to manganese element in the manganese source is (0.1 - 0.4):(0.5 - 0.8), preferably (0.2 - 0.3):(0.6 - 0.7); Preferably, the N source includes any one of acetate, chloride, nitrate, carbonate, or hydroxide containing doping element N, preferably acetate containing doping element N; Preferably, the L source includes any one of acetate, chloride, nitrate, carbonate, or hydroxide containing doping element L, preferably acetate containing doping element L; Preferably, the Q source includes any one of sodium salt, ammonium salt, potassium salt, or acid containing doping element Q, preferably sodium source containing doping element Q.

8. The preparation method according to any one of claims 5 to 7, characterized in that: The rotation speeds of the first mixing and the second mixing are independently selected from 200 - 500 rpm, preferably 300 - 400 rpm; Preferably, the temperature of the heating is 60 - 100 °C, preferably 75 - 85 °C; Preferably, the temperature of the drying is 120 - 180 °C, preferably 140 - 160 °C; Preferably, the time of the drying is 4 - 10 h, preferably 5 - 7 h; Preferably, the calcination includes a first calcination stage and a second calcination stage; Preferably, the heating rate of the first calcination stage and the second calcination stage are independently selected from 1 - 10 °C / min, preferably 4 - 6 °C / min; Preferably, the temperature of the first calcination stage is 300-600°C, preferably 400-500°C; Preferably, the first calcination stage is performed for 4-8 hours, preferably 5-7 hours; Preferably, the temperature of the second calcination stage is 700-1100°C, preferably 850-950°C; Preferably, the second calcination stage is performed for 10-20 hours, preferably 14-16 hours; Preferably, the calcination atmosphere is any one of air atmosphere, oxygen atmosphere or argon atmosphere, preferably air atmosphere.

9. A sodium ion battery, characterized in that: The sodium ion battery comprises a positive electrode sheet, an electrolyte, a separator and a negative electrode sheet, and the positive electrode sheet comprises the modified positive electrode material according to any one of claims 1 to 3.