Method for manufacturing lithium ion battery
By adopting the two injection method in the manufacture of lithium-ion batteries, the low viscosity rapid penetration of organic solvents and the diffusion of electrolytes are used to solve the problem of poor electrolyte infiltration, improving battery performance and cycle stability, saving Energy costs and improve the flexibility of electrolyte formulations.
Patent Information
- Application Number
- CN202411488939.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the injection process of lithium-ion batteries, there is a problem that the electrolyte has poor wetting effect on the electrode sheet, which leads to limited battery performance, especially in cylindrical batteries and square winding batteries.
The method of two injections is adopted. The first injection is injected with only organic solvents, and the second injection is injected into the remaining part of the electrolyte. It uses the low viscosity of the organic solvent to penetrate into the pores of the poles quickly and passes through the principle of molecular diffusion. Improve the permeability efficiency of the electrolyte and avoid high pressure and high temperature standing.
It achieves good infiltration of the electrolyte, improves the charging and discharging performance and cycle stability of the battery, saves energy costs, and reduces the requirements of the electrolyte formulation, and has better universality.
Smart Images

Figure CN119009403A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular, to a method for manufacturing a lithium-ion battery. Background Art
[0002] Lithium-ion batteries are the most mature lithium-series secondary batteries currently, and are widely used in 3C digital, electric vehicles, energy storage and other fields. The increase in battery energy density has resulted in an increase in electrode surface density and an increase in pole piece compaction density, leading to difficulties in battery injection and wetting, which is more serious in cylindrical batteries and square wound batteries. The existing injection method has the problem of poor electrolyte wetting of the pole piece, which limits the performance of the battery.
[0003] In view of this, this application is hereby filed. Summary of the invention
[0004] The purpose of the present application is to provide a method for manufacturing a lithium-ion battery, wherein the electrolyte can well infiltrate the pole piece, thereby improving the battery performance.
[0005] This application is implemented as follows: The present application provides a method for manufacturing a lithium-ion battery, wherein the lithium-ion battery comprises a battery housing, and a pole piece and an electrolyte disposed in the battery housing, wherein the electrolyte comprises an organic solvent and an electrolyte salt dispersed in the organic solvent, and the method for manufacturing the lithium-ion battery comprises sequentially performing a liquid injection step and a formation step, wherein the liquid injection step comprises: Primary injection: injecting only a portion of the organic solvent used to constitute the electrolyte into the battery housing, and the organic solvent injected in the primary injection accounts for more than 50% of the total mass of the electrolyte; Secondary injection: injecting the remaining part of the electrolyte into the battery housing, wherein the remaining part of the electrolyte is the rest of the electrolyte except the organic solvent injected in the primary injection.
[0006] In an optional embodiment, the viscosity of the organic solvent injected in the first injection is lower than 0.7 mPa·s, and the viscosity of the remaining part of the electrolyte injected in the second injection is higher than the viscosity of the organic solvent injected in the first injection and lower than 2.0 mPa·s.
[0007] In an optional embodiment, the organic solvent includes a linear carbonate solvent.
[0008] In an optional embodiment, the linear carbonate solvent is selected from one or more of ethyl methyl carbonate, dimethyl carbonate and diethyl carbonate.
[0009] In an optional embodiment, the organic solvents injected in the first injection are all chain carbonate solvents.
[0010] In an optional embodiment, a portion of the organic solvent is a linear carbonate solvent, and all the linear carbonate solvent in the electrolyte is injected through the single injection.
[0011] In an optional embodiment, the linear carbonate solvent accounts for less than 70% of the total mass of the electrolyte.
[0012] In an optional embodiment, the injection pressure of the primary injection and the secondary injection is no more than 0.3 MPa.
[0013] In an optional embodiment, the liquid injection step further includes standing at room temperature for a first preset time between the first liquid injection and the second liquid injection; The method for manufacturing a lithium-ion battery further includes: between the injection step and the formation step, standing at room temperature for a second preset time.
[0014] This application has the following beneficial effects: The manufacturing method of the lithium-ion battery provided in the embodiment of the present application includes sequentially performing the injection step and the formation step. The injection step includes a primary injection and a secondary injection. The primary injection includes injecting only a part of the organic solvent used to form the electrolyte into the battery housing; the secondary injection includes injecting the remaining part of the electrolyte used to form the electrolyte into the battery housing, wherein the remaining part of the electrolyte is the remaining part of the electrolyte except the organic solvent injected in the primary injection. The primary injection only injects part of the organic solvent and does not contain electrolyte salt, so the viscosity is relatively low, and it can be injected into the battery housing at low pressure, and the injection difficulty is relatively low. And after the primary injection, the organic solvent has a low viscosity, so it can quickly penetrate into the pores of the pole piece to achieve good infiltration. The secondary injection injects the remaining part of the electrolyte into the battery housing. Using the diffusion principle of molecules, the relatively high concentration of the injected substance can quickly diffuse along the organic solvent injected in the primary injection, and the penetration efficiency in the pole piece is significantly improved compared to the electrolyte of the complete component. After the secondary injection, the subsequent formation can be carried out after the diffusion is uniform. The manufacturing method of the embodiment of the present application has high electrolyte infiltration efficiency and good infiltration effect, and does not require high-pressure injection and high-temperature standing, thereby saving energy costs and avoiding the decomposition of low-temperature additives in the electrolyte at high temperatures to ensure battery performance. In addition, the embodiment of the present application has low requirements for the electrolyte formula and has good universality. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0016] Figure 1 The present invention is a flowchart of a method for manufacturing a lithium-ion battery in one embodiment of the present invention. DETAILED DESCRIPTION
[0017] Electrolyte Filling of lithium-ion batteries is a key step in the battery manufacturing process, which directly affects the performance, safety and life of lithium-ion batteries. Multiple parameters need to be strictly controlled during the filling process to ensure the uniform distribution of the electrolyte and the high quality of the battery. Among them, the electrolyte is required to be able to well infiltrate the pole piece after the filling step, in order to ensure that the electrolyte can fully penetrate into the electrode material, form a uniform electrolyte environment, and promote the effective transmission of lithium ions, thereby improving the battery's charge and discharge performance and cycle stability. In some related technologies, the electrolyte is first configured and then injected into the battery housing at one time. When injecting the electrolyte in this way, the viscosity of the electrolyte is often large, and there may be problems such as poor pole piece wetting effect, uneven electrolyte distribution, and dead zones in the battery, which may negatively affect the battery performance. And because the viscosity of the electrolyte is high, it may rely on high-cost injection methods such as high-pressure injection. In other related technologies, the step-by-step injection method is used. Although the wetting effect is improved to a certain extent, the electrolyte used in the first injection of the existing step-by-step injection method is obtained by mixing lithium salts and solvents in a strict ratio, which has high requirements on the formulation of the electrolyte and limits the selection and application of the electrolyte. Because batteries with different surface densities, different compaction densities, different positive electrode material systems, different rate requirements, and different shapes have different requirements for electrolytes. Therefore, the existing step-by-step injection method does not have good universality.
[0018] To this end, an embodiment of the present application provides a method for manufacturing a lithium-ion battery, in which the electrolyte is injected through a primary injection and a secondary injection, and only a portion of the organic solvent is injected in the primary injection. The electrode is first wetted by utilizing the low viscosity and good wetting effect of the organic solvent, and the remaining portion of the electrolyte is injected in the subsequent secondary injection. The remaining portion of the electrolyte can diffuse well in the organic solvent of the primary injection and wet the electrode.
[0019] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0020] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0021] In an embodiment of the present application, the lithium-ion battery to be manufactured in the present application includes a battery housing, and a pole piece and an electrolyte disposed in the battery housing. Among them, the electrolyte includes an organic solvent and an electrolyte salt. In addition, the electrolyte may also include additives, and the additives and the electrolyte salt are dispersed in the organic solvent. In an embodiment of the present application, the lithium-ion battery may be a soft-pack, cylindrical, or square lithium-ion battery. The type of organic solvent may include carbonate organic solvents and / or carboxylate organic solvents. Among them, the carbonate organic solvent may be one or more of a chain carbonate solvent and a cyclic carbonate solvent; the carboxylate organic solvent may be one or more of ethyl acetate (EA) and ethyl propionate (EP).
[0022] The chain carbonate solvent can be selected from one or more of ethyl methyl carbonate (EMC), dimethyl carbonate (DMC) and diethyl carbonate (DEC). Chain carbonate solvents have good electrochemical stability and dissolving ability, can effectively promote the transmission of lithium ions, and improve the performance of batteries.
[0023] The cyclic carbonate solvent may be selected from one or more of ethylene carbonate (EC) and propylene carbonate (PC).
[0024] The following table shows the physical and chemical parameters of several organic solvents.
[0025]
[0026] EC and PC have high dielectric constants, so lithium salts have high solubility in these two solvents, thus having high conductivity. PC has a very low melting point and a very high boiling point. Compared with PC, EC is less likely to have the problem of co-embedded graphite causing peeling. However, the high melting point of EC means that it is solid or has poor fluidity at low temperatures, which greatly affects the low-temperature use of the electrolyte, so it can be used in conjunction with low-melting-point solvents, such as PC and EMC. Chain carbonate solvents (such as EMC, DMC, and DEC) generally have the characteristics of low viscosity and low melting point, and are easy to infiltrate the electrode; when in use, they can be mixed with high-viscosity, high-melting-point cyclic carbonate solvents for better performance. Among chain carbonate solvents, DMC has a higher melting point than DEC and EMC, but its viscosity is the lowest, and its toxicity is also low. EA and EP are carboxylic acid ester organic solvents. EA can absorb water, which makes EA decompose into acidic, while EP is irritating and highly toxic, and its vapor can form an explosive mixture with air. In addition, EA and EP have slightly lower boiling points, and their melting points are close to those of linear carbonates. Therefore, the organic solvent of the embodiment of the present application can be selected from a mixed solvent containing a linear carbonate solvent and a cyclic carbonate solvent.
[0027] Optionally, the electrolyte salt in the electrolyte may be one or more of lithium hexafluorophosphate LiPF6, lithium tetrafluoroborate LiBF4, lithium bistrifluoromethanesulfonyl imide LiTFSI, lithium bisfluorosulfonyl imide LiFSI, and lithium perchlorate LiClO4.
[0028] Furthermore, the additives in the electrolyte can be selected from one or more of 1,3-propane sultone (PS), vinylene carbonate (VC), and lithium bis(oxalatoborate) (LiBOB). PS can form a stable SEI film (solid electrolyte interface film) on the surface of the negative electrode, reduce side reactions, and improve the cycle stability and safety of the battery; it can also inhibit the growth of lithium dendrites, reduce the risk of short circuits inside the battery, and improve the safety of the battery; PS can also improve the performance of the battery under low temperature conditions and improve the low-temperature charge and discharge efficiency of the battery. VC can form an SEI film, inhibit the growth of lithium dendrites, and improve the thermal stability of the electrolyte. LiBOB can form an SEI film, inhibit the growth of lithium dendrites, improve the low-temperature performance of the battery, and improve the thermal stability of the electrolyte.
[0029] Optionally, in an embodiment of the present application, the chain carbonate solvent in the electrolyte accounts for less than 70% of the total mass of the electrolyte; further, the chain carbonate solvent accounts for 50% to 70% of the total mass of the electrolyte.
[0030] Figure 1 Flow chart of a method for manufacturing a lithium-ion battery in one embodiment of the present application. Figure 1As shown, the manufacturing method of the lithium ion battery provided in the embodiment of the present application includes a liquid injection step and a formation step. It should be understood that other process steps may be included before the liquid injection step and after the formation step, such as pole piece production, battery housing production, etc. These steps can refer to the prior art and will not be described one by one in this application. The liquid injection step and the formation step in the embodiment of the present application are specifically introduced below.
[0031] Step S100, liquid injection step.
[0032] In the embodiment of the present application, the liquid injection step S100 specifically includes the following steps: Step S110, one injection.
[0033] In this embodiment, the primary injection includes injecting only a portion of the organic solvent used to constitute the electrolyte into the battery housing. Optionally, the viscosity of the organic solvent injected in the primary injection is lower than 0.7 mPa·s.
[0034] Optionally, the electrolyte includes a linear carbonate solvent, and the organic solvents injected during the one-time injection process are all linear carbonate solvents. As can be seen from the above introduction, the linear carbonate solvent has a low melting point and has a low viscosity at room temperature, so the one-time injection can be carried out at room temperature, and the injection pressure can be selected to be a lower value. Optionally, the injection pressure of the one-time injection is not greater than 0.3MPa, and the lower injection pressure can reduce the process cost.
[0035] Optionally, the organic solvent injected in one injection accounts for more than 50% of the total mass of the electrolyte. It should be understood that if the injection amount of one injection is too small, it may not be able to fill the pores of the electrode. Optionally, the organic solvent injected in one injection accounts for 50% to 70% of the total mass of the electrolyte.
[0036] Step S120: leaving the mixture to stand at room temperature for a first preset time period.
[0037] Optionally, the first preset time is 6 to 15 hours. During the standing period at room temperature, the organic solvent injected in the first injection can quickly penetrate into the pores of the electrode. In the case where the chain carbonate solvent is injected in the first injection, the chain carbonate solvent has a lower viscosity and wetting performance at room temperature, so the wetting effect can be ensured by standing at room temperature, which can save energy consumption and reduce process costs.
[0038] Step S130, secondary liquid injection.
[0039] In an embodiment of the present application, the secondary injection includes injecting the remaining part of the electrolyte into the battery housing, wherein the remaining part of the electrolyte is the remaining part of the electrolyte except the organic solvent injected by the primary injection. For example, the substance injected by the secondary injection may include electrolyte salts, additives, and another part of the organic solvent other than the primary injection. Optionally, the viscosity of the remaining part of the electrolyte injected by the secondary injection is higher than the viscosity of the organic solvent injected by the primary injection, and is lower than 2.0 mPa·s. Although the viscosity of the remaining part of the electrolyte of the secondary injection is higher than the viscosity of the organic solvent injected by the primary injection, before the secondary injection, the organic solvent in the battery housing has fully infiltrated the pole piece, and the high concentration of the remaining part of the electrolyte can be quickly diffused along the organic solvent injected by the primary injection, and the penetration rate is significantly improved compared to the penetration rate of the electrolyte of the complete component in the pole piece. It can be understood that the viscosity of the remaining part of the electrolyte injected by the secondary injection should not be too high. Excessive viscosity may increase the difficulty of injection, such as taking longer and requiring greater pressure.
[0040] Optionally, the injection pressure of the secondary injection is not greater than 0.3 MPa, and a lower injection pressure can reduce process costs. In the embodiment of the present application, both the primary injection and the secondary injection can be achieved using a low-pressure injection machine. Compared with high-pressure injection machines and ultra-high-pressure injection machines, low-pressure injection machines have lower equipment prices and lower operating costs, and also have a smaller site footprint.
[0041] After the secondary liquid injection is completed, the liquid injection step is completed. Optionally, after the liquid injection step S100, the method for manufacturing a lithium-ion battery may further include: Step S200: leaving the mixture at room temperature for a second preset time period.
[0042] In the embodiment of the present application, optionally, the second preset time is 2 to 10 hours. During the normal temperature standing process of step S200, the remaining part of the high-concentration electrolyte can be fully diffused to make the electrolyte uniform, thereby ensuring the battery performance. In the embodiment of the present application, the standing in step S120 and step S200 is performed at room temperature, which can not only save energy costs compared to high-temperature infiltration, but also avoid the decomposition of low-temperature additives at high temperatures.
[0043] Step S300, a formation step.
[0044] After standing at room temperature for a second preset time, the components in the electrolyte diffuse evenly, and the formation step can be carried out. The formation step can activate the electrochemical reaction inside the battery through a specific charge and discharge cycle to form a stable SEI film, thereby improving the performance and cycle stability of the battery.
[0045] The manufacturing method and beneficial effects of the present application are specifically introduced below through Examples 1 to 4 and Comparative Examples 1 to 2.
[0046] Example 1 This embodiment uses a 40135 large cylindrical wound battery (diameter 40mm, height 135mm) for injection and infiltration verification. The lithium-ion battery has a lithium iron phosphate positive electrode with a capacity of 20Ah. The designed injection volume is 70g, and the designed electrolyte formula is LiPF6 7g, EC is 19.6g, DMC is 42g, vinylene carbonate VC is 1.4g, and the viscosity is 1.00mPa·s. Obtain a semi-finished battery (including a battery shell and a pole piece) that has passed the moisture test after drying, and inject 35g of DMC solvent (viscosity 0.59mPa·s) into the battery shell at room temperature using a low-pressure injection machine. The injection time is 30s, and then it is left to stand at room temperature for 12h. Then, the remaining electrolyte (7g LiPF6, 19.6g EC, 7g DMC, 1.4g VC, viscosity 1.41 mPa·s) of the original electrolyte formula was injected into the battery shell using a low-pressure injection machine at room temperature for 60 seconds, followed by immersion at room temperature for 6 hours. After that, the formation and capacity separation were carried out, and the lithium-ion battery was subjected to a 1C charge and discharge cycle test at room temperature.
[0047] Example 2 This embodiment uses a 40135 large cylindrical wound battery (diameter 40mm, height 135mm) for injection and infiltration verification. The lithium-ion battery has a lithium iron phosphate positive electrode with a capacity of 20Ah. The designed injection volume is 70g, and the designed electrolyte formula is LiPF6 7g, EC is 19.6g, DMC is 42g, vinylene carbonate VC is 1.4g, and the viscosity is 1.00mPa·s. Obtain a semi-finished battery (including a battery shell and a pole piece) that has passed the moisture test after drying, and inject 42g of DMC solvent (viscosity 0.59mPa·s) into the battery shell at room temperature using a low-pressure injection machine. The injection time is 30s, and then it is left to stand at room temperature for 12h. After that, the remaining electrolyte (7g LiPF6, 19.6g EC, 1.4g VC, viscosity 1.615 mPa·s) of the original electrolyte formula was injected into the battery shell using a low-pressure injection machine at room temperature for 62 seconds, followed by immersion at room temperature for 6 hours. After that, the formation and capacity separation were carried out, and the lithium-ion battery was subjected to a 1C charge and discharge cycle test at room temperature.
[0048] Example 3 This embodiment uses 17119 square laminated cells (thickness 17mm, width 119, height 129mm) for injection and infiltration verification. The lithium-ion battery has a lithium manganese oxide positive electrode with a capacity of 24Ah. The designed injection volume is 100g, and the designed electrolyte formula contains 10g LiPF6, 16g EC, 35g DMC, 35g EMC, 2g vinyl carbonate VC, 1,3-propane sultone PS, 1g lithium dioxalate borate LiBOB, and a viscosity of 1.00mPa·s. Obtain a semi-finished battery (including a battery shell and a pole piece) that has passed the moisture test after drying, and inject 35g DMC+15g EMC (viscosity after mixing is 0.608mPa·s) into the battery shell at room temperature using a low-pressure injection machine. The injection time is 25s, and then it is left to stand at room temperature for 12h. After that, the remaining electrolyte of the original electrolyte formula (10g LiPF6, 16g EC, 20g EMC, 1g VC, 2g PS, 1g LiBOB, viscosity 1.392 mPa·s) was injected into the battery shell using a low-pressure injection machine at room temperature for 55 seconds, followed by immersion at room temperature for 6 hours. After that, the formation and capacity separation were carried out, and the lithium-ion battery was subjected to a 1C charge and discharge cycle test at room temperature.
[0049] Example 4 This embodiment uses 17119 square laminated cells (thickness 17mm, width 119, height 129mm) for injection and infiltration verification. The lithium-ion battery has a lithium manganese oxide positive electrode with a capacity of 24Ah. The designed injection volume is 100g, and the designed electrolyte formula contains 10g LiPF6, 16g EC, 35g DMC, 35g EMC, 2g vinyl carbonate VC, 1,3-propane sultone PS, 1g lithium dioxalate borate LiBOB, and a viscosity of 1.00mPa·s. Obtain a semi-finished battery (including a battery shell and a pole piece) that has passed the moisture test after drying, and inject 35g DMC+30g EMC (viscosity after mixing is 0.608mPa·s) into the battery shell at room temperature using a low-pressure injection machine. The injection time is 26s, and then it is left to stand at room temperature for 12h. After that, the remaining electrolyte (10g LiPF6, 16g EC, 5g EMC, 1g VC, 2g PS, 1g LiBOB, viscosity 1.382 mPa·s) of the original electrolyte formula was injected into the battery shell using a low-pressure injection machine at room temperature. The injection time was 55s, followed by 6h of room temperature immersion. After that, the formation and capacity separation were carried out, and the lithium-ion battery was subjected to room temperature 1C charge and discharge cycle test.
[0050] Comparative Example 1 A 40135 large cylindrical wound battery (40 mm in diameter and 135 mm in height) was used for injection and infiltration verification. The lithium-ion battery has a lithium iron phosphate positive electrode with a capacity of 20 Ah. The designed injection volume is 70 g, and the designed electrolyte formula is 7 g of LiPF6, 19.6 g of EC, 42 g of DMC, 1.4 g of vinyl carbonate VC, and a viscosity of 1.00 mPa·s. Obtain a semi-finished battery (including a battery shell and a pole piece) with qualified moisture after drying. The above parameter design is the same as that of Examples 1 and 2. 35 g of electrolyte S1 is injected for the first time, and the first injection time is 115 s. After the first injection, formation is carried out, and after the formation, a second injection is carried out. 35 g of electrolyte S2 is injected for the second time, and the second injection time is 40 s. The electrolyte S1 is made of LiPF6 (0.9 mol / L) and additive VC (1.5%) dissolved in a mixed solvent of EC / DMC=2:8 (volume ratio) (viscosity 0.89 mPa·s). The electrolyte S2 is made of LiPF6 (1.1 mol / L) and additive VC (1.5%) dissolved in a mixed solvent of EC / DMC=5:5 (volume ratio) (viscosity 1.25 mPa·s). The formed lithium-ion battery is divided into different capacities, and then the battery is subjected to a 1C charge and discharge cycle test at room temperature.
[0051] Comparative Example 2 A 40135 large cylindrical wound battery (40 mm in diameter and 135 mm in height) was used for injection and infiltration verification. The lithium-ion battery has a lithium iron phosphate positive electrode with a capacity of 20 Ah. The designed injection volume is 70 g, and the designed electrolyte formula is 7 g of LiPF6, 19.6 g of EC, 42 g of DMC, 1.4 g of vinyl carbonate VC, and a viscosity of 1.00 mPa·s. Obtain a semi-finished battery (including a battery shell and a pole piece) with qualified moisture after drying. The above parameter design is the same as that of Examples 1 and 2. 42 g of electrolyte S1 was injected for the first time, and the first injection time was 117 s. After the first injection, formation was carried out, and after the formation, a second injection was carried out. 28 g of electrolyte S2 was injected for the second injection, and the second injection time was 40 s. The electrolyte S1 is made of LiPF6 (0.9 mol / L) and additive VC (1.5%) dissolved in a mixed solvent of EC / DMC=2:8 (volume ratio) (viscosity 0.89 mPa·s). The electrolyte S2 is made of LiPF6 (1.1 mol / L) and additive VC (1.5%) dissolved in a mixed solvent of EC / DMC=5:5 (volume ratio) (viscosity 1.25 mPa·s). The formed lithium-ion battery is divided into different capacities, and then the battery is subjected to a 1C charge and discharge cycle test at room temperature.
[0052] The following table compares the injection time and battery performance of Examples 1 to 4 and Comparative Examples 1 to 2.
[0053]
[0054] It can be seen that in Examples 1 and 2, since only DMC is injected into the first injection before formation, the first injection time is very short, only 30s. The secondary injection before formation utilizes the diffusion and mutual dissolution of two electrolytes. Whether it is injection or later infiltration, the time is relatively short, and the secondary injection time is 60s and 62s. The infiltration time of the 40135 large cylinder in the industry is 24h at high temperature (45°C), while the embodiment of the present application only takes 18h, and high temperature conditions are not required, so the energy consumption is low. Comparing Examples 1 and 2 with the same battery design parameters with Comparative Examples 1 and 2, due to the different injection methods, there are differences in the infiltration effect of the electrolyte, which is ultimately reflected in the difference in the first efficiency and the capacity retention rate after 1000 cycles. The lithium-ion batteries prepared in Examples 1 and 2 of the present application are superior to Comparative Examples 1 and 2 in terms of both the first efficiency and the capacity retention rate after 1000 cycles.
[0055] In summary, the embodiment of the present application provides a method for manufacturing a lithium-ion battery, which includes sequentially performing a liquid injection step and a formation step. The liquid injection step includes a primary liquid injection and a secondary liquid injection, wherein the primary liquid injection includes injecting only a portion of the organic solvent used to form the electrolyte into the battery housing; the secondary liquid injection includes injecting the remaining portion of the electrolyte used to form the electrolyte into the battery housing, wherein the remaining portion of the electrolyte is the remaining portion of the electrolyte except the organic solvent injected in the primary liquid injection. The primary liquid injection only injects part of the organic solvent and does not contain electrolyte salt, so the viscosity is relatively low, and it can be injected into the battery housing at low pressure, and the injection difficulty is relatively low. And after the primary liquid injection, the organic solvent has a low viscosity, so it can quickly penetrate into the pores of the pole piece to achieve good infiltration. The secondary liquid injection injects the remaining part of the electrolyte into the battery housing. Using the molecular diffusion principle, the relatively high concentration of the injected substance can quickly diffuse along the organic solvent injected in the primary liquid injection, and the penetration efficiency in the pole piece is significantly improved compared to the electrolyte of the complete component. After the secondary liquid injection, the subsequent formation can be carried out after the diffusion is uniform. The manufacturing method of the embodiment of the present application has high electrolyte infiltration efficiency and good infiltration effect, and does not require high-pressure injection and high-temperature standing, thereby saving energy costs and avoiding the decomposition of low-temperature additives in the electrolyte at high temperatures to ensure battery performance. In addition, the embodiment of the present application has low requirements for the electrolyte formula and has good universality.
[0056] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for manufacturing a lithium-ion battery, wherein the lithium-ion battery comprises a battery housing, a pole piece and an electrolyte disposed in the battery housing, wherein the electrolyte comprises an organic solvent and an electrolyte salt dispersed in the organic solvent, wherein: The manufacturing method of the lithium ion battery comprises sequentially performing a liquid injection step and a formation step, wherein the liquid injection step comprises: Primary injection: injecting only a portion of the organic solvent used to constitute the electrolyte into the battery housing, and the organic solvent injected in the primary injection accounts for more than 50% of the total mass of the electrolyte; Secondary injection: injecting the remaining part of the electrolyte into the battery housing, wherein the remaining part of the electrolyte is the rest of the electrolyte except the organic solvent injected in the primary injection.
2. The method for manufacturing a lithium-ion battery according to claim 1, characterized in that: The viscosity of the organic solvent injected in the first injection is lower than 0.7 mPa·s, and the viscosity of the remaining part of the electrolyte injected in the second injection is higher than the viscosity of the organic solvent injected in the first injection and lower than 2.0 mPa·s.
3. The method for manufacturing a lithium-ion battery according to claim 1, characterized in that: The organic solvent includes a chain carbonate solvent.
4. The method for manufacturing a lithium ion battery according to claim 3, characterized in that: The linear carbonate solvent is selected from one or more of ethyl methyl carbonate, dimethyl carbonate and diethyl carbonate.
5. The method for manufacturing a lithium ion battery according to claim 3, characterized in that: The organic solvents injected in the first injection are all chain carbonate solvents.
6. The method for manufacturing a lithium ion battery according to claim 5, characterized in that: A portion of the organic solvent is a chain carbonate solvent, and all the chain carbonate solvent in the electrolyte is injected through the primary injection.
7. The method for manufacturing a lithium ion battery according to claim 3, characterized in that: The linear carbonate solvent accounts for less than 70% of the total mass of the electrolyte.
8. The method for manufacturing a lithium ion battery according to any one of claims 1 to 7, characterized in that: The injection pressure of the primary injection and the secondary injection is no more than 0.3 MPa.
9. The method for manufacturing a lithium ion battery according to any one of claims 1 to 7, characterized in that: The liquid injection step further comprises standing at room temperature for a first preset time between the first liquid injection and the second liquid injection; The method for manufacturing a lithium-ion battery further includes: between the injection step and the formation step, standing at room temperature for a second preset time.
Citation Information
Patent Citations
Lithium ion battery electrolyte injection method
CN108054337A
Preparation method of liquid-replaceable lithium slurry battery
CN113206357A
Liquid injection method of battery and battery
CN118099677A
Manufacturing method of battery and injection method of electrolyte solution
JP2005203120A
Cited By
Battery secondary liquid injection formation method and battery
CN119674284A