NiCo-Li2Se lithium supplement additive for lithium iron phosphate positive electrode as well as preparation method and application of NiCo-Li2Se lithium supplement additive
NiCoSe2 was prepared by annealing of NiCo-ZIF with selenium powder by deriving NiCo-ZIF and selenium powder, and reacting with molten lithium to form NiCo-Li2Se lithium supplement additive, which solved the problem of poor reaction kinetics and lithium loss caused by Li2Se instability, and significantly improved iron phosphate The performance of lithium batteries is suitable for photovoltaic energy storage.
Patent Information
- Application Number
- CN202411194133.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-22
AI Technical Summary
The instability of Li2Se at room temperature in air limits its application in battery manufacturing, resulting in poor reaction kinetics and high lithium loss, affecting the battery's initial charging efficiency and energy density.
NiCoSe2 is prepared by annealing the transition metal NiCo-ZIF precursor with selenium powder by derivatizing the transition metal NiCo-ZIF precursor and annealing with selenium powder, and reacting with molten lithium to form NiCo-Li2Se lithium supplement additive, improving the reaction kinetics and stability of Li2Se in carbonate-based electrolytes sex.
NiCo-Li2Se lithium supplement additive significantly improves the initial charge and discharge capacity and energy density of lithium iron phosphate batteries, extends battery life, improves conductivity and stability, and is suitable for large-scale photovoltaic energy storage industries.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium ion battery materials, and specifically relates to a lithium iron phosphate positive electrode NiCo-Li 2 Se lithium supplement additive and preparation method and application thereof. Background Art
[0002] With the rapid development of renewable energy power generation industries such as wind power and photovoltaic power generation, the problem of abandoned solar and wind power generation is becoming increasingly serious. Energy storage batteries can store the energy of photovoltaic power generation systems and supply power to loads when there is insufficient sunshine, at night, and in emergency situations. Among various energy storage batteries, lithium iron phosphate (LiFePO 4 ) batteries have the characteristics of large input and output power, wide operating temperature range, long service life (> 2000 times), no memory effect, abundant raw material reserves, and volume energy is 4-5 times that of traditional lead-acid batteries, which can greatly reduce the space occupied by batteries. It is the best choice for practical application of photovoltaic energy storage lithium batteries. However, like other lithium-ion batteries, LiFePO 4 During the first charge process, the organic electrolyte decomposes on the surface of the negative electrode to form a solid electrolyte interface (SEI) layer, which permanently consumes a large amount of positive electrode lithium (5-20%), resulting in a low initial coulombic efficiency (ICE), and ultimately reducing the energy density of the entire battery.
[0003] Pre-lithiation technology can minimize the loss of lithium during the formation of SEI, including chemical pre-lithiation, electrochemical pre-lithiation, and the introduction of lithium supplement additives in the electrode, which all compensate for lithium loss by introducing additional active lithium ions into the system. The ideal positive electrode lithium supplement additive should have a high lithium supply capacity, an appropriate lithium extraction potential, and good compatibility with the battery system. It is mainly divided into lithium-rich compounds (such as Li 2 NiO 2 , Li 2 MoO 3 , Li 2 CuO 2 ), sacrificial lithium salts (such as Li 5 FeO 4 , Li 2 C 2 O 4 ) and binary compounds and their derivatives based on conversion reactions (including Li 2 O. Li 2 O 2 , Li 2 S. Li 3 N, LiF, Li 3 P and corresponding metal complexes). Lithium selenide (Li 2 Se) and Li 2S has similar properties, high theoretical volumetric capacity, suitable operating voltage window, compatibility with carbonate electrolytes, and higher than Li 2 The conductivity of S makes it a competitive cathode pre-lithiation material. 2 Se particles have poor reaction kinetics in carbonate-based electrolytes, and Li 2 The instability of Se in air at room temperature limits its application in battery manufacturing. Therefore, it is necessary to develop a Li-ion battery that can take into account high specific capacity, suitable voltage window, good compatibility, rapid reaction kinetics, and air stability. 2 Se-based additive materials are used in lithium iron phosphate battery systems. Summary of the invention
[0004] The purpose of the present invention is to provide a lithium iron phosphate positive electrode NiCo-Li 2 Preparation method of Se lithium supplement additive to solve Li 2 The instability of Se in air at room temperature limits its application in battery manufacturing.
[0005] Another object of the present invention is to provide a lithium iron phosphate positive electrode NiCo-Li 2 Se lithium supplement additive.
[0006] The third object of the present invention is to provide a lithium iron phosphate positive electrode NiCo-Li 2 Application of Se lithium supplement additives.
[0007] The technical solution of the present invention is: (one) A lithium iron phosphate positive electrode NiCo-Li 2 The preparation method of the Se lithium supplement additive comprises the following steps: A. Put Co(NO 3 ) 2 •6H 2 O and Ni (NO 3 ) 2 •6H 2 O was dissolved in methanol and 2-methylimidazole (C 4 H 6 N 2 ) is dissolved in methanol, and the two methanol solutions are mixed evenly by magnetic stirring, the speed of the magnetic stirrer is 300-400 rpm / min, the stirring time is 15-30 min, and then the mixture is allowed to stand at room temperature for 12-24 h, and then centrifuged and washed 3-5 times with methanol and dried to obtain NiCo-ZIF precursor powder; B. Mix NiCo-ZIF precursor powder with Se powder, grind thoroughly and anneal, and cool to room temperature after annealing to obtain NiCoSe2 ; C. In a glove box filled with argon, molten lithium foil and NiCoSe 2 The powders were mixed evenly in a stainless steel crucible at 150-180°C and stirred continuously for full reaction. After cooling naturally to room temperature, NiCo-Li 2 Se lithium supplement additive.
[0008] As a further improvement of the present invention, in step A, the molar ratio of Co to Ni is 1:1, and the amount of methanol is about the same as that of Co(NO 3 ) 2 •6H 2 O and Ni (NO 3 ) 2 •6H 2 The total amount ratio of O is 100~300ml:4mmol, and the total amount ratio of methanol to 2-methylimidazole is 100~200ml:40mmol.
[0009] As a further improvement of the present invention, in step A, vacuum drying is used for drying at a drying temperature of 60-80°C.
[0010] As a further improvement of the present invention, in step B, the mass ratio of NiCo-ZIF precursor powder to Se powder is 1:0.5-2.
[0011] As a further improvement of the present invention, in step B, the annealing conditions are: heating to 600-800° C. at a heating rate of 5-10° C. / min, and annealing at the temperature for 4-5 hours.
[0012] As a further improvement of the present invention, in step C, the lithium foil and the NiCoSe 2 The molar ratio is 1.80~7.25:1.
[0013] The present invention uses metal organic frameworks (MOFs) to obtain a transition metal NiCo-doped porous cubic framework (NiCo-ZIF), and obtains a binary metal selenide (NiCoSe) by mixing with selenium powder and annealing. 2 ), further through chemical conversion reaction with molten lithium foil to obtain NiCo-Li 2 Se lithium supplement additive, thus accelerating Li 2 Reaction kinetics of Se particles in carbonate-based electrolytes to enhance Li 2 The stability of Se during battery preparation process. NiCo-Li 2 Lithium iron phosphate batteries modified with Se lithium supplement additives have the advantages of high capacity, high energy density, long life, low cost, and environmental friendliness, and are expected to be used in the large-scale photovoltaic energy storage industry. (two) A lithium iron phosphate positive electrode NiCo-Li 2 Se lithium supplement additive, comprising the above-mentioned lithium iron phosphate positive electrode NiCo-Li 2 The NiCo-Li Se lithium supplement additive is prepared by a preparation method. 2 Se-supplemented lithium is added as a dodecahedral deformed cubic structure with a size between 0.6-1μm; NiCo-Li 2 A large amount of Li in Se lithium supplement additives 2 Se nanoparticles are encapsulated inside the carbon cubic structure, and Ni and Co are co-doped into the particle surface or the cubic surface.
[0015] NiCo-Li 2 Se compared to the existing Li 2 The advantage of the S lithium supplementation additive strategy is that it has higher conductivity and can provide efficient current conduction. 2 The advantage of Se lithium supplementation strategy is that NiCo ions on the porous framework derived from MOFs can form highly uniformly dispersed NiCoSe with Se. 2 The intermediate product finally obtains the equally evenly dispersed Li 2 Se nanoparticles accelerate the reaction kinetics and enable it to exist stably in air at room temperature. (three) A NiCo-Li 2 Application of Se lithium iron phosphate positive electrode lithium supplement additive in lithium iron phosphate battery.
[0017] Furthermore, the application method comprises the following steps: S1, NiCo-Li 2 Se-supplemented lithium iron phosphate (LiFePO 4 ) powder is used as the positive electrode active material, the conductive carbon black (Super P) and the binder polyvinylidene fluoride (PVDF) are mixed evenly, and N-methylpyrrolidone (NMP) solvent is added dropwise to prepare an electrode slurry. The mixed slurry is coated on the surface of the aluminum foil current collector, and after being fully dried in a vacuum drying oven, a composite positive electrode sheet is made by a sheet cutting machine; S2, with the composite cathode as the working electrode, metallic lithium as the counter electrode and reference electrode, Celgard 2500 membrane as the diaphragm, and lithium hexafluorophosphate as the electrolyte (lithium hexafluorophosphate LiPF 6 As solute, ethylene carbonate EC, dimethyl carbonate DMC, and ethyl methyl carbonate EMC as solvents), and button-type lithium iron phosphate batteries were assembled in a glove box filled with argon.
[0018] Furthermore, NiCo-Li 2The mass ratio of Se lithium supplement additive, lithium iron phosphate powder, conductive carbon black and polyvinylidene fluoride is 5~20:60~75:10:10.
[0019] The beneficial effects of the present invention are: (1) NiCo-Li of the present invention 2 Se lithium supplement additives main body Li 2 Se and Li 2 S has similar properties, but Li 2 Se has a higher conductivity (10 -5 S•m -1 ), which can achieve more efficient current conduction. Li 2 Se nanoparticles are uniformly dispersed in the NiCo-ZIF-derived cubic framework. On the one hand, the uniform dispersion at the nanoscale can accelerate the Li 2 Se in carbonate-based electrolytes; on the other hand, the comprehensive coverage of the carbon skeleton can improve the Li 2 Stability of Se in air at room temperature.
[0020] (2) NiCo-Li in the present invention 2 Se lithium supplement additive is NiCoSe 2 It is prepared by chemical conversion reaction with metal Li. On the one hand, the introduction of transition metal elements Ni / Co makes the intermediate product NiCoSe 2 On the other hand, transition metal Ni / Co is very effective for Li 2 The reaction of Se additive releasing lithium ions has a certain catalytic effect.
[0021] (3) NiCo-Li of the present invention 2 The first charge / discharge capacity of the lithium iron phosphate composite cathode modified with Se lithium supplementation additive is as high as 204.75 / 169.24 mA•h•g -1 , much higher than the original lithium iron phosphate cathode of 171.63 / 158.90 mA•h•g -1 , effectively compensating for the lithium source loss caused by the formation of the SCI film. After 140 cycles at 1C current density, the specific capacity can still be maintained above 90%, and the coulombic efficiency of the 140th cycle reaches 98.2%, which is higher than that of the original LiFePO 4 The positive electrode has increased by 1.7%. After charging and discharging at a low rate of 1C, it can still maintain 152 mA•h•g -1 The high reversible specific capacity of the original LiFePO 4 The specific capacity is only 139 mA•h•g -1 Therefore, NiCo-Li 2The lithium iron phosphate composite positive electrode modified with Se lithium supplement additive has the advantages of high capacity, high energy density, long life, low cost and environmental friendliness, and is expected to be used in the large-scale photovoltaic energy storage industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The NiCo-ZIF precursor and NiCo-Li prepared in Example 1 of the present invention 2 X-ray diffraction pattern of Se lithium supplement additive; Figure 2 NiCo-Li prepared in Example 1 of the present invention 2 Scanning electron microscope photo of Se lithium supplement additive; Figure 3 The first cycle characteristic voltage curve of the lithium iron phosphate battery prepared in Example 1 of the present invention; Figure 4 The first cycle characteristic voltage curve of the lithium iron phosphate battery prepared in Example 1-3 of the present invention; Figure 5 It is a cycle performance diagram of the lithium iron phosphate battery prepared in Example 1 of the present invention and the original lithium iron phosphate electrode prepared in Comparative Example 1 for the first 140 cycles; Figure 6 The dQ / dV curve of the first 5 cycles of the lithium iron phosphate battery prepared in Example 1 of the present invention; Figure 7 Constant current charge and discharge curves at different rates for the lithium iron phosphate battery prepared in Example 1 of the present invention and the original lithium iron phosphate electrode prepared in Comparative Example 1; Figure 8 The cycle performance diagram of the lithium iron phosphate batteries prepared in Examples 1, 4, and 5 for the first 300 cycles. DETAILED DESCRIPTION
[0023] The present invention is further described in detail below in conjunction with specific implementation modes.
[0024] Embodiment 1, A lithium iron phosphate positive electrode NiCo-Li 2 The preparation method of the Se lithium supplement additive comprises the following steps: A. Co(NO 3 ) 2 •6H 2 O (4 mmol) and Ni(NO 3 ) 2 •6H 2 O (4 mmol) was dissolved in 200 mL of methanol, labeled as solution a; 40 mmol of 2-methylimidazole (C 4 H 6 N 2) was dissolved in 200 mL of methanol and marked as solution b; solution a was slowly poured into solution b, magnetically stirred at 300 rpm / min for 30 min, and allowed to stand at room temperature for 20 h, then washed with methanol and centrifuged 5 times. The resulting precipitate was vacuum dried at 80 °C overnight to obtain a purple NiCo-ZIF precursor powder; B. NiCo-ZIF powder and Se powder were mixed at a mass ratio of 1:2 and fully ground for more than half an hour. The mixture was placed in a high-temperature tube furnace under an argon atmosphere and annealed at 800°C for 4 hours at a heating rate of 5°C / min. The mixture was successfully converted into transition metal selenide NiCoSe 2 , annealed and then cooled to room temperature; C. In a glove box filled with argon (water and oxygen contents were both less than 0.1 ppm), a lithium foil (2.32 mmol) was placed in a stainless steel crucible on a heated magnetic stirrer. When the lithium foil was completely melted and in liquid form, NiCoSe 2 (0.64 mmol) powder was added to a stainless steel crucible, and the temperature was raised to 150 °C while stirring continuously for at least 30 min, then the temperature was raised to 180 °C and reacted for 2 h under continuous stirring, and then naturally cooled to room temperature to obtain NiCo-Li 2 Se lithium supplement additive.
[0025] Figure 1 The NiCo-ZIF precursor and NiCo-Li prepared in Example 1 of the present invention 2 X-ray diffraction (XRD) pattern of Se lithium supplement additive. It can be seen from the spectrum that both conform to the hexagonal NiCoSe 2 The characteristic peaks of NiCo-Li 2 Se shows a lithiated peak at around 26°.
[0026] Figure 2 NiCo-Li prepared in Example 1 of the present invention 2 Scanning electron microscope (SEM) photo of Se lithium supplement additive. It can be seen from the photo that it has a dodecahedral deformed cube structure with a size between 0.6-1μm and a large number of nanoparticles embedded inside.
[0027] The NiCo-Li prepared in Example 1 2 Se lithium supplement additive and lithium iron phosphate are combined as positive electrode active materials to assemble lithium-ion batteries. The specific steps are as follows: S1, NiCo-Li 2 Se-supplemented lithium iron phosphate (LiFePO 4) powder (purchased from MTI) as the positive electrode active material, conductive carbon black (Super P) as the conductive agent, polyvinylidene fluoride (PVDF) as the binder, N-methylpyrrolidone (NMP) as the solvent, NiCo-Li 2 Se lithium supplement additive, LiFePO 4 Powder, Super P and PVDF were uniformly mixed in a mass ratio of 10:70:10:10 (i.e. NiCo-Li 2 Se addition amount is 10%), N-methylpyridine alkanone solvent is added dropwise to prepare electrode slurry; aluminum foil is used as current collector, the mixed slurry is coated on its surface, and after drying at 120 ° C in a vacuum drying oven for 24 h, NiCo-Li with a diameter of 13 mm is cut by a sheet cutting machine. 2 Se-LiFePO 4 Composite positive electrode sheet; S2. Using the composite positive electrode as the working electrode, metallic lithium as the counter electrode and reference electrode, Celgard 2500 membrane as the separator, and lithium hexafluorophosphate (volume % of ethyl carbonate EC, dimethyl carbonate DMC, and ethyl methyl carbonate EMC in a volume ratio of 1:1:1) as the electrolyte, a button-type lithium iron phosphate battery was assembled in a glove box filled with argon gas with water and oxygen contents both below 0.01 ppm.
[0028] Comparative Example 1 Preparation of original lithium iron phosphate electrode: LiFePO 4 The powder, Super P and PVDF were mixed in an N-methylpyrrolidone solvent at a mass ratio of 80:10:10, and the coating-drying-cutting-assembly process was the same as that in Example 1.
[0029] The lithium iron phosphate battery prepared in Example 1 and the original lithium iron phosphate electrode prepared in Comparative Example 1 were tested for charge and discharge cycle stability and charge and discharge performance at different rates. The specific process is as follows: (1) Test of charge and discharge cycle stability: The electrochemical performance of the lithium iron phosphate battery prepared in Example 1 and the original lithium iron phosphate electrode prepared in Comparative Example 1 were tested using the Xinwei battery testing system. The charge cut-off voltage and discharge cut-off voltage were set to 4.0V and 2.0V, respectively. According to the theoretical specific capacity of lithium iron phosphate (170 mA•h•g -1 ) and the corresponding positive electrode active material mass, the current density is 1C, after 140 cycles, the specific capacity of the lithium iron phosphate battery prepared in Example 1 can still maintain 92.3%, and its cycle performance curve is shown in Figure 5 .
[0030] Figure 5It is a cycle performance diagram (cycle characteristic voltage curve and coulombic efficiency) of the lithium iron phosphate battery prepared in Example 1 of the present invention and the original lithium iron phosphate electrode prepared in Comparative Example 1 for the first 140 cycles. It can be seen from the figure that under the conditions of 1C, 2.0-4.0V, after 140 cycles, the specific capacity of the lithium iron phosphate battery prepared in Example 1 can still maintain 92.3% of its initial capacity, and the coulombic efficiency of the 140th cycle reaches 98.2%, which is 1.7% higher than that of the original lithium iron phosphate electrode prepared in Comparative Example 1.
[0031] (2) Test of charge and discharge performance at different rates: The electrochemical performance of the lithium iron phosphate battery prepared in Example 1 and the original lithium iron phosphate electrode prepared in Comparative Example 1 were tested using the Xinwei battery testing system. The charge cut-off voltage and discharge cut-off voltage were set to 4.0 V and 2.0 V, respectively. According to the theoretical specific capacity of lithium iron phosphate (170 mA•h•g -1 ) and the corresponding positive electrode active material mass, and the electrochemical performance tests were carried out at current densities of 0.05C, 0.2C, 0.5C and 1C respectively.
[0032] Figure 6 The dQ / dV curve of the first 5 cycles of the lithium iron phosphate battery prepared in Example 1 of the present invention shows that a peak at about 3.0 V is observed, which can be attributed to Li 2 The oxidation peak of Se delithiation process is observed, while no relevant lithiation peak is observed in the discharge cut-off voltage range (2.0 V), indicating that NiCo-Li 2 The electrochemical reaction of Se within the working voltage range is completely irreversible.
[0033] Figure 7 The constant current charge-discharge curves of the lithium iron phosphate battery prepared in Example 1 of the present invention and the original lithium iron phosphate electrode prepared in Comparative Example 1 at different rates. It can be seen from the figure that the lithium iron phosphate battery prepared in Example 1 can still maintain 152 mA•h•g after high rate current 1C charge and discharge. -1 The high reversible specific capacity of the original lithium iron phosphate electrode prepared in comparative example 1 is only 139 mA•h•g -1 , which shows that the composite negative electrode has good structural stability and rate performance.
[0034] Embodiment 2, The difference between this embodiment and embodiment 1 is that when assembling lithium-ion batteries, NiCo-Li 2 Se lithium supplement additive, LiFePO 4 Powder, Super P and PVDF were uniformly mixed in a mass ratio of 5:75:10:10 (i.e. NiCo-Li 2The addition amount of Se is 5%), and the quality of lithium iron phosphate powder remains unchanged.
[0035] Embodiment 3, When assembling lithium-ion batteries, NiCo-Li 2 Se lithium supplement additive, LiFePO 4 Powder, Super P and PVDF were uniformly mixed in a mass ratio of 20:60:10:10 (i.e. NiCo-Li 2 The addition amount of Se is 20%), and the quality of lithium iron phosphate powder remains unchanged.
[0036] The following electrochemical performance tests were performed on the lithium iron phosphate batteries prepared in Examples 1-3. The specific test steps are as follows: The electrochemical performance of the lithium iron phosphate batteries prepared in Examples 1-3 was tested using the Xinwei battery testing system. The charge cut-off voltage and discharge cut-off voltage were set to 4.0 V and 2.0 V, respectively. According to the theoretical specific capacity of lithium iron phosphate (170 mA•h•g -1 ) and the corresponding positive electrode active material mass, the charge and discharge performance at a current density of 0.1C was tested. The experimental results are shown in Figure 3 , Figure 4 And as shown in Table 1.
[0037] It can be seen from Table 1 that the 10% NiCo-Li prepared in Example 1 2 The performance of lithium iron phosphate battery with Se addition is better than that of other embodiments. 2 The amount of Se added is the optimal ratio.
[0038] from Figure 3 and Figure 4 It can be seen that the first cycle charge capacity of the material prepared in Example 1 can reach 204.75 mA•h•g at 0.1C and 2.0-4.0V voltage. -1 , the introduced NiCo-Li 2 Se lithium supplementation additives provide additional active lithium and contribute approximately 30 mA•h•g -1 When discharged to 2.0V, the discharge capacity can reach 169.24 mA•h•g -1 The capacity is higher than that of most other lithium-supplementing additive-modified LiFePO 4 Battery.
[0039] Embodiment 4, The difference between this embodiment and embodiment 1 is that the mass ratio of NiCo-ZIF precursor powder to Se powder in step B is changed to 1:1.
[0040] Embodiment 5, The difference between this embodiment and embodiment 1 is that the mass ratio of NiCo-ZIF precursor powder to Se powder in step B is changed to 2:1.
[0041] The following electrochemical performance tests were performed on the lithium iron phosphate batteries prepared in Examples 1, 4 and 5. The specific test steps are as follows: The electrochemical performance of the lithium iron phosphate batteries prepared in Examples 1, 4 and 5 was tested using the Xinwei battery testing system. The charge cut-off voltage and discharge cut-off voltage were set to 4.0 V and 2.0 V, respectively. 4 Theoretical specific capacity (170 mA•h•g -1 ) and the corresponding positive electrode active material mass, the charge and discharge performance under the test current density of 1C is tested. The experimental results are as follows Figure 8 And as shown in Table 2.
[0042] As can be seen from Table 2, the performance of the lithium iron phosphate battery prepared in Example 1 with a mass ratio of NiCo-ZIF precursor powder to Se powder of 1:2 is better than that of other examples, and the mass ratio of NiCo-ZIF precursor powder to Se powder of 1:2 is the optimal ratio.
[0043] Figure 8 The cycle performance diagram (cycle characteristic voltage curve and coulombic efficiency) of the lithium iron phosphate battery prepared in Examples 1, 4 and 5 before 300 cycles is shown in FIG. Figure 8 It can be seen that the first cycle charge and discharge specific capacity of the material prepared in Example 1 under 1C and 2.0-4.0V voltage conditions can reach 166.20 mA h g -1 and 153.83 mA hg -1 The corresponding first coulombic efficiency can reach 92.56%, which is higher than that of LiFePO modified with lithium supplement additives obtained when the mass ratio of NiCo-ZIF to Se powder is 1: 1 and 2: 1. 4 Battery.
[0044] Embodiment 6, The difference between this embodiment and embodiment 1 is that the lithium foil and NiCoSe in step C are changed. 2 The molar mass ratio of the powders is 1.16:0.64.
[0045] Embodiment 7, The difference between this embodiment and embodiment 1 is that the lithium foil and NiCoSe in step C are changed. 2 The molar mass ratio of the powders is 4.64:0.64.
[0046] The NiCo-Li prepared in Examples 1, 6 and 7 2 Se lithium supplementation additives were used for macroscopic evaluation. In Example 6, the metal lithium foil melted rapidly and was replaced by NiCoSe 2 The powder was covered and no lithium metal molten balls appeared even after continued stirring; however, in Example 7, part of the metal lithium foil was melted and mixed with NiCoSe 2 The powder forms a hard granular solid, and further heating and stirring cannot transform it into NiCo-Li 2 Se powder. Therefore, in Example 1, the metal lithium foil and NiCoSe 2 The molar ratio of the powder is 2.43:0.64, which is the best ratio.
[0047] Embodiment 8, The difference between this embodiment and embodiment 1 is that in step A, the amount of methanol used in solution a is 600 mL, and the amount of methanol used in solution b is 100 mL.
[0048] Embodiment 9, The difference between this embodiment and embodiment 1 is that in step A, the vacuum drying temperature is 60°C.
[0049] Embodiment 10 The difference between this embodiment and embodiment 1 is that in step B, the annealing conditions are: heating to 600° C. at a heating rate of 10° C. / min and annealing at the temperature for 5 hours.
[0050] In summary, compared with the current research on binary compound lithium supplement additives based on conversion reactions, the lithium iron phosphate positive electrode NiCo-Li 2 Se lithium supplement additives have high specific capacity, suitable voltage window, good compatibility with electrolyte, rapid reaction kinetics, and good air stability. They play an important role in improving the performance of lithium iron phosphate batteries and are expected to be used in the large-scale photovoltaic energy storage industry.
Claims
1. A method for preparing a lithium iron phosphate positive electrode NiCo-Li2Se lithium supplement additive, characterized in that The following steps are involved: A. Dissolve Co(NO3)2•6H2O and Ni(NO3)2•6H2O in methanol, dissolve 2-methylimidazole in methanol, mix the two methanol solutions evenly, let stand, wash with methanol and dry to obtain NiCo-ZIF precursor powder; B. Mixing NiCo-ZIF precursor powder and Se powder, grinding them thoroughly and then annealing them, and cooling them to room temperature after annealing to obtain NiCoSe2; C. In a glove box filled with argon, the molten lithium foil and NiCoSe2 powder are mixed evenly at a temperature of 150-180°C, and stirred continuously for sufficient reaction. After naturally cooling to room temperature, the NiCo-Li2Se lithium supplement additive is obtained.
2. The method for preparing a lithium iron phosphate positive electrode NiCo-Li2Se lithium supplement additive according to claim 1, characterized in that: In step A, the molar ratio of Co to Ni is 1:1, the ratio of methanol to the total amount of Co(NO3)2•6H2O and Ni(NO3)2•6H2O is 100~300ml:4mmol, and the ratio of methanol to the total amount of 2-methylimidazole is 100~200ml: 40mmol.
3. The method for preparing a lithium iron phosphate positive electrode NiCo-Li2Se lithium supplement additive according to claim 1, characterized in that: In step A, vacuum drying is used for drying at a temperature of 60-80°C.
4. The method for preparing a lithium iron phosphate positive electrode NiCo-Li2Se lithium supplement additive according to claim 1, characterized in that: In step B, the mass ratio of NiCo-ZIF precursor powder to Se powder is 1:0.5-2.
5. The method for preparing a lithium iron phosphate positive electrode NiCo-Li2Se lithium supplement additive according to claim 1, characterized in that: In step B, the annealing conditions are: heating to 600-800° C. at a heating rate of 5-10° C. / min, and annealing at this temperature for 4-5 hours.
6. The method for preparing a lithium iron phosphate positive electrode NiCo-Li2Se lithium supplement additive according to claim 1, characterized in that: In step C, the molar ratio of lithium foil to NiCoSe2 is 1.80-7.25:
1.
7. A lithium iron phosphate positive electrode NiCo-Li2Se lithium supplement additive, characterized in that: The invention is prepared by the preparation method of a NiCo-Li2Se lithium supplement additive for lithium iron phosphate positive electrode according to any one of claims 1 to 6.
8. Use of the NiCo-Li2Se lithium iron phosphate positive electrode lithium supplement additive according to claim 7 in a lithium iron phosphate battery.
9. The use of a lithium iron phosphate positive electrode NiCo-Li2Se lithium supplement additive in a lithium iron phosphate battery according to claim 8, characterized in that The following steps are involved: S1. Using lithium iron phosphate powder with NiCo-Li2Se lithium supplement additive as positive electrode active material, conductive carbon black as conductive agent and polyvinylidene fluoride as binder are mixed evenly, adding N-methylpyrrolidone solvent to prepare electrode slurry, coating the mixed slurry on the surface of aluminum foil current collector, and preparing composite positive electrode sheet after fully drying; S2. A button-type lithium iron phosphate battery was assembled in a glove box filled with argon using a composite positive electrode as the working electrode, metallic lithium as the counter electrode and reference electrode, a Celgard 2500 membrane as the diaphragm, and lithium hexafluorophosphate as the electrolyte.
10. The use of a lithium iron phosphate positive electrode NiCo-Li2Se lithium supplement additive in a lithium iron phosphate battery according to claim 9, characterized in that: The mass ratio of NiCo-Li2Se lithium supplement additive, lithium iron phosphate powder, conductive carbon black and polyvinylidene fluoride is 5~20:60~75:10:10.