Atomically dispersed non-noble metal catalyst based on defect ligand as well as preparation method and application of atomically dispersed non-noble metal catalyst
By embedding MN4 structure in the carbon support and using defective ligands to form a multi-fraction pore structure, the problems of low activity and insufficient stability of single-atom transition metal carbon-based catalysts are solved, and efficient oxygen reduction reaction and stable catalytic performance are achieved. , suitable for the new energy field.
Patent Information
- Application Number
- CN202411089246.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing single-atom transition metal carbon-based catalysts have low catalytic activity in oxygen reduction reactions and insufficient stability and utilization, which limits their application in new energy fields such as proton exchange membrane fuel cells.
Using atomic-scale dispersed non-noble metal catalyst based on defective ligands, the multi-fraction porous structure and the use of 5-aminotetrazole as defective ligand is formed by pyrolysis and porous treatment. Symmetrical strain environment improves the activity and stability of the catalyst.
The rate of oxygen reduction reaction and the stability of the catalyst are significantly improved. The half-wave potential is reduced by only 16mV after aging in the acidic electrolyte. The catalyst exhibits efficient oxygen reduction performance in proton exchange membrane fuel cells and metal air batteries.
Smart Images

Figure CN119008985A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of preparation and application of oxygen reduction electrocatalysts, and specifically relates to atomically dispersed non-precious metal catalysts and preparation methods and applications thereof. Background Art
[0002] As the world faces energy crisis and climate change, the demand for sustainable energy technologies is becoming increasingly urgent. Proton exchange membrane fuel cells (PEMFCs) are considered to be cutting-edge energy technologies, but their widespread application is still hindered by the sluggish kinetics of the oxygen reduction reaction (ORR). Among them, single-atom transition metal carbon-based catalysts (Fe, Mn, Co, Ni) M-NCs overcome the limitations of traditional Pt-based catalysts and become very promising ORR catalysts. In general, the M-N4 site with a symmetrical electronic structure is not conducive to the adsorption-desorption of oxygen-containing intermediates, thereby hindering the ORR kinetics.
[0003] At the same time, the high-activity Fe-NC catalysts are limited in further practical applications due to the insufficient utilization of active sites and low stability. In order to achieve higher catalytic performance, Fe-NC catalysts often have higher loadings and thicker catalytic layers. However, excessive loading may lead to mutual shielding between active sites and affect mass transfer, thereby affecting the efficiency of the catalytic reaction. Summary of the invention
[0004] The present invention aims to solve the technical problem of low catalytic activity of existing single-atom transition metal carbon-based catalysts, and to provide an atomically dispersed non-precious metal catalyst based on defective ligands and its preparation method and application. The catalyst is a strain-regulated transition metal-based single-atom catalyst with high activity and high stability, and can be applied to cathode oxygen reduction in new energy fields such as proton exchange membrane fuel cells and metal-air batteries.
[0005] The atomically dispersed non-precious metal catalyst based on defective ligands of the present invention is composed of MN4 embedded in a carbon carrier, wherein M is coordinated with N with two sets of different MN bond lengths, showing 2N t =M=2N c Coordination structure, wherein t represents tensile, c represents compressive, the mass fraction of M is 0.5% to 1%, and M is Fe, Mn, Co or Ni.
[0006] The above-mentioned preparation method of the atomic-level dispersion of defective ligand-based non-precious metal catalyst is carried out according to the following steps:
[0007] 1. Preparation of a three-dimensional nitrogen-doped porous defective flower-like carbon carrier precursor: Dissolve a zinc source and a nitrogen source in methanol respectively, then mix them, stir rapidly and vigorously for 2 to 2.5 hours, and keep them at 60 to 65° C. for 2 to 2.5 hours to produce a white suspension in the solution; then centrifuge, wash, and dry to obtain a three-dimensional nitrogen-doped porous defective flower-like carbon carrier precursor, which is a white powder; wherein the nitrogen source is 5-aminotetrazolyl monohydrate (5-ATZ) and 2-methylimidazole (2-MIM) in a molar ratio of 1:(3 to 5);
[0008] 2. Preparation of nitrogen-doped porous carbon carrier: The precursor prepared in step 1 is subjected to a stepwise high-temperature heat treatment under an inert atmosphere, and cooled to room temperature to obtain a nitrogen-doped porous carbon carrier (NC); wherein the stepwise high-temperature heat treatment is: firstly heating to 200-220°C and maintaining for 0.5-0.6h, then heating to 400-420°C and maintaining for 0.5-0.6h, then heating to 700-720°C and maintaining for 1-1.3h, and finally heating to 1000-1050°C and maintaining for 2-2.5h;
[0009] 3. Preparation of single-atom catalyst precursor: first, immerse the nitrogen-doped porous carbon support into a soluble salt solution of metal M, vigorously stir for 2 to 2.5 hours under an inert atmosphere, then ultrasonically disperse for 2 to 2.5 hours, filter or centrifuge, and dry the solid phase to obtain a single-atom catalyst precursor;
[0010] 4. Preparation of single atom catalysts: Place the single atom catalyst precursor in a furnace, heat it to 950-1050°C in an argon atmosphere, and heat treat it for 2-3 hours to obtain an atomically dispersed non-precious metal catalyst based on defective ligands, represented by MN4-SM.
[0011] Furthermore, the zinc source in step 1 is zinc acetate dihydrate ((CH3COO)2Zn), anhydrous zinc nitrate (Zn(NO3)2) or zinc nitrate hexahydrate (Zn(NO3)2·6H2O).
[0012] Furthermore, the inert atmosphere in step 2 and step 3 is Ar or N2.
[0013] Furthermore, the drying in step 1 and step 3 is vacuum drying at a temperature of 60 to 80° C. for 6 to 8 hours.
[0014] Furthermore, the solvent of the metal M soluble salt solution in step 3 is N,N-dimethylformamide.
[0015] Furthermore, the vigorous stirring in step three has a stirring speed of 500-700 rpm.
[0016] Furthermore, the heating rate in step 4 is 5-20°C min -1 .
[0017] The application of the above-mentioned atomically dispersed non-precious metal catalyst based on defective ligands is to use the catalyst as a cathode catalyst of a proton exchange membrane fuel cell or a metal-air battery.
[0018] The method for preparing strain-regulated single-atom catalysts of the present invention produces the following two effects through the thermal decomposition of defective ligand 5-aminotetrazolyl. First, a one-step porous treatment greatly reduces the process complexity and cost of preparing single-atom catalysts, produces a multi-level pore structure, improves its pore size and pore structure, and improves the accessible utilization rate of active sites and material transport capacity. Second, it induces CN cracking to regulate atomic strain, ensuring the efficient preparation of single-atom sites. This method is applicable to Fe, Mn, Co, and Ni metal elements and has good universality.
[0019] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows:
[0020] 1. The present invention introduces 5-aminotetrazolyl as a defective ligand to prepare a three-dimensional porous defective flower-like sphere for the nitrogen-doped carbon support of the oxygen reduction reaction, resulting in CN cracking. The induced hierarchical porous structure is beneficial to promoting the mass transfer of O2 and H2O without the need for secondary porous treatment.
[0021] 2. The one-step porous heat treatment produces a multi-level pore structure, which helps to increase defects and thus improve the density of M-N4 centers; the two-step graphitization heat treatment enhances the corrosion resistance of the carbon substrate, thereby improving the stability of the catalyst under working conditions.
[0022] 3. Compared with single-atom Fe-based catalysts, strain-regulated MN4-SM (M = Fe, Mn, Co, Ni) can relax the adsorption affinity to intermediates and effectively promote the desorption of oxygen-containing intermediates, thereby effectively increasing the rate of the oxygen reduction reaction of the catalyst.
[0023] 4. The atomically dispersed Fe-based catalyst prepared in the present invention exhibits a relatively high half-wave potential in acidic and alkaline electrolytes. After 60,000 cycles of aging in an acidic medium, the half-wave potential only decreases by 16 mV.
[0024] The atomically dispersed catalyst of the present invention uses 5-aminotetrazole as a defective ligand and cooperates with dimethylimidazole as a dual ligand to prepare a porous defective carbon carrier. The thermal instability of 5-aminotetrazole during pyrolysis is used to generate gas to cause CN cracking. While supplementing the nitrogen source, the asymmetric strain generated helps to regulate the Fe site, and the content is low. At the same time, the carbon carrier has a hierarchical porous structure of micropores and mesopores, wherein the pore size of the micropores is 0.5 to 2 nm, the pore size of the mesopores is 2 to 30 nm, and the pore volume is 1.383 cm 3 g -1 ; The specific surface area of the catalyst particles is 400 to 1000 m 2 g -1 This catalyst with a three-dimensional hierarchical porous structure has high intrinsic activity and accessible active site density, and effectively promotes material transport. The maximum power density of the fuel cell assembled with this catalyst as the cathode reaches 862mW cm -2 , which can be used in the cathode oxygen reduction reaction of proton exchange membrane fuel cells and metal-air batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 XRD spectra of FeN4-SM prepared in Example 1, FeN4-SM3, FeN4-SM5 and FeN4 prepared in Comparative Examples 2, 3 and 4, and their corresponding precursors.
[0026] Figure 2 High-resolution transmission electron microscope images of FeN4-SM prepared in Example 1, FeN4-SM3, FeN4-SM5 and FeN4 prepared in Comparative Examples 2, 3 and 4. From left to right, the columns are FeN4, FeN4-SM3, FeN4-SM and FeN4-SM5.
[0027] Figure 3 This is a scanning electron microscope image of FeN4-SM in Example 1.
[0028] Figure 4 This is the transmission electron microscope image of FeN4-DH in Comparative Example 5.
[0029] Figure 5 This is a transmission electron microscope energy dispersive X-ray spectroscopy (EDS) surface scan analysis of FeN4-SM prepared in Example 1. From left to right, they are respectively, EDS surface scan C element distribution image, EDS surface scan N element distribution image, and EDS surface scan Fe element distribution image.
[0030] Figure 6 These are the nitrogen adsorption and desorption isotherms of FeN4-SM prepared in Example 1 and FeN4 prepared in Comparative Example 4.
[0031] Figure 7 It is a pore size distribution curve diagram of FeN4-SM in Example 1 and FeN4 in Comparative Example 4.
[0032] Figure 8 This is the spherical aberration electron microscope image of FeN4-SM prepared in Example 1.
[0033] Fig. 9 C1s high-resolution spectra of X-ray photoelectron spectra of FeN4-SM prepared in Example 1, FeN4-SM3, FeN4-SM5 and FeN4 prepared in Comparative Examples 2, 3 and 4. From left to right, the columns are FeN4, FeN4-SM3, FeN4-SM and FeN4-SM5.
[0034] Fig.10 It is the Fe 2p high-resolution spectrum of X-ray photoelectron spectrum of FeN4-SM prepared in Example 1, FeN4-SM3, FeN4-SM5 and FeN4 prepared in Comparative Examples 2, 3 and 4.
[0035] Fig.11 The FeN4-SM prepared in Example 1 and the FeN4 prepared in Comparative Example 4 are 13 C NMR spectrum.
[0036] Fig.12 The X-ray absorption near-edge structure and extended X-ray absorption fine structure analysis diagram of the Fe element of FeN4-SM in Example 1;
[0037] Fig.13 It is the structural model diagram of FeN4-SM in Example 1;
[0038] Fig.14 These are the in-situ Raman spectra of FeN4-SM in Example 1 and FeN4 in Comparative Example 1 at different potentials.
[0039] Fig.15 This is a comparison chart of the oxygen reduction performance test curve of FeN4-SM in Example 1 in an oxygen-saturated 0.1M KOH solution with other catalysts.
[0040] Fig.16 This is a comparison chart of the oxygen reduction performance test curve of FeN4-SM in Example 1 in an oxygen-saturated 0.1M HClO4 solution with other catalysts.
[0041] Fig.17 This is a polarization curve diagram of FeN4-SM in Example 1 after 60,000 cycles of accelerated cyclic voltammetry test in an oxygen-saturated 0.1M HClO4 solution.
[0042] Fig.18It is a comparison chart of the discharge power curves of the fuel cell assembled with FeN4-SM in Example 1 and FeN4 catalyst in Comparative Example 1.
[0043] Fig.19 This is the transmission electron microscope EDS surface scan image of MnN4-SM in Example 2; from left to right, they are respectively, the EDS surface scan C element distribution image, the EDS surface scan N element distribution image, and the EDS surface scan Mn element distribution image.
[0044] Fig. 20 This is a test curve of the oxygen reduction performance of MnN4-SM in Example 2 in an oxygen-saturated 0.1M KOH solution. DETAILED DESCRIPTION
[0045] The technical solutions and applications of the present invention are described in detail below through specific examples, but the scope of protection of the present invention is not limited thereto.
[0046] Example 1: The preparation method of the atomically dispersed non-precious metal catalyst based on defective ligands in this example is carried out according to the following steps:
[0047] 1. Preparation of three-dimensional nitrogen-doped porous defective flower-like carbon carrier precursor: 428 mg of zinc acetate dihydrate was dissolved in 150 mL of methanol to obtain a zinc acetate solution; 492 mg of 2-methylimidazole and 154 mg of 5-aminotetrazole monohydrate were dissolved in 150 mL of methanol to obtain a nitrogen source solution; the zinc acetate solution and the nitrogen source solution were then mixed and vigorously stirred for 2 h at a stirring speed of 500-700 rpm, and placed in an oven at a temperature of 65°C for 2 h, and a white suspension was generated in the solution; the solid phase was washed with methanol three times by centrifugation, and then placed in a vacuum drying oven at a temperature of 65°C for vacuum drying for 8 h to obtain a nitrogen-doped porous carbon carrier precursor, which is a white powder;
[0048] 2. Preparation of nitrogen-doped porous carbon support: The precursor prepared in step 1 was placed in a high-temperature furnace under an argon atmosphere at 5 °C min -1 The heating rate was first raised to 200 °C and maintained for 0.5 h, then increased at 5 °C min -1 The heating rate was raised to 400℃ and maintained for 0.5h, then increased to 5℃min -1 The heating rate was raised to 700℃ and maintained for 1h, and finally at 5℃min -1 The temperature was raised to 1000°C at a heating rate of 200 °C and maintained for 2 h to obtain a nitrogen-doped porous carbon support (NC);
[0049] 3. Preparation of single-atom catalyst precursor: 50 mg of ferrous sulfate heptahydrate was dissolved in 40 mL of N, N-dimethylformamide liquid to obtain a ferrous sulfate solution; 100 mg of nitrogen-doped porous carbon support was immersed in the ferrous sulfate solution, and stirred vigorously at a stirring speed of 500-700 rpm for 2 h under an argon atmosphere, and then ultrasonically dispersed in an ultrasonic cleaner for 2 h, filtered, and the separated solid components were placed in a vacuum drying oven at a temperature of 65 ° C and vacuum dried for 8 h to obtain a single-atom catalyst precursor;
[0050] 4. Preparation of single atom catalysts: The single atom catalyst precursor is placed in a high-temperature furnace, heated to 1000°C in an argon atmosphere and maintained for 3 hours for heat treatment to obtain an atomically dispersed non-precious metal catalyst based on defective ligands, represented by FeN4-SM.
[0051] Comparative Example 1: This comparative example is to prepare FeN4-SM0 catalyst. The difference between this comparative example and Example 1 is that the "492 mg of 2-methylimidazole" in step one is replaced by "773 mg of 5-aminotetrazole monohydrate", and the other steps and parameters are the same as Example 1. The obtained catalyst is recorded as FeN4-SM0.
[0052] In this comparative example, 5-aminotetrazolyl (5-ATZ) completely replaces 2-methylimidazole (2-MIM). Since the ligand is only 5-aminotetrazolyl, 5-aminotetrazolyl is almost completely pyrolyzed into gas volatilization during the high temperature treatment of step 2, and the yield is very small and difficult to collect. It is speculated that in the precursor structure prepared based on the defective ligand, 2-methylimidazole is used as the skeleton and 5-aminotetrazolyl is mainly used as the defective ligand.
[0053] Comparative Example 2: This comparative example is to prepare FeN4-SM3 catalyst. The difference between this comparative example and Example 1 is that the "492 mg 2-methylimidazole and 154 mg 5-aminotetrazole monohydrate" in step one is replaced by "461 mg 2-methylimidazole and 193 mg 5-aminotetrazole monohydrate", so that the molar ratio of 5-aminotetrazole monohydrate to 2-methylimidazole is 1:3. The other steps and parameters are the same as in Example 1, and the obtained catalyst is recorded as FeN4-SM3.
[0054] Comparative Example 3: This comparative example is to prepare FeN4-SM5 catalyst. The difference between this comparative example and Example 1 is that the "492 mg 2-methylimidazole and 154 mg 5-aminotetrazole monohydrate" in step one is replaced by "129 mg 2-methylimidazole and 512 mg 5-aminotetrazole monohydrate", so that the molar ratio of 5-aminotetrazole monohydrate to 2-methylimidazole is 1:5. The other steps and parameters are the same as in Example 1, and the obtained catalyst is recorded as FeN4-SM5.
[0055] Comparative Example 4: This comparative example is to prepare FeN4 catalyst. The difference between this comparative example and Example 1 is that step 1 is replaced by the following operation:
[0056] 1. Dissolve 320 mg of 2-methylimidazole (2-MIM) in 300 mL of methanol to obtain a 2-methylimidazole solution; dissolve 290 mg of Zn(NO3)2·6H2O in 300 mL of methanol to obtain a zinc nitrate solution; mix the 2-methylimidazole solution and the zinc nitrate solution and stir for 1 day to react; then centrifuge and separate, wash the solid phase with ethanol 3 times, and place it in a vacuum drying oven at a temperature of 65°C for 12 hours to obtain a nitrogen-doped carbon support;
[0057] The other steps and parameters are the same as those in Example 1 to obtain a FeN4 catalyst.
[0058] Comparative Example 5: This comparative example is to prepare FeN4-DH (Direct Heating) catalyst. The difference between this comparative example and Example 1 is that step 2 is replaced by the following operation: 2. The precursor prepared in step 1 is placed in a high temperature furnace under an argon atmosphere at 5°C min -1 The temperature was directly raised to 1000° C. at a heating rate of 1000° C. and maintained for 2 h to obtain a nitrogen-doped porous carbon support; the other steps and parameters were the same as those in Example 1, and the obtained catalyst was recorded as FeN4-DH.
[0059] The FeN4-SM prepared in Example 1, the FeN4-SM3, FeN4-SM5 and FeN4 prepared in Comparative Examples 2, 3 and 4 and their corresponding precursors were subjected to X-ray diffraction pattern tests, and the obtained X-ray diffraction patterns are as follows: Figure 1 As shown, from Figure 1 As shown in a, the precursor of FeN4-SM is the same as the precursor of FeN4-SM3 and FeN4-SM5, and has a high similarity with the precursor of FeN4, further highlighting the inheritance of its main framework. This indirectly proves that 2-methylimidazole is the skeleton of the precursor structure and 5-aminotetrazolyl is the defective ligand, which is consistent with the extremely low yield of comparative example 1. Figure 1 It can be seen from b that in the X-ray diffraction patterns of FeN4, FeN4-SM3, FeN4-SM, and FeN4-SM5, only the diffraction peaks of carbon (002) and (101) crystal planes appear at 26° and 44°, which preliminarily indicates the absence of iron nanoparticles.
[0060] The high-resolution transmission electron microscopy images of FeN4-SM prepared in Example 1, FeN4-SM3, FeN4-SM5 and FeN4 prepared in Comparative Examples 2, 3 and 4 are shown in FIG. Figure 2 As shown, Figure 2The columns from left to right are FeN4-SM, FeN4, FeN4-SM3 and FeN4-SM5. Figure 2 It can be seen that the introduction of 5-ATZ causes the prepared catalyst to gradually develop holes and eventually form pores. The pore size increases with the increase of 5-ATZ concentration. The generation of pores originates from the thermal instability of the 5-ATZ linker as a defective ligand in the nitrogen-doped carbon support. The micropores in the crystal will produce crystal defects under high temperature conditions, and then form mesopores with independent open pores to enhance the transfer of oxygen-containing species and electrolytes, which also proves the possible existence of CN cracking. At the same time, it is proved that the proportion of 5-aminotetrazole ligand is too large, resulting in the collapse of the catalyst pore structure, which is not conducive to the exposure of active sites. The scanning electron microscopy of FeN4-SM prepared in Example 1 is as follows Figure 3 It is shown that the prepared FeN4-SM appears as three-dimensional defect spheres assembled from nanosheets.
[0061] The high-resolution transmission electron microscopy of FeN4-DH prepared in Comparative Example 5 is as follows: Figure 4 As shown, from Figure 4 It can be seen that in the direct heating process, the catalyst has no obvious pores, which indicates that the direct thermal decomposition of 5-aminotetrazolyl results in insufficient gas generation, insufficient pore formation, and insufficient formation of a stable pore structure.
[0062] The high-angle annular dark field scanning transmission electron microscope and elemental surface scanning analysis of FeN4-SM prepared in Example 1 are shown in Figure 2. Figure 5 As shown. Figure 5 It can be seen that there are no metal-containing nanoparticles in the prepared catalyst, and the energy dispersive X-ray spectroscopy (EDS) results show the uniform distribution of Fe elements in the carbon substrate, without the appearance of metal nanoclusters and particles, which indicates that the iron elements are atomically dispersed rather than aggregated together.
[0063] The nitrogen adsorption and desorption isotherms of FeN4-SM prepared in Example 1 and FeN4 prepared in Comparative Example 4 are as follows: Figure 6 The corresponding pore size distribution curve is shown in Figure 7 FeN4-SM exhibits obvious IV-type hysteresis loop characteristics, proving its hierarchical porous structure with coexistence of micropores and mesopores. The specific surface area of FeN4-SM is 477.12 m 2 g -1 , with a large accessible surface area, which can expose a large number of single-atom Fe sites and allow rapid mass transfer of reactants.
[0064] The aberration-corrected high-angle annular dark-field scanning transmission electron microscope of the FeN4-SM prepared in Example 1 is as follows: Figure 8As shown, many isolated bright spots were accurately identified, indicating that the iron elements were atomically dispersed rather than clustered together.
[0065] The C1s high-resolution spectra of the X-ray photoelectron spectra of FeN4-SM prepared in Example 1, FeN4-SM3, FeN4-SM5 and FeN4 prepared in Comparative Examples 2, 3 and 4 are as follows: Fig. 9 As shown in the figure, the Fe 2p high-resolution spectrum is shown in Fig.10 As shown in the figure, the high-resolution XPS spectrum of C1s is subjected to peak fitting processing. The deconvoluted high-resolution C1s spectrum has three N species, corresponding to CC (284.6 eV), CN (285.5 eV) and C=O (288.0 eV). X The obvious positive shift of the peaks proves that the electronic structure of the atomically dispersed Fe sites has changed, which is also confirmed by the high-resolution Fe 2p spectrum. The cleavage of the CN bond adjacent to Fe-N4 may be the reason for the increase in the binding energy of the Fe-N bond, which is consistent with the TEM images. It is worth noting that during the pore expansion process, a synchronous decrease in the CN content and the pyridinic N content can be observed, which indicates that the gaseous products produced during the pyrolysis of 5-ATZ may trigger the selective cleavage of the CN bond, which first occurs on the pyridinic N.
[0066] The FeN4-SM prepared in Example 1 and the FeN4 prepared in Comparative Example 4 13 C NMR spectroscopy Fig.11 As shown, two broad peaks were observed at δ = 110-190 and 70-100 ppm for FeN4 and FeN4-SM, corresponding to sp 2 -hybridized graphitic carbon structure and N-alkyl carbon (denoted as C*). In contrast, the peak intensity of N-alkyl carbon (C*) in FeN4-SM begins to weaken, and a new N-alkyl carbon peak (denoted as C*) appears at δ = 45-70 ppm. # ), which is related to the cleavage of C=N and CN bonds in graphitic N and pyridinic N. Due to the cleavage of CN bonds, FeN4-SM shows sp at δ = 20-40 ppm. 3 The signal peaks of the -hybridized carbon structure are also found, which in turn weakens the resonance of the N-alkyl carbon. The results show that the CN bond undergoes selective cleavage during the entire pore expansion process, which is consistent with the results of X-ray photoelectron spectroscopy.
[0067] The X-ray absorption near-edge structure and extended X-ray absorption fine structure analysis of FeN4-SM prepared in Example 1 are as follows: Fig.12 As shown. Fig.12 It can be seen from a that the near absorption edge of FeN4-SM is located between FeO and Fe2O3, which proves that the positively charged Feδ+ species (3>δ>2). In order to obtain reliable structural information, the least squares EXAFS curve fitting analysis was further performed, such as Fig.12 The best fitting result shows that The peak centered at t and Fe-N2 c The double scattering paths have coordination numbers of 2.33 and 1.98 and distances of 1.75 and These results show that the Fe-NC configuration has different bond lengths, which is consistent with the theoretical calculation model of FeN4-SM. Combining the synchrotron radiation and spherical aberration electron microscopy data results, the structural model is as follows Fig.13 As shown in the differential charge density diagram, it can be seen that the asymmetric electronic structure leads to the charge difference of the ligand N atom, thus forming an asymmetric electron cloud in the Fe site. The resulting tensile and compressive strains regulate the dp orbital hybridization of Fe / O and reduce the adsorption affinity to the intermediate. All the above evidence confirms that it is feasible to adjust the atomic strain environment of the iron metal center through selective CN cleavage to improve the acidic oxygen reduction activity and reduce the adsorption strength of *OH.
[0068] The in-situ Raman spectra of FeN4-SM prepared in Example 1 and FeN4 prepared in Comparative Example 4 are shown in FIG. Fig.14 As shown in a and b, with the decrease of the applied potential, the ions at 1150 and 1550 cm-1 were detected in FeN4 and FeN4-SM, respectively. -1 The peak centered on corresponds to the stretching vibrations of *OO and *OOH, which verifies that the catalyst performs oxygen reduction reaction by a correlation mechanism. Due to the short lifetime of oxygen-containing intermediates, the formation of intermediates mainly occurs at low potentials. Therefore, Raman signals from intermediates are usually observed after the onset of ORR. Fig.14 c analysis shows that the increase in the red-shift position and the main peak height indicates that the interaction strength between the Fe atom center of FeN4-SM and *OOH is weakened. Therefore, the result that asymmetric atomic strain will cause changes in the stretching vibration frequency of the Fe-O bond has been verified, which is beneficial to the desorption of oxygen-containing intermediates.
[0069] The FeN4-SM prepared in Example 1 and the FeN4-SM3, FeN4-SM5 and FeN4 prepared in Comparative Examples 2, 3 and 4 were used to evaluate the electrocatalytic activity of the catalysts using a rotating ring disk electrode measurement method in a 0.1M KOH electrolyte. A three-electrode test system was used, with a glassy carbon electrode as the working electrode, Ag / AgCl as the reference electrode, and a Pt mesh as the counter electrode. The staged cyclic voltammetry test was performed at a speed of 1600 rpm and a voltage range of 1.20-0.05 V (vs. RHE). Fig.15As shown in the figure, it can be seen from the oxygen reduction polarization curve that FeN4-SM has the best half-wave potential, reaching 0.948V (vs.RHE), which is higher than 0.927V (vs.RHE) of FeN4, and the limiting current density is much higher than that of FeN4.
[0070] The electrocatalytic activity of the FeN4-SM prepared in Example 1 and the catalyst of the comparative example was evaluated in 0.1M HClO4 electrolyte using a rotating ring disk electrode measurement method. The obtained step cyclic voltammetry curves are shown in FIG. Fig.16 As shown. Fig.16 From the cyclic voltammetry curve in a, it can be seen that the half-wave potential of FeN4-SM is 0.83V (vs. RHE). Fig.16 As can be seen from b, the kinetic current density of FeN4-SM catalyst at 0.8V (12.94mAcm -2 ) is more than 2.15 times higher than that of FeN4, which indicates that the geometric structure modulation has an enhancement effect.
[0071] The electrochemical stability of the FeN4-SM prepared in Example 1 was evaluated by accelerated cyclic voltammetry test, and the polarization curve obtained was as follows: Fig.17 As shown. Fig.17 It can be seen that after 60,000 times of accelerated cycle aging, the half-wave potential of FeN4-SM only shifted negatively by 16 mV, proving that the catalyst has excellent stability.
[0072] The FeN4-SM prepared in Example 1 and the FeN4 prepared in the comparative example were used in proton exchange membrane fuel cells, and proton exchange membrane fuel cells (PEMFCs) with Pt / C as anode were assembled to evaluate the application prospects of FeN4-SM. The obtained polarization curves are shown in FIG. Fig.18 As shown. Fig.18 It can be seen that under the condition of H2 / O2 with a back pressure of 2.0 bar, the peak power density of the FeN4-SM-based fuel cell reaches 862 mW cm -2 , exceeding the 640mW cm of FeN4 -2 For FeN4-SM, the current density reaches 418 mA cm at 0.7 V. -2 , exceeding the 383 mA cm of FeN4 -2 It is shown that FeN4-SM with asymmetric atomic strain environment has excellent PEMFC performance and has good commercial application prospects.
[0073] Example 2: This example is to prepare MnN4-SM. The difference between this example and Example 1 is that the "50 mg of ferrous sulfate heptahydrate" in step three is replaced by "12 mg of manganese chloride tetrahydrate", and the other steps and parameters are the same as those in Example 1, to obtain an atomically dispersed non-precious metal catalyst based on defective ligands, represented by MnN4-SM.
[0074] The transmission EDS surface scanning analysis diagram of MnN4-SM prepared in Example 2 is as follows: Fig.19 As shown. Fig.19 It can be seen that there are no metal-containing nanoparticles in the prepared catalyst. The energy dispersive X-ray spectroscopy (EDS) results show that the Mn element is evenly distributed in the carbon carrier. The Mn element is atomically dispersed rather than aggregated together, which preliminarily proves that there are no metal nanoclusters and particles.
[0075] The electrocatalytic activity of the MnN4-SM catalyst prepared in Example 2 was evaluated in a 0.1M KOH electrolyte using a rotating ring disk electrode measurement method. A three-electrode test system was used, with a glassy carbon electrode as the working electrode, Ag / AgCl as the reference electrode, and a Pt mesh as the counter electrode. The catalyst was first activated (CV) using a cyclic voltammetry test, and then a staged cyclic voltammetry test was performed at a speed of 1600r and a voltage range of 1.20-0.05V (vs.RHE). The obtained oxygen reduction polarization curve is shown in FIG. Fig. 20 As shown. Fig. 20 It can be seen that MnN4-SM also exhibits excellent oxygen reduction performance in alkaline electrolyte, and its half-wave potential reaches 0.933V.
[0076] The present invention utilizes the strain effect constructed by CN cracking to break the electronic symmetry of the square planar transition metal MN4 active center, utilizes the asymmetric electronic structure to improve the adsorption between the M site and the oxygen-containing intermediate to improve the ORR activity, and simultaneously utilizes a stepped high-temperature heat treatment to generate a multi-level pore structure to improve the accessibility of the single-atom metal site, thereby improving the stability and reaction rate of the catalyst, and promoting the application of nitrogen-doped porous carbon-supported single-atom transition metal catalysts (MNCs) in the fields of energy conversion and storage.
Claims
1. A non-precious metal catalyst based on atomically dispersed defective ligands, characterized in that: The catalyst is composed of MN4 embedded in a carbon support, where M is coordinated with N in two sets of different MN bond lengths, showing 2N t =M=2N c Coordination structure, wherein t represents tension, c represents compression, the mass fraction of M is 0.5% to 1%, and M is Fe, Mn, Co or Ni.
2. A method for preparing a non-precious metal catalyst based on atomically dispersed defective ligands according to claim 1, characterized in that The method proceeds as follows:
1. Preparation of a three-dimensional nitrogen-doped porous defective flower-like carbon carrier precursor: Dissolve a zinc source and a nitrogen source in methanol respectively, then mix them, stir rapidly and vigorously for 2 to 2.5 hours, and keep them at 60 to 65° C. for 2 to 2.5 hours to produce a white suspension in the solution; then centrifuge, wash, and dry to obtain a three-dimensional nitrogen-doped porous defective flower-like carbon carrier precursor, which is a white powder; wherein the nitrogen source is 5-aminotetrazole and 2-methylimidazole in a molar ratio of 1:(3 to 5); 2. Preparation of nitrogen-doped porous carbon carrier: The precursor prepared in step 1 is subjected to a stepwise high-temperature heat treatment under an inert atmosphere, and cooled to room temperature to obtain a nitrogen-doped porous carbon carrier; wherein the stepwise high-temperature heat treatment is: firstly heating to 200-220°C and maintaining for 0.5-0.6h, then heating to 400-420°C and maintaining for 0.5-0.6h, then heating to 700-720°C and maintaining for 1-1.3h, and finally heating to 1000-1050°C and maintaining for 2-2.5h; 3. Preparation of single-atom catalyst precursor: first, immerse the nitrogen-doped porous carbon support into a soluble salt solution of metal M, vigorously stir for 2 to 2.5 hours under an inert atmosphere, then ultrasonically disperse for 2 to 2.5 hours, filter or centrifuge, and dry the solid phase to obtain a single-atom catalyst precursor; 4. Preparation of single-atom catalysts: Place the single-atom catalyst precursor in a furnace, raise the temperature to 950-1050°C in an argon atmosphere, and heat treat for 2-3 hours to obtain an atomically dispersed non-precious metal catalyst based on defective ligands.
3. The method for preparing a non-precious metal catalyst based on atomic-level dispersion of defective ligands according to claim 2, characterized in that: The zinc source in step 1 is zinc acetate dihydrate, anhydrous zinc nitrate or zinc nitrate hexahydrate.
4. A method for preparing a non-precious metal catalyst based on atomic-level dispersion of defective ligands according to claim 2 or 3, characterized in that: The inert atmosphere described in step 2 and step 3 is Ar or N2.
5. The method for preparing a non-precious metal catalyst based on atomic-level dispersion of defective ligands according to claim 2 or 3, characterized in that: The drying described in step 1 and step 3 is vacuum drying at a temperature of 60 to 80° C. for 6 to 8 hours.
6. A method for preparing a non-precious metal catalyst based on atomic-level dispersion of defective ligands according to claim 2 or 3, characterized in that: The solvent of the metal M soluble salt solution described in step 3 is N,N-dimethylformamide.
7. A method for preparing a non-precious metal catalyst based on atomic-level dispersion of defective ligands according to claim 2 or 3, characterized in that: The vigorous stirring described in step 3 has a stirring speed of 500-700 rpm.
8. The method for preparing a non-precious metal catalyst based on atomic-level dispersion of defective ligands according to claim 2 or 3, characterized in that: The heating rate in step 4 is 5-20℃min -1 .
9. The use of a non-precious metal catalyst based on atomic-level dispersion of defective ligands as claimed in claim 1, characterized in that The application is to use atomically dispersed non-precious metal catalysts based on defective ligands as cathode catalysts in proton exchange membrane fuel cells or metal-air batteries.
Citation Information
Patent Citations
Dissimilar metal atom pair catalyst and preparation method and application thereof
CN115064705A
Monatomic electrocatalyst containing defects and application thereof
CN117080469A
Precious metal nanoparticle synergistic transition metal monatomic catalyst, preparation and application
CN117497787A
Non-platinum group metal electrocatalysts using metal organic framework materials and method of preparation
US20120077667A1
Non-noble metal based catalyst and method of manufacturing the same
US20180175395A1
Cited By
Zinc metal organic framework material as well as preparation method and application thereof
CN120484272A