Carbon-plastic composite bipolar plate for all-vanadium redox flow battery and preparation method of carbon-plastic composite bipolar plate

Through the wet mix hot pressing curing process of carbon plastic composite bipolar plates, combined with the design of conductive auxiliary materials and carbon blanks, the problems of taking into account the conductivity and mechanical properties of the bipolar plates of all vanadium liquid flow battery are solved, and efficient conductivity is achieved and mechanical properties improve and simplify production processes, suitable for large-scale production and large-scale manufacturing.

CN119008995AInactive Publication Date: 2024-11-22HYDROGEN TECH (FOSHAN) CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411018486.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing bipolar plate materials of all vanadium flow battery are difficult to take into account both conductivity, electrochemical stability and mechanical properties, and the preparation process is complex and not suitable for mass production, resulting in low conductivity and insufficient mechanical properties.

Method used

Using carbon plastic composite bipolar plate, wet mix composed of conductive carbon fillers, polymers, additives and carbon blanks is prepared by hot pressing curing, and the number and position of carbon blanks are adjusted to achieve controllability of different mechanical properties. , and construct a conductive network through conductive auxiliary materials to improve conductivity.

Benefits of technology

It achieves high conductivity (conductivity up to 200S/cm or above) and excellent mechanical properties (flexural strength up to 90MPa), and simplifies the preparation process, suitable for large-scale production and large-size bipolar plate manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008995A_ABST
    Figure CN119008995A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon-plastic composite bipolar plate for an all-vanadium redox flow battery and a preparation method of the carbon-plastic composite bipolar plate. The carbon-plastic composite bipolar plate is obtained by hot-pressing and curing a wet mixed material and a carbon blank, wherein the wet mixed material comprises a conductive carbonaceous filler, a polymer, an auxiliary agent and a solvent. By adding the conductive auxiliary material and the auxiliary agent, the dispersion uniformity of the conductive carbonaceous filler and the flowability of the composite material are improved, and the conductivity of the bipolar plate is enhanced; the added carbon blank enhances the mechanical property of the bipolar plate, and various conductive carbonaceous fillers are uniformly mixed in different mixing modes, so that the internal consistency of the bipolar plate is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery manufacturing, and in particular to a carbon-plastic composite bipolar plate for a large-sized all-vanadium liquid flow battery with high conductivity, high mechanical properties, and a preparation method thereof. Background Art

[0002] Among various energy storage systems, all-vanadium flow batteries have attractive features such as high energy power, long cycle life, easy expansion, good recyclability, and zero cross-contamination of active components. They are one of the most popular energy storage technologies in power grid applications. In the all-vanadium flow battery system, the battery stack composed of multiple single cells in series is the core component, which is composed of key components such as bipolar plates, current collectors, ion conductive membranes, electrodes and end plates.

[0003] As a multifunctional key component in the all-vanadium liquid flow battery system, the bipolar plate can collect and conduct the current generated during the battery charging and discharging process, provide effective mechanical support for the membrane and electrode, connect multiple single cells and prevent the mixing of positive and negative electrolytes and direct contact of electrodes, which has a significant impact on the energy efficiency of the battery stack. Therefore, the ideal bipolar plate material usually needs to have good conductivity, electrochemical stability, corrosion resistance and a certain mechanical strength, etc., but it is often difficult to take into account all these characteristics.

[0004] Bipolar plate materials are mainly divided into three types according to the composition of the materials: metal bipolar plates, graphite bipolar plates and carbon-plastic composite bipolar plates. In all-vanadium liquid flow batteries, the use of highly corrosive vanadium electrolytes severely limits the material selection for the development of bipolar plates. Metal bipolar plates exhibit extremely poor chemical stability in corrosive vanadium electrolytes, while graphite bipolar plates have problems such as high manufacturing costs, poor mechanical strength, easy expansion and electrolyte leakage. Carbon-plastic composite bipolar plates have the advantages of good corrosion resistance, excellent mechanical properties, easy molding, low cost, simple production, and one-step flow channel molding. They can be used as an alternative material to metal and graphite bipolar plates in all-vanadium liquid flow batteries.

[0005] Carbon-plastic composite bipolar plates are usually made of a polymer resin matrix (thermoplastic and thermosetting) mixed with carbon fillers through compression molding, injection molding and casting processes. However, since the conductivity of carbon-plastic composite bipolar plates is lower than that of metal or graphite bipolar plates, when the number of charge and discharge cycles is small, the carbon in the bipolar plates will not be completely consumed due to the low current density, but will leave some gaps between the two plates. These gaps will cause a large amount of heat to be generated when the current passes through, thereby further increasing the resistance of the bipolar plates. Therefore, the preparation of bipolar plates with high conductivity and good corrosion resistance has become an important research direction for current collectors for all-vanadium liquid flow batteries.

[0006] Chinese patents CN 113980377 A, CN 113956498 A, and CN 113921844 A all adopt chemical reaction to modify and graft expanded graphite, thereby forming a better conductive path and improving the conductivity and mechanical properties of the plate. The disadvantages of this method are as follows: chemical grafting modification has the hidden danger of whether the reaction is complete, thus causing performance defects.

[0007] Chinese patent CN 110676479 A provides a method for preparing a bipolar plate for an all-vanadium liquid flow battery, the preparation method comprising the following steps: coating the surfaces of both sides of the conductive carbon fiber with a conductive composite adhesive, laminating the surfaces of both sides of the conductive carbon fiber with flexible graphite paper through the conductive composite adhesive, and repeating the above steps to form different thicknesses, and then placing the plates in a flat hot press for hot pressing and curing to prepare the bipolar plates for an all-vanadium liquid flow battery. The disadvantages of this method are as follows: the method requires multiple layers of hot pressing and laminating, which is prone to stratification, reduces mechanical properties, increases in-plane contact resistance, and thus increases conductivity, and the process is complex and not suitable for mass production, and has low economic efficiency. Summary of the invention

[0008] In view of the shortcomings of the prior art in all-vanadium liquid flow battery bipolar plates, the first object of the present invention is to provide a carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery, which has the characteristics of high electrical conductivity, excellent mechanical properties and large size, and can achieve controllability of different mechanical properties by regulating the number of carbon blanks in the bipolar plate and their position in the wet mixture.

[0009] The second object of the present invention is to provide a method for preparing carbon-plastic composite bipolar plates for all-vanadium redox flow batteries with simple operation, mild conditions and low production cost. The preparation process is simple, easy to produce on an assembly line, conducive to large-scale production, and due to wet molding, it is not limited by the size of the molding die and the table, and large-sized bipolar plates can be produced.

[0010] In order to achieve the above technical objectives, the present invention provides a carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery, wherein the composite bipolar plate is obtained by hot pressing and curing a wet mixture including a conductive carbon filler, a polymer, an additive, and a solvent and a carbon blank.

[0011] The present invention enhances the mechanical properties of the bipolar plate by adding a carbon blank. The carbon blank is a carbon fiber composite paper, in which the main material is carbon fiber. The carbon fiber particles are rigid and have a strong preferential bearing capacity. The entire carbon blank is like a piece of tough "cloth". Therefore, after the carbon blank is added to the wet mixture to make a plate, the composite material is not easy to break under the action of external force, and the mechanical properties such as bending and compression resistance are enhanced. Secondly, the present invention can achieve the controllability of different mechanical properties by regulating the number of carbon blanks and the position in the wet mixture. For example, when the number of carbon blanks is greater than 1, the carbon fiber therein will be exposed on the surface of the plate, and at this time, the contact resistance between the carbon felt electrode and the bipolar plate can be well reduced. At the same time, by adding additives to improve the dispersion uniformity of the conductive carbon filler and the fluidity of the composite material, the conductivity and uniformity of the bipolar plate are greatly enhanced. Finally, the carbon blank and the wet mixture can be formed into a tight whole by hot pressing and curing, which further ensures the comprehensive performance of the composite bipolar plate.

[0012] As a preferred solution, the total thickness of the wet mixture in the mold during hot pressing and curing is H, the length and width of the carbon blank are consistent with the mold, and when the number of carbon blanks is 1, the position of the carbon blank in the wet mixture is H / 2; when the number of carbon blanks is N, the position of the first carbon blank in the wet mixture is 0, and the subsequent carbon blanks are H / (N-1) away from the first carbon blank, where N is a natural number greater than 1, and the maximum value of N is limited by the total mass of the carbon blank, which is less than or equal to 10% of the dry weight of the composite bipolar plate.

[0013] An important feature of the present invention is that the different mechanical properties of the composite bipolar plate can be controlled by adjusting the number of carbon blanks and their positions in the wet mixture, as follows:

[0014] (1) When the number of carbon blanks is 1, the carbon blank is located at H / 2 of the wet mixture. At this time, the external force first acts on the surface of the plate. Since the mechanical properties of the plate surface are mainly reflected by the polymer material itself, the surface may be broken but the middle is still connected. At this time, the upper and lower surfaces are evenly stressed.

[0015] (2) When the number of carbon blanks is greater than 1, the position of the carbon blanks will be symmetrical with the middle as the axis of symmetry. At this time, there will be one carbon blank on the upper and lower surfaces of the electrode plate. When external force is applied, it will first act on the carbon blank on the surface, and the mechanical properties will be enhanced through the toughness of the carbon blank.

[0016] The inventors found that if the carbon blanks are not arranged in the wet mixture according to the position rule of the present invention, the toughness of the carbon blanks themselves will also enhance the mechanical properties of the plate. However, due to the uncertainty of their positions, the mechanical properties of various parts of the plate will be inconsistent. At the same time, when the number of carbon blanks is 1, if the carbon blanks are not located on the surface, their conductivity will not be enhanced and the contact resistance will not be reduced.

[0017] As a preferred solution, the carbon blank is a raw carbon blank and / or a sprayed carbon blank; the single carbon blank has a gram weight of 5 to 20 g / cm 2 , such as 5g / cm 2 、10g / cm 2 , 15g / cm 2 or 20g / cm 2 As the gram weight increases, the mechanical strength of the carbon blank will increase under the same area, thereby increasing the mechanical properties of the plate under the same number of sheets.

[0018] As a preferred solution, the wet mixture is composed of the following raw materials by weight: 20-40 parts of conductive carbon filler, 5-30 parts of polymer; 5-15 parts of additives; 50-70 parts of solvent. The amount of each component in the wet mixture of the present invention has a certain influence on the comprehensive performance of the composite bipolar plate. For example, when the total amount of solid components (conductive carbon filler, polymer and additives) is different, it will affect the thickness of the initial wet mixture: the total amount of solid components increases, and the thickness of the initial wet mixture decreases; and when the total amount of solid components is constant, within a limited range, the increase in the amount of conductive carbon filler will enhance the conductivity of the manufactured plate, but at the same time, the reduction in the amount of polymer will reduce the mechanical properties of the manufactured composite bipolar plate and weaken the bonding force; the change in the amount of additives will affect the leveling and viscosity of the wet mixture and increase the processability, and the increase in its amount will reduce the viscosity and improve the leveling, etc.

[0019] As a preferred solution, the conductive carbon filler is composed of expanded graphite and conductive auxiliary materials; the conductive auxiliary materials are at least one of conductive carbon black, carbon nanotubes and graphene; the conductive carbon black is at least one of Ketjen black, acetylene black and superconducting carbon black. The conductive auxiliary materials selected in the present invention can all construct a good conductive network for the composite bipolar plate.

[0020] As a preferred solution, the polymer is at least one of phenolic resin, boron phenolic resin, bisphenol A epoxy resin, polyethylene, polypropylene, polyvinylidene fluoride, polyphenylene sulfide and polyaniline.

[0021] As a preferred solution, the solvent is anhydrous ethanol.

[0022] As a preferred solution, the auxiliary agent is composed of a film former, a coupling agent and a surfactant; the film former includes polyvinyl alcohol and / or polyvinyl pyrrolidone; the coupling agent includes a titanate coupling agent; and the surfactant includes N-methylpyrrolidone. The auxiliary agent selected in the present invention can significantly improve the dispersion uniformity of the conductive carbon filler and the fluidity of the composite material, thereby enhancing the conductivity of the composite bipolar plate.

[0023] The present invention also provides a method for preparing a carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery, the method comprising the steps of ball-milling a conductive carbonaceous filler and adding the resultant to a polymer, an additive and a solvent in batches to obtain a wet mixture; alternately pouring the wet mixture and the carbon blank into a hot pressing mold, and obtaining a polar plate after drying; and hot-pressing and curing the polar plate to obtain the resultant.

[0024] As a preferred solution, the present invention provides a method for preparing a carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery, which specifically comprises the following steps:

[0025] 1) preparing a wet mixture I of a polymer, an additive and a solvent and a dry mixture of a conductive carbonaceous filler respectively;

[0026] 2) adding the dry mix to the wet mix I in batches to obtain a wet mix II;

[0027] 3) alternately pouring the wet mixed material II and the carbon blank into a hot pressing mold, and obtaining the electrode plate after drying;

[0028] 4) The electrode plate is cured by hot pressing.

[0029] The conductive carbon filler of the present invention is obtained by ball-milling and dry-mixing the conductive auxiliary material and the main material expanded graphite to obtain a dry material, and then mixing the dry material and the wet mixture under high-speed stirring, so that various conductive carbon materials can be mixed evenly, and at the same time, by adding in batches, the consistency inside the prepared bipolar plate can be well guaranteed.

[0030] As a preferred solution, the conditions for hot pressing curing are: temperature of 160-300°C and pressure of 3-5MPa. Under the same polymer mass fraction, increasing the curing temperature and curing pressure within the scope of the present invention can improve the bending strength of the material, but will reduce the electrical conductivity of the material; since the carbon-plastic composite bipolar plate requires both excellent mechanical properties and excellent electrical conductivity, the present invention can select polymer types according to different needs to match the conditions of hot pressing curing.

[0031] As a preferred solution, the ball milling conditions are: a rotation speed of 300-500 r / min and a time of 0.5-1.5 h. The expanded graphite main material and the conductive auxiliary material in the conductive carbon filler can be fully mixed by ball milling to ensure the uniformity of conductivity.

[0032] As a preferred solution, when the conductive carbon filler is added in batches, the rotation speed of each batch is 1000-1500r / min and the time is 10-15min. The rotation speed will affect the interval time of each batch. Within the limit, the faster the rotation speed, the shorter the time; and under the same rotation speed condition, the longer the ball milling time, the greater the uniformity of material mixing, but there is an upper limit to the time. After this value, the increase in time will not affect the uniformity of the material.

[0033] As a preferred solution, the mixing stirring speed is 1000-1800 r / min.

[0034] As a preferred solution, the drying temperature is 40-50°C.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1) The carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery provided by the present invention constructs a good conductive network by adding a conductive auxiliary material to the conductive carbonaceous filler; at the same time, adding an auxiliary agent to the wet mixture improves the dispersion uniformity of the conductive carbonaceous filler and the fluidity of the composite material, thereby greatly enhancing the conductivity of the bipolar plate (the conductivity can reach more than 200S / cm).

[0037] 2) The present invention provides a method for preparing a carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery. By performing ball milling dry mixing between auxiliary materials and main materials and adding conductive carbonaceous fillers to the wet mixture in batches, various conductive carbonaceous materials can be mixed evenly, which can well ensure the internal consistency of the prepared bipolar plate.

[0038] 3) The present invention enhances the mechanical properties of the bipolar plate by adding carbon blanks (bending strength can reach 90MPa), and at the same time achieves controllability of different mechanical properties by regulating the number of carbon blanks and their position in the wet mixture. When the carbon fibers of the carbon blanks are exposed on the surface of the plate, the contact resistance between the carbon felt electrode and the bipolar plate can be greatly reduced.

[0039] 4) The preparation method of the present invention has a simple process and is easy to produce in an automated production line, which is conducive to large-scale production. Moreover, due to the wet molding, it is not limited by the size of the molding die and the table, and large-sized bipolar plates can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a process flow chart of a method for preparing a carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery in Example 1.

[0041] Figure 2 This is a cross-sectional view of the carbon-plastic composite bipolar plate for the all-vanadium liquid flow battery prepared in Example 1. From the cross-sectional view, it can be observed how tightly the carbon blank is combined with other parts when placed inside the plate. DETAILED DESCRIPTION

[0042] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the following specific embodiments. Obviously, the embodiments described below are only a part of the embodiments, and all other embodiments obtained by professionals in this field without creative work still belong to the protection scope of the present invention.

[0043] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0044] Example 1

[0045] This embodiment is a carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery, which is prepared from the following raw materials by mass percentage: 64% anhydrous ethanol, 20% expanded graphite, 0.5% graphene, 3% N-methylpyrrolidone, 2% polyvinylpyrrolidone, 0.5% titanate coupling agent, and 10% boron phenolic resin; the carbon blank is a green carbon blank with a gram weight of 5g / cm 2 , 1 sheet, the total mass of the carbon blank is less than 10% of the dry weight of the composite bipolar plate.

[0046] The preparation method of a carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery in this embodiment is as follows:

[0047] Add boron phenolic resin, N-methylpyrrolidone, polyvinylpyrrolidone and anhydrous ethanol into a beaker in proportion, place it on a magnetic stirrer for constant temperature heating at 40°C, and stir and mix it in a high-speed stirrer at a speed of 1200r / min;

[0048] Graphene and expanded graphite were dry-mixed and ball-milled in proportion, with a ball mill speed of 300 r / min for 1 h;

[0049] Add the dry material to the wet material in 4 batches and place it in a high-speed mixer at a speed of 1500r / min, with an interval of 10min between each batch, for a total of 40min;

[0050] Pour the wet material into the leveling mold with a thickness of 1.6mm, put the green carbon blank into the mold, spread it on the wet material, and introduce the wet material again on the green carbon blank with a thickness of 1.6mm. Use the pressing plate to squeeze it first to ensure that the wet material is immersed in the carbon blank; after leveling, put the mold into the oven at 50℃ for 2h;

[0051] The dried electrode plate was hot pressed and cured at a press temperature of 160°C and a pressure of 3 MPa.

[0052] The manufactured bipolar plate was tested and its conductivity was 143S / cm and its bending performance could reach 66MPa.

[0053] Example 2

[0054] This embodiment is a carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery, which is prepared from the following raw materials by mass percentage: 57% anhydrous ethanol, 22% expanded graphite, 1% Ketjen black, 7% N-methyl pyrrolidone, 2% polyvinyl alcohol, 1% titanate coupling agent, and 10% phenolic resin; the carbon blank is a green carbon blank with a gram weight of 5g / cm 2 , 2 sheets; the total mass of the carbon blank is less than 10% of the dry weight of the composite bipolar plate.

[0055] The preparation method of a carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery in this embodiment is as follows:

[0056] Phenolic resin, N-methylpyrrolidone, polyvinyl alcohol and anhydrous ethanol were added into a beaker in proportion, placed on a magnetic stirrer for constant temperature heating at 40°C, and stirred and mixed in a high-speed stirrer at a speed of 1200 r / min;

[0057] Ketjen black and expanded graphite were dry-mixed and ball-milled in proportion, with a ball mill speed of 300 r / min for 1 h;

[0058] Add the dry material to the wet material in 4 batches and place it under a high-speed mixer at a speed of 1800r / min, with an interval of 10min between each batch, for a total of 40min;

[0059] Place a green carbon blank into the leveling mold, pour the wet material into the green carbon blank with a thickness of 2.12mm, and place another green carbon blank on the wet material; use a pressing plate to squeeze first to ensure that the wet material is immersed in the carbon blank; after leveling, place the mold in an oven at 50℃ for 2 hours;

[0060] The dried electrode plate is heat-pressed and cured at a press temperature of 180°C and a pressure of 5 MPa.

[0061] The manufactured bipolar plate was tested and its conductivity was 210S / cm and its bending performance could reach 92MPa.

[0062] Example 3

[0063] The difference between this embodiment and embodiment 1 is that the conditions for hot pressing curing are changed to a press temperature of 180° C. and a pressure of 3 MPa.

[0064] The manufactured bipolar plate was tested, and its conductivity was 152S / cm and its bending performance was 42MPa.

[0065] Comparative Example 1

[0066] The difference between this comparative example and Example 1 is that the carbon blank is not placed in the middle, and the other steps and conditions are the same. The preparation process is as follows:

[0067] Pour the wet material into the leveling mold with a thickness of 3.2mm, put the raw carbon blank into the mold, spread it flat on the wet material, and use a pressing plate to squeeze it first to ensure that the wet material is immersed in the carbon blank; after leveling, put the mold into an oven and dry it at 50℃ for 2h; hot press and cure the dried plate with a press temperature of 160℃ and a pressure of 3MPa.

[0068] The manufactured bipolar plate was tested, and its conductivity was 138S / cm and its bending performance was 48MPa.

[0069] Comparative Example 2

[0070] The difference between this comparative example and Example 1 is that no carbon blank is added, and the other steps and conditions are the same.

[0071] The manufactured bipolar plate was tested and its conductivity was 141S / cm and its bending performance was 27MPa.

[0072] Comparative Example 3

[0073] The only difference between this comparative example and Example 1 is that no titanate coupling agent is added, and the other steps and conditions are the same.

[0074] The manufactured bipolar plate was tested and its conductivity was 97S / cm and its bending performance was 51MPa.

[0075] Comparative Example 4

[0076] The difference between this comparative example and Example 1 is that the conditions for hot pressing curing are changed to a press temperature of 160° C. and a pressure of 1 MPa, and the other steps and conditions are the same.

[0077] The manufactured bipolar plate was tested, and its conductivity was 72S / cm and its bending performance was 24MPa.

Claims

1. A carbon-plastic composite bipolar plate for an all-vanadium liquid flow battery, characterized in that: The carbon blank is obtained by hot pressing and curing a wet mixture including conductive carbon filler, polymer, additive and solvent.

2. The carbon-plastic composite bipolar plate for all-vanadium liquid flow battery according to claim 1, characterized in that: During the hot pressing and curing, the total thickness of the wet mixture in the mold is H, the length and width of the carbon blank are consistent with the mold, and when the number of carbon blanks is 1, the position of the carbon blank in the wet mixture is H / 2; when the number of carbon blanks is N, the position of the first carbon blank in the wet mixture is 0, and the subsequent carbon blanks are H / (N-1) away from the first carbon blank, where N is a natural number greater than 1, and the maximum value of N is limited by the total mass of the carbon blank, which is less than or equal to 10% of the dry weight of the composite bipolar plate.

3. The carbon-plastic composite bipolar plate for all-vanadium liquid flow battery according to claim 2, characterized in that: The carbon blank is a raw carbon blank and / or a sprayed carbon blank; the single carbon blank has a gram weight of 5 to 20 g / cm 2 .

4. The carbon-plastic composite bipolar plate for all-vanadium redox flow battery according to claim 1, characterized in that: The wet mixed material is composed of the following raw materials in parts by weight: 20 to 40 parts of conductive carbon filler, 5 to 30 parts of polymer, 5 to 15 parts of auxiliary agent, and 50 to 70 parts of solvent.

5. A carbon-plastic composite bipolar plate for an all-vanadium redox flow battery according to any one of claims 1 to 4, characterized in that: The conductive carbon filler consists of expanded graphite and conductive auxiliary materials.

6. The carbon-plastic composite bipolar plate for all-vanadium redox flow battery according to claim 5, characterized in that: The polymer is at least one of phenolic resin, boron phenolic resin, bisphenol A epoxy resin, polyethylene, polypropylene, polyvinylidene fluoride, polyphenylene sulfide and polyaniline; The auxiliary agent consists of a film-forming agent, a coupling agent and a surfactant; The film-forming agent includes polyvinyl alcohol and / or polyvinyl pyrrolidone; The coupling agent includes a titanate coupling agent; The surfactant includes N-methylpyrrolidone.

7. The method for preparing a carbon-plastic composite bipolar plate for an all-vanadium redox flow battery according to any one of claims 1 to 6, characterized in that: Conductive carbon fillers are ball-milled and then added to polymers, additives and solvents in batches to obtain a wet mixture; the wet mixture and carbon blanks are alternately poured into a hot pressing mold, and polar plates are obtained after drying; and the polar plates are hot-pressed and cured.

8. The method for preparing a carbon-plastic composite bipolar plate for an all-vanadium redox flow battery according to claim 7, characterized in that: The conditions for the hot pressing curing are: a temperature of 160 to 300° C. and a pressure of 3 to 5 MPa.

9. The method for preparing a carbon-plastic composite bipolar plate for an all-vanadium redox flow battery according to claim 8, characterized in that: The ball milling conditions are: a rotation speed of 300 to 500 r / min and a time of 0.5 to 1.5 h.

10. The method for preparing a carbon-plastic composite bipolar plate for an all-vanadium redox flow battery according to claim 9, characterized in that: The mixing stirring speed is 1000-1800 r / min.

Citation Information

Cited By

  • Composite bipolar plate for flow battery as well as preparation method and application of composite bipolar plate

    CN119858268A

  • High-strength graphite bipolar plate and preparation method thereof

    CN122314940A