Perovskite / crystalline silicon laminated solar cell passivation layer and preparation method and application thereof

The passivation layer is formed by spraying fluoropyridine organic amine hydrochloride, which solves the problems of high manufacturing cost of perovskite/crystalline silicon stacked solar cells on single crystal silicon wafers, and improves photovoltaic performance and stability.

CN119012729APending Publication Date: 2024-11-22NANCHANG UNIV
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411075997.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing perovskite/crystalline silicon stacked solar cells on single crystal silicon wafer polishing and nano-scale suede etching treatment have high manufacturing costs, destroying the optical capture system, and the perovskite film prepared by traditional solution method is on suede The structure is poor in quality and has high density defects, which affects the efficiency and stability of the device.

Method used

Fluoropyridine organic amine hydrochloride is used as a passivator to form a uniform organic ligand passivation layer on the perovskite film by dynamic spraying, inhibiting the formation of low-dimensional perovskites, enhancing the passivation effect, and through dual-dimensional Source coevaporation deposition and spin coating technology prepare perovskite light absorbing layers on suede structures.

Benefits of technology

It effectively improves the photovoltaic performance and stability of solar cells, improves the coverage effect of the passivation layer on the suede texture structure, reduces defect density, and improves the photoelectric conversion efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119012729A_ABST
    Figure CN119012729A_ABST
Patent Text Reader

Abstract

The invention discloses a perovskite / crystalline silicon laminated solar cell passivation layer and a preparation method and application thereof, and fluoropyridine organic amine is deposited on the upper surface of a perovskite film prepared on a large suede heterogeneous crystalline silicon bottom cell through dynamic spraying, so that a uniform shape-maintaining passivation layer is formed on a perovskite top cell absorption layer. The high-polarity fluoropyridine organic amine molecules can effectively passivate defects on the surface of the perovskite thin film, form an interface dipole to improve an interface work function and promote selective transport of carriers, so that the photoelectric property of the large-textured perovskite / crystalline silicon laminated solar cell is remarkably improved, and particularly, the open-circuit voltage and the fill factor are remarkably improved. The method is completely compatible with crystalline silicon cells in an industrial production line, and has important significance for further promoting the commercialization process of perovskite / crystalline silicon solar energy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a perovskite / crystalline silicon stacked solar cell passivation layer and a preparation method thereof. Background Art

[0002] Organic-inorganic hybrid perovskite solar cells have attracted much attention due to their wide absorption range, high absorption coefficient, long carrier lifetime, adjustable band gap in a wide range, and simple solution processing, and have great application prospects. The perovskite / crystalline silicon tandem solar cell obtained by integrating the perovskite top cell with the single-crystalline silicon bottom cell has achieved an ultra-high photoelectric conversion efficiency (PCE) of 33.9%, far exceeding the theoretical efficiency limit of a single solar cell.

[0003] At present, most high-efficiency perovskite / crystalline silicon tandem cells use heterogeneous crystalline silicon bottom cells with single-sided polishing or nano-scale velvet texture structure, which is compatible with the mainstream solution-based deposition of perovskite films. However, polishing and nano-scale velvet etching on single-crystalline silicon wafers will generate a lot of manufacturing costs, destroy the original velvet texture structure's optical capture system, and cause optical absorption loss, thus hindering the commercialization of perovskite / crystalline silicon tandem solar cells.

[0004] The perovskite / crystalline silicon stacked solar cells developed based on heterogeneous crystalline silicon cells with large velvet texture structures of micron-scale pyramids are fully compatible with the current industrial production line silicon wafers. The vacuum / solution mixed two-step deposition method can prepare a conformal perovskite light absorption layer on the velvet texture structure silicon bottom cell, but compared with the traditional solution method, the perovskite film prepared by this method has poor quality, especially on the surface of the perovskite film, which inevitably has a high density of defects, resulting in non-radiative recombination, thereby damaging the efficiency and stability of the device.

[0005] Surface molecular passivation is an effective solution to reduce defects in perovskite / crystalline silicon tandem solar cells. Organic molecules have been widely used in the passivation of high-performance perovskite solar cells, especially amine ligands containing alkyl or aromatic halides, but ligand insertion may induce the formation of low-dimensional perovskites with uncontrollable phase purity. More importantly, the widely used surface passivation method of introducing organic molecules by solution processing faces the great challenge of conformal coverage on velvet-structured perovskite films.

[0006] Therefore, it is necessary to design the corresponding molecular structure and develop a controllable strategy for preparing solar cells suitable for velvet structures. Summary of the invention

[0007] The present invention aims to provide a perovskite / crystalline silicon laminated solar cell passivation layer and a preparation method and application thereof, wherein a fluoropyridine organic amine hydrochloride is sprayed on a perovskite film to form a uniform and conformal organic ligand passivation layer, while inhibiting the formation of low-dimensional perovskite, wherein the fluoropyridine organic amine hydrochloride contains fluorine, pyridine, and amine groups; wherein the electron-withdrawing fluorine group makes the dipole moment of the organic ligand larger, the molecular polarity is high, and it is helpful to combine with the uncoordinated defects on the surface of the perovskite; the pyridine and amine groups can combine with the undercoordinated lead ions (Pb 2+ ) interacts strongly, inhibiting the metallic lead (Pb 0 ) is formed; the fluoropyridine organic amine hydrochloride molecules form a dipole layer, which causes band bending at the perovskite interface and generates an additional built-in electric field; the present invention uses fluoropyridine organic amine hydrochloride as a passivating agent to effectively improve the broad electrical performance of solar cells.

[0008] In a first aspect, the present invention provides a method for preparing a passivation layer of a perovskite / crystalline silicon tandem solar cell, comprising the following steps:

[0009] Using dynamic spraying, a fluoropyridine organic amine hydrochloride solution is sprayed onto the light absorption layer of the perovskite top cell;

[0010] After annealing, forming the perovskite / crystalline silicon stacked solar cell passivation layer on the perovskite top cell light absorption layer;

[0011] The structural formula of the fluoropyridine organic amine hydrochloride is shown in Formula I:

[0012]

[0013] Wherein, the value of n shown in Formula I includes any one of 0, 1, and 2.

[0014] Optionally, the preparation of the perovskite top cell light absorption layer comprises the following steps:

[0015] Depositing a mixed inorganic layer on a silicon bottom cell by dual-source co-evaporation; the mixed inorganic layer comprises lead iodide and cesium bromide;

[0016] The mixed inorganic layer is spin-coated with a mixed formamidine organic amine solution, and the perovskite top cell light absorption layer is prepared after annealing.

[0017] Optionally, during the dynamic spraying process, the rotation speed of the perovskite top cell light absorption layer is 2000-5000r / min.

[0018] Optionally, the silicon bottom cell comprises a heterogeneous crystalline silicon solar cell; the surface of the heterogeneous crystalline silicon solar cell is a micron-scale pyramid velvet surface; the height of the pyramid is 1-5 μm.

[0019] Optionally, the mixed formamidine-organic amine solution includes formamidine hydrochloride, formamidine bromide, and formamidine iodide.

[0020] Optionally, the formamidine concentration in the mixed formamidine-organic amine solution is (0.55-0.65) mol / L.

[0021] In a second aspect, the present invention provides a passivation layer for a perovskite / crystalline silicon tandem solar cell.

[0022] In a third aspect, the present invention provides an application of a passivation layer of a perovskite / crystalline silicon stacked solar cell in preparing a solar cell, comprising the following steps:

[0023] After depositing the composite layer on the heterogeneous crystalline silicon bottom cell, the perovskite top cell was prepared;

[0024] The perovskite top cell comprises: a hole transport layer, a perovskite light absorption layer, a perovskite light absorption layer passivation layer, an electron transport layer, and a perovskite top cell top electrode.

[0025] Optionally, the composite layer includes an indium tin oxide composite layer; the composite layer connects the heterogeneous crystalline silicon bottom cell and the perovskite top cell.

[0026] Optionally, the electron transport layer comprises C 60 Electron transport layer.

[0027] Optionally, the top electrode of the perovskite top cell includes a front indium tin oxide transparent electrode, a silver grid line electrode and a magnesium fluoride anti-reflection layer.

[0028] The beneficial effects of the present invention include:

[0029] (1) The fluoropyridine organic amine hydrochloride provided by the present invention can passivate surface defects by passivating the fluorine, pyridine, and amine groups in the molecules, inhibit non-radiative recombination, and improve carrier collection and transport, thereby effectively improving the photovoltaic performance and stability of the stacked device;

[0030] (2) The method for preparing a passivation layer by dynamic spraying provided by the present invention can form a uniform conformal organic ligand passivation layer on the perovskite film prepared on the velvet silicon substrate. The dynamic spray passivation method improves the disadvantage that the traditional solution method cannot effectively passivate on the velvet texture structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Schematic diagram of dynamic spraying for preparing the passivation layer of perovskite / crystalline silicon tandem solar cells;

[0032] Figure 2 These are the performance test results of the perovskite / crystalline silicon tandem solar cells prepared in the examples and comparative examples. DETAILED DESCRIPTION

[0033] The present invention will be further described through the following embodiments in conjunction with the accompanying drawings.

[0034] In a first aspect, an embodiment of the present invention provides a method for preparing a passivation layer of a perovskite / crystalline silicon tandem solar cell, comprising the following steps:

[0035] Using dynamic spraying, a fluoropyridine organic amine hydrochloride solution is sprayed onto the light absorption layer of the perovskite top cell;

[0036] After annealing, forming the perovskite / crystalline silicon stacked solar cell passivation layer on the perovskite top cell light absorption layer;

[0037] The structural formula of the fluoropyridine organic amine hydrochloride is shown in Formula I:

[0038]

[0039] Wherein, the value of n shown in Formula I includes any one of 0, 1, and 2.

[0040] In some embodiments, the preparation of the perovskite top cell light absorption layer comprises the following steps:

[0041] Depositing a mixed inorganic layer on a silicon bottom cell by dual-source co-evaporation; the mixed inorganic layer comprises lead iodide and cesium bromide;

[0042] The mixed inorganic layer is spin-coated with a mixed formamidine organic amine solution, and the perovskite top cell light absorption layer is prepared after annealing.

[0043] In some embodiments, during the dynamic spraying process, the rotation speed of the perovskite top cell light absorption layer is 2000-5000 r / min.

[0044] In some embodiments, the silicon bottom cell comprises a heterogeneous crystalline silicon solar cell; the surface of the heterogeneous crystalline silicon solar cell is a micron-scale pyramid velvet surface; the height of the pyramid is 1-5 μm.

[0045] Specifically, the mixed formamidine organic amine solution includes formamidine hydrochloride, formamidine bromide, and formamidine iodide.

[0046] Specifically, the formamidine concentration in the mixed formamidine-organic amine solution is (0.55-0.65) mol / L.

[0047] In a second aspect, an embodiment of the present invention provides a passivation layer for a perovskite / crystalline silicon tandem solar cell.

[0048] In a third aspect, an embodiment of the present invention provides an application of a passivation layer of a perovskite / crystalline silicon stacked solar cell in preparing a solar cell, comprising the following steps:

[0049] After depositing the composite layer on the heterogeneous crystalline silicon bottom cell, the perovskite top cell was prepared;

[0050] The perovskite top cell comprises: a hole transport layer, a perovskite light absorption layer, a perovskite light absorption layer passivation layer, an electron transport layer, and a perovskite top cell top electrode.

[0051] In some embodiments, the composite layer includes an indium tin oxide composite layer; the composite layer connects the heterogeneous crystalline silicon bottom cell and the perovskite top cell.

[0052] In some embodiments, the electron transport layer comprises C 60 Electron transport layer.

[0053] In some embodiments, the top electrode of the perovskite top cell includes a front indium tin oxide transparent electrode, a silver grid line electrode and a magnesium fluoride anti-reflection layer.

[0054] The raw materials and reagents used in the examples of the present invention were purchased through commercial channels; the fluoropyridine organic amine hydrochloride used in the examples of the present invention was purchased from Shanghai Bid Pharmaceutical Technology Co., Ltd.

[0055] Preparation Example 1

[0056] Preparation Example 1 of the present invention provides a method for preparing a passivation layer of a perovskite / crystalline silicon stacked solar cell, wherein the spraying method is as follows: Figure 1 As shown, the following steps are included:

[0057] Dissolve 4-fluoropyridine ethylamine hydrochloride in isopropanol to prepare a 4-fluoropyridine ethylamine hydrochloride solution with a concentration of 1.0 mg / mL, pour the solution into a spraying device, spray for 30s-90s, and form a passivation layer with a thickness of 1-3nm; the spraying parameters are set as follows: the distance between the nozzle and the perovskite light absorption layer is 5cm, the spray pressure is 0.3MPa, and the spraying speed is 2.5mm / s;

[0058] The perovskite absorption layer in the coating machine was rotated at a speed of 4000 r / min. After spraying, it was annealed at 100° C. for 2 min to obtain the passivation layer of the perovskite / crystalline silicon stacked solar cell.

[0059] Example 1

[0060] Embodiment 1 of the present invention provides an application of a passivation layer in a perovskite / crystalline silicon tandem solar cell, comprising the following steps:

[0061] D1. Preparation of heterogeneous crystalline silicon bottom cells

[0062] Take an intrinsic single crystal silicon wafer with a resistivity of 1-5 ohms and a thickness of 150 μm, and grow 7 nm of intrinsic amorphous silicon on the front and back of the intrinsic single crystal silicon wafer respectively by plasma enhanced chemical vapor deposition;

[0063] On the intrinsic amorphous silicon grown on the front side, a 6nm thick n-type amorphous silicon film is deposited by plasma enhanced chemical vapor deposition, and on the intrinsic amorphous silicon grown on the back side, a 8nm thick p-type amorphous silicon film is deposited by plasma enhanced chemical vapor deposition;

[0064] A back indium tin oxide transparent electrode with a thickness of 80 nm is deposited on the p-type amorphous silicon film using a magnetron sputtering device;

[0065] A 400nm thick silver electrode was deposited on the back indium tin oxide transparent electrode by thermal evaporation vacuum deposition equipment to prepare a heterogeneous crystalline silicon bottom cell;

[0066] D2. Preparation of composite layer

[0067] The heterogeneous crystalline silicon bottom cell facing downward is placed in a customized mask, and the mask is placed on a carrier in a magnetron sputtering device to deposit 20nm of indium tin oxide as a composite layer; the composite layer connects the heterogeneous crystalline silicon bottom cell and the perovskite top cell;

[0068] D3. Preparation of perovskite top cell

[0069] D31. Preparation of hole transport layer of perovskite top cell

[0070] A nickel oxide hole transport layer with a thickness of 20 nm is deposited on the composite layer by magnetron sputtering to prepare a conductive substrate with a hole transport layer;

[0071] D32. Preparation of perovskite top cell light absorption layer

[0072] The conductive substrate prepared in step D31 is transferred to a dual-source co-evaporation thin film deposition system on a customized mask, and the temperatures of the two evaporation sources are increased to stabilize the evaporation rate ratio of lead iodide and cesium bromide at 1.0 angstroms / second and 0.1 angstroms / second, and then the substrate baffle is opened. After the co-evaporation is completed, a mixed inorganic layer with a thickness of 480 nm is obtained;

[0073] Dissolve formamidine hydroiodide, formamidine hydrobromide, and formamidine hydrochloride in anhydrous ethanol at a molar ratio of 0.75:0.25:0.02, and the total concentration of formamidine is 0.59 mol / L, to obtain a mixed formamidine organic amine solution;

[0074] In a nitrogen atmosphere glove box, 100 μL of the mixed formamidine organic amine solution was spin-coated on the mixed inorganic layer at a speed of 4000 r / min;

[0075] After the spin coating is completed, the perovskite light absorption layer is prepared by annealing in air at a relative humidity of 45% and 150°C for 30 minutes;

[0076] D33. Preparation of perovskite top cell passivation layer

[0077] The passivation layer was prepared by the same steps and conditions as in Preparation Example 1;

[0078] D34. Preparation of electron transport layer of perovskite top cell

[0079] On the surface of the passivation layer, a 12 nm C layer was deposited at a deposition rate of 0.15 Å / s using a thermal evaporation device. 60 As an electron transport layer, it was transferred to an atomic layer deposition device and deposited by tin source and water source for 100 cycles to obtain a SnO layer with a thickness of 20 nm. 2 Buffer layer;

[0080] The parameters were set as follows: tin source pulse time 1 s, water source deposition pulse time 0.1 s, purge time 15 s, gas flow rate 40 sccm;

[0081] D35. Preparation of top electrode of perovskite cell

[0082] Using magnetron sputtering equipment on SnO 2 A layer of 80nm thick indium tin oxide transparent electrode is deposited on the surface of the buffer layer, and then a 400nm thick silver grid electrode is deposited. The effective area of ​​the silver grid electrode is 1cm 2 , and finally a magnesium fluoride anti-reflection layer with a thickness of 100nm is deposited; finally, a perovskite / crystalline silicon stacked solar cell is produced.

[0083] Comparative Example 1

[0084] Comparative Example 1 of the present invention provides a preparation of a perovskite / crystalline silicon tandem solar cell, which is different from Example 1 in that the passivation layer preparation in step D33 is not performed, and a perovskite / crystalline silicon tandem solar cell without a passivation layer is obtained.

[0085] Performance Verification

[0086] (1) Battery performance verification

[0087] The performance of the solar cells in Example 1 and Comparative Example 1 was tested by a solar simulator. The results are as follows: Figure 2 As shown, Figure 2 A in is the test result of comparative example 1, Figure 2 B in is the test result of Example 1;

[0088] See also Figure 2 , Comparative Example 1( Figure 2The current-voltage curve of the unpassivated perovskite / crystalline silicon tandem solar cell in A) shows that the short-circuit current density is 20.25 mA / cm 2 , the open circuit voltage is 1.87V, the fill factor is 76.61%, and the photoelectric conversion efficiency (PCE) is 28.72%; Example 1 ( Figure 2 The short-circuit current density of the perovskite / crystalline silicon tandem solar cell in B) is 20.28 mA / cm 2 , the open circuit voltage is 1.94V, the fill factor is 79.13%, and the photoelectric conversion efficiency (PCE) is 31.13%; compared with Comparative Example 1, the open circuit voltage and fill factor of the stacked device are significantly improved, thereby improving the photoelectric performance.

[0089] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A method for preparing a passivation layer of a perovskite / crystalline silicon tandem solar cell, characterized in that: The following steps are involved: Using dynamic spraying, a fluoropyridine organic amine hydrochloride solution is sprayed onto the light absorption layer of the perovskite top cell; After annealing, forming the perovskite / crystalline silicon stacked solar cell passivation layer on the perovskite top cell light absorption layer; The structural formula of the fluoropyridine organic amine hydrochloride is shown in Formula I: Wherein, the value of n shown in Formula I includes any one of 0, 1, and 2.

2. The preparation method according to claim 1, characterized in that: The preparation of the perovskite top cell light absorption layer comprises the following steps: Depositing a mixed inorganic layer on a silicon bottom cell by dual-source co-evaporation; the mixed inorganic layer comprises lead iodide and cesium bromide; The mixed inorganic layer is spin-coated with a mixed formamidine organic amine solution, and the perovskite top cell light absorption layer is prepared after annealing.

3. The preparation method according to claim 1, characterized in that: During the dynamic spraying process, the rotation speed of the perovskite top cell light absorption layer is 2000-5000r / mmin.

4. The preparation method according to claim 2, characterized in that: The silicon bottom cell comprises a heterogeneous crystalline silicon solar cell; the surface of the heterogeneous crystalline silicon solar cell is a micron-level pyramid velvet surface; the height of the pyramid is 1-5 μm.

5. The preparation method according to claim 2, characterized in that: The mixed formamidine organic amine solution comprises formamidine hydrochloride, formamidine bromide and formamidine iodide.

6. A passivation layer for a perovskite / crystalline silicon tandem solar cell prepared by the preparation method according to any one of claims 1 to 5.

7. An application of the preparation method according to any one of claims 1 to 5 in the preparation of a perovskite / crystalline silicon tandem solar cell, characterized in that: The following steps are involved: After depositing the composite layer on the heterogeneous crystalline silicon bottom cell, the perovskite top cell was prepared; The perovskite top cell comprises: a hole transport layer, a perovskite light absorption layer, a perovskite light absorption layer passivation layer, an electron transport layer, and a perovskite top cell top electrode.

Citation Information

Cited By

  • Perovskite solar cell based on synergistic effect of additive and passivator and preparation method thereof

    CN121001506A

  • Perovskite solar cell based on action of strong electron withdrawing group substituted fluoropyridine additive and preparation method thereof

    CN121152466A

  • Perovskite solar cell based on fluoropyridine additive with strong electron-withdrawing group substitution and preparation method thereof

    CN121152466B

  • Perovskite / crystalline silicon laminated solar cell and packaging method and application thereof

    CN121152480A