High-conductivity and high-viscosity current collector carbon coating slurry
By calcining and grinding modified carbon black and graphene oxide, combining modified binder and solvent, the problems of conductivity and bonding properties in lithium-ion battery coating slurry are solved, and uniform dispersion and high efficiency of conductive agents are achieved Current collector performance.
Patent Information
- Application Number
- CN202411343410.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lithium-ion battery current collector coating slurry doped with oxygen-containing functional groups has impurities, which reduces the conductivity, and the adhesion of high-purity conductive substances to binders and solvents is poor, resulting in the conductive agent being coated in the coating. It is prone to agglomeration and uneven distribution in the slurry.
Using high-temperature calcination of modified carbon black and graphene oxide powder, the particle size is reduced by grinding, and combined with modified binder and solvent to form a composite conductive agent and modified binder, which is improved by blending and cross-linking reaction. Conductivity and bonding properties ensure uniform dispersion of conductive agents.
It improves the conductivity and bonding properties of the coating slurry, ensures that the conductive agent is evenly distributed in the current collector, enhances the rate performance and flexibility of the battery, and improves the coating performance.
Smart Images

Figure BDA0005060325200000031 
Figure BDA0005060325200000101 
Figure BDA0005060325200000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a current collector carbon-coated slurry with high conductivity and high viscosity. Background Art
[0002] In recent years, the electric vehicle industry has developed rapidly and the demand for power batteries has increased dramatically. Lithium iron phosphate batteries have become the first choice for power batteries due to their significant advantages in cycle life, safety, cost, etc. For pure electric vehicles, the battery's specific energy / specific power must be as high as possible to meet the needs of long-distance driving, climbing, acceleration and other performance requirements.
[0003] As the current collector of lithium-ion batteries, aluminum foil plays an important role in the battery. The surface of aluminum foil carries active substances and gathers the electrons generated by the positive active substances to the external circuit to form current. The surface treatment of the positive current collector of the battery using a functional coating can improve the adhesion between the active substance and the current collector and improve the ability of the positive electrode to collect the microcurrent of the active substance, thereby achieving the purpose of improving the rate performance of the battery. Therefore, the carbon-coated slurry coated on the surface of the current collector needs to have excellent bonding and conductive properties.
[0004] Patent application CN112864383A discloses a water-soluble power lithium-ion battery, whose positive electrode current collector is an oily carbon-coated aluminum foil, and the conductive agent includes an aqueous conductive slurry and carbon black, wherein the aqueous conductive slurry is a carbon nanotube slurry or a graphene conductive slurry, and the aqueous conductive slurry and the carbon black form a long- and short-range conductive network to improve the conductivity; however, there are different amounts of oxygen-containing groups on the surface of the carbon black particles, which have a great influence on the transmission of electrons, and its aqueous binder includes modified polyethylene oxide, modified gum arabic and modified styrene-butadiene rubber, and the three binders are mixed to improve the bonding performance of the electrode sheet and the flexibility of the positive electrode sheet, while the electrostatic adsorption force between the conductive agent itself and the aqueous binder is weak, and agglomeration is prone to occur, and there may be a phenomenon of uneven distribution of the conductive agent in the positive electrode current collector.
[0005] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a highly conductive and highly viscous current collector carbon-coated slurry, which is used to solve the technical problems in the prior art that when preparing the current collector carbon-coated slurry, conductive materials such as graphene and carbon black doped with oxygen-containing functional groups contain impurities, which reduces the conductivity, and the high-purity conductive materials have poor adhesion with binders and solvents, which makes the conductive materials easy to agglomerate and unevenly distributed in the current collector carbon-coated slurry.
[0007] The object of the present invention can be achieved by the following technical scheme: A highly conductive and highly viscous current collector carbon coating slurry comprises 20-30 parts of a composite conductive agent, 5-10 parts of a modified binder and 50-60 parts of a solvent;
[0008] The preparation method of the composite conductive agent comprises the following steps:
[0009] A1. Place carbon black in a corundum boat, and then place the corundum boat in a high-temperature heat treatment electric furnace; in a nitrogen atmosphere, first heat the corundum boat to 1300-1400°C and keep the temperature constant for 1 hour; then heat the high-temperature heat treatment electric furnace to 1400-1500°C and keep the temperature constant for 1 hour; then heat the high-temperature heat treatment electric furnace to 1500-1600°C and keep the temperature constant for 1 hour, then stop heating, and naturally cool to room temperature to obtain high-temperature calcined carbon black; ball-mill the high-temperature calcined carbon black to 100 mesh to obtain modified carbon black powder;
[0010] A2, graphene oxide is ground in a mortar to obtain graphene oxide powder of 500-600 mesh; the graphene oxide powder is then placed in a tissue grinder for secondary grinding to obtain graphene oxide powder;
[0011] The graphene oxide is first coarsely ground in a mortar and then ground again in a tissue grinder to reduce the particle size of the graphene oxide to obtain graphene oxide powder.
[0012] A3, guar gum is dissolved in deionized water to obtain a guar gum aqueous solution; then the graphene oxide powder is immersed in the guar gum aqueous solution, reacted, filtered, and a solid is obtained; the solid is vacuum dried to obtain a modified graphene oxide powder;
[0013] A4. Evenly mix the modified carbon black powder and the modified graphene oxide powder in a mass ratio of 1:3-5 to obtain a composite conductive agent.
[0014] Furthermore, in step A2, the grinding frequency of the tissue grinder is 50-100 Hz, and the number of grindings is 50 times; in step A3, the dosage ratio of guar gum and deionized water is 5-10 g:50 mL; the solid-liquid ratio of graphene oxide powder and guar gum aqueous solution is 1:5-6; the temperature of solid vacuum drying is 150° C., and the vacuum drying time is 10-12 h.
[0015] Furthermore, the preparation method of the modified binder comprises the following steps:
[0016] Polyvinyl alcohol powder, methyl methacrylate, catalyst dibutyltin dilaurate, inhibitor hydroquinone and 30-40%wt ethanol solution are added into a three-necked flask with a fractionation column, the temperature of the fractionation column of the three-necked flask is maintained at 60-70°C, the reaction is carried out for 2-3h, and then the reaction is stopped; the temperature of the water bath is set to 102-105°C, fractionation is carried out at this temperature, and the remaining organic liquid is collected to obtain a modified adhesive.
[0017] The modified adhesive is prepared by ester exchange reaction between polyvinyl alcohol and methyl methacrylate.
[0018] The reaction formula of polyvinyl alcohol and methyl methacrylate is as follows:
[0019]
[0020] Furthermore, the dosage ratio of polyvinyl alcohol powder, methyl methacrylate, catalyst, inhibitor and ethanol solution is 100 mL: 10-20 mL: 40-50 mL: 0.5-1 g: 1-2 g: 100 mL.
[0021] Furthermore, the solvent is obtained by mixing ethyl butyl carbonate, diisopropyl carbonate and methyl acetate in a mass ratio of 1:1:1.
[0022] As another aspect of the present invention, the present invention also provides a method for preparing a highly conductive and highly viscous current collector carbon-coated slurry, comprising the following steps:
[0023] The composite conductive agent, modified binder and solvent are mixed evenly, dispersed at a high speed of 1000-2000 rpm for 30 minutes, and allowed to stand at room temperature for 2-3 hours to obtain a current collector carbon coating slurry.
[0024] The present invention has the following beneficial effects:
[0025] 1. The composite conductive agent prepared by the present invention is obtained by mixing modified carbon black powder and modified graphene oxide powder in a specific mass ratio. Carbon black has a polyaromatic hydrocarbon structure, and each carbon atom in carbon black is SP 2 Hybridization forms covalent bonds with three adjacent carbon atoms, and the lone electrons of the Z orbital of each carbon atom overlap to form a delocalized large π bond, which makes carbon black have a certain conductivity. However, carbon black only has good conductivity in the direction parallel to the layer; the layers of carbon black are arranged in disordered layers, and the layer size is small and the defect density is large, which reduces the conductivity of carbon black. However, after high-temperature calcination, the interlayer spacing of carbon black is reduced and its own crystallinity is increased, thereby improving the conductivity of carbon black itself. In addition, after high-temperature calcination, the distance between particles is reduced after grinding, which reduces resistance and enhances conductivity.
[0026] 2. Graphene oxide is a derivative of graphene after oxidation. Graphene oxide retains the SP of graphene. 2 Based on the carbon skeleton structure, oxygen-containing functional groups are introduced to form SP 3 The hybrid structure makes the graphene oxide have a high specific surface area and sufficient oxygen-containing functional groups. The guar gum surface contains a large number of hydroxyl groups, which can be firmly bonded with the carboxyl functional groups rich in the surface of the graphene oxide, thereby obtaining guar gum-modified graphene oxide with ionic conductivity; the above-mentioned modified carbon black powder and modified graphene oxide powder are mixed, and the conductive substances of different particle sizes fill the pores with each other, so that the prepared composite conductive agent has high conductivity. In addition, the graphene oxide ground to a smaller particle size in the present invention is easier to disperse in the modified binder and solvent after modification, so that each component can be highly dispersed by simple mixing to obtain the current collector carbon coating slurry.
[0027] 3. The present invention is to prepare a modified adhesive by heat-treating polyvinyl alcohol and methyl methacrylate containing a carboxyl group, and the polyvinyl alcohol and methyl methacrylate react to form an ester bond, so that the polyvinyl alcohol and methyl methacrylate undergo a cross-linking reaction to form a bonding network. In addition, polyvinyl alcohol, as a vinyl polymer rich in hydroxyl groups, contains a large number of hydroxyl groups on its molecular chain, which can form hydrogen bonds with the hydroxyl groups on the surface of the composite conductive agent, thereby improving the bonding performance between the composite conductive agent and the modified adhesive. The modified adhesive prepared by the present invention has excellent bonding performance to each component in the current collector carbon coating slurry. The present invention uses a mixture of three esters as a solvent, thereby improving the solvent's solubility for the modified adhesive; the carbon coating slurry mixed with the solvent has good fluidity and uniform coating performance. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] The present embodiment provides a method for preparing a composite conductive agent for a current collector carbon coating slurry with high conductivity and high viscosity, comprising the following steps:
[0031] A1. Weigh 10g of carbon black and place it in a corundum boat, then place the corundum boat in a high-temperature heat treatment furnace; nitrogen is introduced into the high-temperature heat treatment furnace three times until all the air in the high-temperature heat treatment furnace is exhausted, so that it is in a nitrogen atmosphere. Then close the gas outlet valve in the high-temperature heat treatment furnace, raise the temperature to 1300℃, and keep the temperature constant for 1h; then raise the temperature to 1400℃, and keep the temperature constant for 1h; then raise the temperature to 1500℃, and keep the temperature constant for 1h, then stop heating, let the high-temperature heat treatment furnace cool naturally to room temperature, take out the sample, and obtain the carbon black after high-temperature calcination. The carbon black after high-temperature calcination is placed on a ball mill and ball-milled to 100 mesh to obtain modified carbon black powder.
[0032] A2. Weigh 2 g of graphene oxide and grind it in a mortar to obtain 500-mesh graphene oxide powder. Then, grind the graphene oxide in a tissue grinder for a second time at a grinding frequency of 50 Hz and 50 times to obtain graphene oxide powder.
[0033] A3, 5g of guar gum and 50mL of deionized water were mixed to prepare a 2%wt guar gum aqueous solution. Then, the graphene oxide powder was immersed in the guar gum aqueous solution and reacted at room temperature for 2h. The solid-liquid ratio of the graphene oxide powder and the guar gum aqueous solution was 1:5. Then, the solid was filtered to obtain a solid; the solid was vacuum dried at 150°C for 10h to obtain a modified graphene oxide powder.
[0034] A4. The modified carbon black powder and the modified graphene oxide powder are evenly mixed in a mass ratio of 1:3 to obtain a composite conductive agent.
[0035] Example 2
[0036] The present embodiment provides a method for preparing a composite conductive agent for a current collector carbon coating slurry with high conductivity and high viscosity, comprising the following steps:
[0037] A1. Weigh 15g of carbon black and place it in a corundum boat, then place the corundum boat in a high-temperature heat treatment furnace; nitrogen is introduced into the high-temperature heat treatment furnace three times until all the air in the high-temperature heat treatment furnace is exhausted, so that it is in a nitrogen atmosphere. Then close the gas outlet valve in the high-temperature heat treatment furnace, raise the temperature to 1350℃, and keep the temperature constant for 1h; then raise the temperature to 1455℃, and keep the temperature constant for 1h; then raise the temperature to 1560℃, and keep the temperature constant for 1h, then stop heating, let the high-temperature heat treatment furnace cool naturally to room temperature, take out the sample, and obtain the carbon black after high-temperature calcination. The carbon black after high-temperature calcination is placed on a ball mill and ball-milled to 100 mesh to obtain modified carbon black powder.
[0038] A2, weigh 2.6g of graphene oxide, grind it in a mortar to obtain 550 mesh graphene oxide powder. Then put the graphene oxide into a tissue grinder for secondary grinding, the grinding frequency is 60Hz, the grinding number is 50 times, and the graphene oxide powder is obtained.
[0039] A3, 8 guar gum and 50 mL of deionized water were mixed to prepare a guar gum aqueous solution. Then, the graphene oxide powder was immersed in the guar gum aqueous solution and reacted at room temperature for 2.3 hours. The solid-liquid ratio of the graphene oxide powder and the guar gum aqueous solution was 1:5. Then, the solid was filtered to obtain a solid. The solid was vacuum dried at 150°C for 11 hours to obtain a modified graphene oxide powder.
[0040] A4. The modified carbon black powder and the modified graphene oxide powder are evenly mixed in a mass ratio of 1:4 to obtain a composite conductive agent.
[0041] Example 3
[0042] The present embodiment provides a method for preparing a composite conductive agent for a current collector carbon coating slurry with high conductivity and high viscosity, comprising the following steps:
[0043] A1. Weigh 20g of carbon black and place it in a corundum boat, then place the corundum boat in a high-temperature heat treatment furnace; nitrogen is introduced into the high-temperature heat treatment furnace three times until all the air in the high-temperature heat treatment furnace is exhausted, so that it is in a nitrogen atmosphere. Then close the gas outlet valve in the high-temperature heat treatment furnace, raise the temperature to 1400℃, and keep the temperature constant for 1h; then raise the temperature to 1500℃, and keep the temperature constant for 1h; then raise the temperature to 1600℃, and keep the temperature constant for 1h, then stop heating, let the high-temperature heat treatment furnace cool naturally to room temperature, take out the sample, and obtain the carbon black after high-temperature calcination. The carbon black after high-temperature calcination is placed on a ball mill and ball-milled to 100 mesh to obtain modified carbon black powder.
[0044] A2, weigh 3g of graphene oxide, grind it in a mortar to obtain 600-mesh graphene oxide powder. Then put the graphene oxide into a tissue grinder for secondary grinding, the grinding frequency is 100Hz, the grinding number is 50 times, and the graphene oxide powder is obtained.
[0045] A3, 10g of guar gum and 50mL of deionized water were mixed to prepare a guar gum aqueous solution. Then, the graphene oxide powder was immersed in the guar gum aqueous solution and reacted at room temperature for 3h. The solid-liquid ratio of the graphene oxide powder and the guar gum aqueous solution was 1:6. Then, the solid was filtered to obtain a solid. The solid was vacuum dried at 150°C for 12h to obtain a modified graphene oxide powder.
[0046] A4. The modified carbon black powder and the modified graphene oxide powder are uniformly mixed in a mass ratio of 1:5 to obtain a composite conductive agent.
[0047] Example 4
[0048] This embodiment provides a method for preparing a highly conductive and highly viscous current collector carbon-coated slurry, comprising the following steps:
[0049] B1. Prepare 100 mL of 30% wt ethanol solution. Add 10 mL of polyvinyl alcohol powder, 40 mL of methyl methacrylate, 0.5 g of catalyst dibutyltin dilaurate, 1 g of inhibitor hydroquinone and 100 mL of ethanol solution into a 500 mL three-necked flask equipped with a thermometer, a fractionating column and a condenser.
[0050] B2. Transfer the three-necked flask to a water bath, pre-set the temperature of the water bath to 50°C, then continuously adjust the temperature of the water bath to maintain the temperature at the top of the distillation column in the three-necked flask at 60°C, react for 2 hours under stirring at 100°C, and then stop the reaction; then set the temperature of the water bath to 102°C, perform distillation at this temperature, and collect the remaining organic liquid in the three-necked flask, which is the modified adhesive.
[0051] B3. Ethyl butyl carbonate, diisopropyl carbonate and methyl acetate are mixed in a mass ratio of 1:1:1 to obtain a solvent; 20 parts of the composite conductive agent prepared in Example 3, 5 parts of the modified binder and 50 parts of the solvent are mixed in parts by weight, and the mixture is dispersed at a high speed of 1000 rpm for 30 min. After standing at room temperature for 2 h, a current collector carbon coating slurry is obtained.
[0052] Example 5
[0053] This embodiment provides a method for preparing a highly conductive and highly viscous current collector carbon-coated slurry, comprising the following steps:
[0054] B1. Prepare 100 mL of 35% wt ethanol solution. Add 15 mL of polyvinyl alcohol powder, 45 mL of methyl methacrylate, 0.6 g of catalyst dibutyltin dilaurate, 1.5 g of inhibitor hydroquinone and 100 mL of ethanol solution into a 500 mL three-necked flask equipped with a thermometer, a fractionating column and a condenser.
[0055] B2. Transfer the three-necked flask to a water bath, pre-set the temperature of the water bath to 56°C, then continuously adjust the temperature of the water bath to maintain the temperature at the top of the three-necked flask fractionation column at 62°C, react for 2.3 hours under stirring at 150°C, and then stop the reaction. Then set the temperature of the water bath to 103°C, perform fractionation at this temperature, and collect the remaining organic liquid, which is the modified adhesive.
[0056] B3. Ethyl butyl carbonate, diisopropyl carbonate and methyl acetate are mixed in a mass ratio of 1:1:1 to obtain a solvent; 25 parts of the composite conductive agent prepared in Example 3, 8 parts of the modified binder and 55 parts of the solvent DMF are mixed in parts by weight, and the mixture is dispersed at a high speed of 1500 rpm for 30 min. After standing at room temperature for 2 h, a current collector carbon coating slurry is obtained.
[0057] Example 6
[0058] This embodiment provides a method for preparing a highly conductive and highly viscous current collector carbon-coated slurry, comprising the following steps:
[0059] B1. Prepare 100 mL of 40% wt ethanol solution. Add 20 mL of polyvinyl alcohol powder, 50 mL of methyl methacrylate, 1 g of catalyst dibutyltin dilaurate, 2 g of inhibitor hydroquinone and 100 mL of ethanol solution into a 500 mL three-necked flask equipped with a thermometer, a fractionating column and a condenser.
[0060] B2. Transfer the three-necked flask to a water bath, pre-set the temperature of the water bath to 60°C, then continuously adjust the temperature of the water bath to maintain the temperature at the top of the distillation column in the three-necked flask at 70°C, react for 3 hours under stirring at 200°C, and then stop the reaction. Then set the temperature of the water bath to 105°C, perform distillation at this temperature, and collect the remaining organic liquid, which is the modified adhesive.
[0061] B3. Ethyl butyl carbonate, diisopropyl carbonate and methyl acetate are mixed in a mass ratio of 1:1:1 to obtain a solvent; 30 parts of the composite conductive agent prepared in Example 3, 10 parts of the modified binder and 60 parts of the solvent DMF are mixed in parts by weight, and the mixture is dispersed at a high speed of 2000 rpm for 30 min. After standing at room temperature for 3 h, a current collector carbon coating slurry is obtained.
[0062] Comparative Example 1
[0063] The difference between this comparative example and Example 3 is that when preparing the composite conductive agent, the carbon black is not calcined at high temperature.
[0064] Comparative Example 2
[0065] The difference between this comparative example and Example 3 is that, when preparing the composite conductive agent, the graphene oxide is not modified by using the guar gum aqueous solution.
[0066] Comparative Example 3
[0067] The difference between this comparative example and Example 6 is that the modified binder is replaced by polyvinyl alcohol of equal mass.
[0068] Performance Testing:
[0069] 1. The intrinsic conductivity of the composite conductive agent prepared in Examples 1-3 and Comparative Examples 1-2 was tested. The composite conductive agent prepared in Examples 1-3 and Comparative Examples 1-2 was pressed into a round sheet in a cylindrical mold with a bottom diameter of 1 / 3 mm at a pressure of 15 MPa; the conductivity of the composite conductive agent prepared in Examples 1-3 and Comparative Examples 1-2 was tested in sequence using a digital four-probe resistance meter; the conductivity of each round sheet was measured 10 times, and the average value was taken as the final result. The specific test results are shown in Table 1.
[0070] Table 1-Performance test data of samples
[0071]
[0072] Data Analysis:
[0073] Comparative analysis of the data in Table 1 shows that the composite conductive agent prepared in Examples 1-3 of the present invention has excellent conductivity, which is manifested by a high conductivity value. However, in Comparative Example 1, since the carbon black was not calcined at high temperature to remove impurities, and in Comparative Example 2, the graphene oxide was not modified with a guar gum aqueous solution, the conductive properties of the prepared composite conductive agent were reduced, which was manifested by a reduced conductivity value.
[0074] 2. The modified adhesives prepared in Examples 4-6 and Comparative Example 3 were subjected to a 180°C peel test. The modified adhesives prepared in Examples 4-6 and Comparative Example 3 were marked as Sample 1, Sample 2, Sample 3 and Sample 4, respectively. The samples and 3M tape were placed on a universal stretching machine at 180°C, and Samples 1-4 were stretched in sequence at a displacement rate of 100 mm / min, and the relationship between the displacement and the peel force was recorded, and the value of the average peel force was recorded.
[0075] 3. The modified binders prepared in Examples 4-6 and Comparative Example 3 were subjected to thermogravimetric analysis, and their retention rates at 100° C., 300° C. and 500° C. were recorded. The specific test results are shown in Table 2.
[0076] Table 2-Sample performance test data table
[0077]
[0078] Data Analysis:
[0079] Comparative analysis of the data in Table 2 shows that the modified adhesives prepared in Examples 4-6 of the present invention all have strong bonding performance and thermal stability, as shown by the large average peeling force values, and still have a high quality retention rate under high temperature conditions. However, in Comparative Example 3, replacing the modified adhesive with a single polyvinyl alcohol will not only reduce the bonding performance of the modified adhesive, as shown by the decrease in the average peeling force value. On the other hand, it will also reduce its own thermal stability, as shown by the significant decrease in the quality retention rate value under high temperature conditions.
[0080] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0081] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0082] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A highly conductive and highly viscous current collector carbon-coated slurry, characterized in that: In parts by weight, it comprises 20-30 parts of a composite conductive agent, 5-10 parts of a modified binder and 50-60 parts of a solvent; The preparation method of the composite conductive agent comprises the following steps: A1. Place carbon black in a corundum boat, and then place the corundum boat in a high-temperature heat treatment electric furnace; in a nitrogen atmosphere, first heat the corundum boat to 1300-1400°C and keep the temperature constant for 1 hour; then heat the high-temperature heat treatment electric furnace to 1400-1500°C and keep the temperature constant for 1 hour; then heat the high-temperature heat treatment electric furnace to 1500-1600°C and keep the temperature constant for 1 hour, then stop heating, and naturally cool to room temperature to obtain high-temperature calcined carbon black; ball-mill the high-temperature calcined carbon black to 100 mesh to obtain modified carbon black powder; A2, graphene oxide is ground with a mortar to obtain graphene oxide powder of 500-600 mesh; the graphene oxide powder is then placed in a tissue grinder for secondary grinding to obtain graphene oxide powder; A3, guar gum is dissolved in deionized water to obtain a guar gum aqueous solution; then the graphene oxide powder is immersed in the guar gum aqueous solution, reacted, filtered, and a solid is obtained; the solid is vacuum dried to obtain a modified graphene oxide powder; A4. Evenly mix the modified carbon black powder and the modified graphene oxide powder in a mass ratio of 1:3-5 to obtain a composite conductive agent.
2. The highly conductive and highly viscous current collector carbon-coated slurry according to claim 1, characterized in that: In step A2, the grinding frequency of the tissue grinder is 50-100 Hz, and the number of grindings is 50 times; in step A3, the dosage ratio of guar gum and deionized water is 5-10 g:50 mL; the solid-liquid ratio of graphene oxide powder and guar gum aqueous solution is 1:5-6; the temperature of solid vacuum drying is 150° C., and the vacuum drying time is 10-12 h.
3. The highly conductive and highly viscous current collector carbon-coated slurry according to claim 1, characterized in that: The preparation method of the modified binder comprises the following steps: Polyvinyl alcohol powder, methyl methacrylate, catalyst dibutyltin dilaurate, inhibitor hydroquinone and 30-40%wt ethanol solution are added into a three-necked flask with a fractionation column, the temperature of the fractionation column of the three-necked flask is maintained at 60-70°C, the reaction is carried out for 2-3h, and then the reaction is stopped; the temperature of the water bath is set to 102-105°C, fractionation is carried out at this temperature, and the remaining organic liquid is collected to obtain a modified adhesive.
4. The highly conductive and highly viscous current collector carbon-coated slurry according to claim 3, characterized in that: The dosage ratio of polyvinyl alcohol powder, methyl methacrylate, catalyst dibutyltin dilaurate, inhibitor hydroquinone and ethanol solution is 100mL: 10-20mL: 40-50mL: 0.5-1g: 1-2g: 100mL.
5. The highly conductive and highly viscous current collector carbon-coated slurry according to claim 1, characterized in that: The solvent is obtained by mixing ethyl butyl carbonate, diisopropyl carbonate and methyl acetate in a mass ratio of 1:1:
1.
6. A method for preparing a highly conductive and highly viscous current collector carbon-coated slurry as claimed in any one of claims 1 to 5, characterized in that: Prepared by the following steps: The composite conductive agent, modified binder and solvent are mixed evenly, dispersed at a high speed of 1000-2000 rpm for 30 minutes, and allowed to stand at room temperature for 2-3 hours to obtain a current collector carbon coating slurry.
Citation Information
Cited By
Elastic current collector and preparation method and application thereof
CN119994071A