Positive electrode and secondary battery including same
By using a combination of single-particle or pseudo-single-particle lithium composite transition metal oxides and few-walled carbon nanotubes and single-walled carbon nanotubes in lithium secondary batteries, the problems of poor conductivity and reduced capacity of positive electrode active materials are solved, achieving high conductivity, low resistance and high capacity of the battery, and improving battery life and stability.
Patent Information
- Application Number
- CN202380034030.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-20
- Filing Date
- 2023-04-20
- Publication Date
- 2024-11-22
AI Technical Summary
In existing lithium secondary batteries, single-particle positive electrode active materials suffer from poor conductivity and reduced capacity. In particular, when using conventional multi-walled carbon nanotubes as conductive agents, it is difficult to effectively cover the surface of the positive electrode active material, resulting in increased resistance and reduced capacity.
Lithium composite transition metal oxides in single-particle or pseudo-single-particle form are used as positive electrode active materials, and few-walled carbon nanotubes and single-walled carbon nanotubes are combined as conductive agents. The few-walled carbon nanotubes with a wall number in the range of 2 to 7 can effectively cover the surface of the positive electrode active material, while the single-walled carbon nanotubes ensure electrical connection, reduce resistance and improve conductivity.
By improving the conductivity and capacity of the positive electrode, reducing resistance, improving battery life and storage performance, while maintaining high capacity, reducing gas generation, and enhancing battery stability.
Smart Images

Figure BDA0005082876520000201 
Figure BDA0005082876520000211
Abstract
Description
Technical Field
[0001] This application claims priority to Korean Patent Application No. 10-2022-0049176, filed on April 20, 2022, the disclosure of which is incorporated herein by reference.
[0002] The present invention relates to a positive electrode and a secondary battery, the positive electrode comprising a positive electrode active material in a single particle form or a pseudo single particle form and a conductive agent including few-walled carbon nanotubes and single-walled carbon nanotubes. Background Art
[0003] A lithium secondary battery is generally composed of a positive electrode, a negative electrode, a separator, and an electrolyte, and the positive electrode and the negative electrode respectively contain active materials capable of intercalating and deintercalating lithium ions.
[0004] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMnO4) or lithium iron phosphate compound (LiFePO4) have been used as positive electrode active materials for lithium secondary batteries. Among them, lithium cobalt oxide has the advantages of high operating voltage and excellent capacity characteristics, but it is difficult to be used commercially for large-capacity batteries due to the high price and supply instability of cobalt as a raw material. Since lithium nickel oxide has poor structural stability, it is difficult to achieve sufficient life characteristics. Lithium manganese oxide has excellent stability, but has the problem of poor capacity characteristics. Therefore, lithium composite transition metal oxides containing two or more types of transition metals have been developed to make up for the problems of lithium transition metal oxides containing only nickel (Ni), cobalt (Co) or manganese (Mn), and among them, lithium nickel cobalt manganese oxide containing Ni, Co and Mn has been widely used in the field of electric vehicle batteries.
[0005] Conventional lithium nickel cobalt manganese oxide is generally in the form of spherical secondary particles in which hundreds of primary particles are aggregated. However, with respect to lithium nickel cobalt manganese oxide in the form of secondary particles in which many primary particles are aggregated as described above, there is a problem that particle breakage in which primary particles fall off during rolling during positive electrode preparation, and cracks appear in particles during charging and discharging may occur. In the event that particle breakage or cracking of the positive electrode active material occurs, because the contact area with the electrolyte solution increases, degradation of the active material and gas generation due to side reactions with the electrolyte solution increase, and thus there is a problem of reduced life characteristics. In particular, with respect to positive electrode active materials having a high nickel content, since a large amount of highly reactive Ni is generated if charging and discharging of the battery is repeated, the positive electrode active material is likely to be damaged. 4+ ions, structural collapse of the positive electrode active material occurs, and thus there is a problem that degradation of the positive electrode active material further increases and the life characteristics and safety of the battery further decrease.
[0006] Therefore, attempts have been made to use positive electrode active materials in the form of single particles with excellent particle strength. However, since the surface area of the positive electrode active material in the form of a single particle is relatively large, a relatively large amount of conductive agent is required to fully cover the surface of the positive electrode active material in the form of a single particle with the conductive agent. In other words, in the case of using the same amount of conductive agent as in the related art, the surface of the positive electrode active material may not be effectively covered by the conductive agent because the number of conductive agents is small. Such a problem particularly occurs when conventional multi-walled carbon nanotubes are used as conductive agents. The conventionally mainly used multi-walled carbon nanotubes are carbon nanotubes with a wall number of 8 or more, wherein, since the number of multi-walled carbon nanotubes contained in the positive electrode is not large, unless the amount of multi-walled carbon nanotubes is increased, the surface of the positive electrode active material may not be effectively covered by the multi-walled carbon nanotubes. Therefore, there is a problem that the resistance of the positive electrode increases due to the decrease in the conductivity of the positive electrode active material. In the case of increasing the amount of the conventionally used conductive agent to solve this problem, the capacity of the positive electrode may decrease due to the relative decrease in the amount of the positive electrode active material.
[0007] Therefore, there is a need to develop a technology capable of ensuring a positive electrode having low resistance and high capacity while using a positive electrode active material in a single particle form. Summary of the invention
[0008] Technical issues
[0009] One aspect of the present invention provides a positive electrode and a secondary battery. Specifically, when a lithium composite transition metal oxide in a single particle form or a pseudo single particle form is used in the positive electrode, an object of the present invention is to provide a technology capable of reducing the resistance of the positive electrode by improving the conductivity of the positive electrode while maintaining the capacity of the positive electrode at a high level.
[0010] Technical Solution
[0011] According to one embodiment of the present invention, a positive electrode is provided, comprising a positive electrode active material layer, wherein the positive electrode active material layer contains a positive electrode active material and a conductive agent, wherein the positive electrode active material comprises a first lithium composite transition metal oxide in the form of a single particle composed of one primary particle or in the form of a pseudo-single particle as an aggregate of 10 or less primary particles, and the conductive agent comprises few-walled carbon nanotubes and single-walled carbon nanotubes, wherein the number of walls of the few-walled carbon nanotubes is in the range of 2 to 7.
[0012] According to another embodiment of the present invention, provided is a secondary battery including the positive electrode.
[0013] Beneficial Effects
[0014] Since the positive electrode according to the present invention comprises a first lithium composite transition metal oxide in the form of a single particle or a pseudo single particle, the capacity and output of the positive electrode can be improved. In addition, with respect to the few-walled carbon nanotubes with a wall number in the range of 2 to 7, a larger number of carbon nanotubes can be included in the same amount compared to conventional multi-walled carbon nanotubes (e.g., a wall number of 8 or more). Therefore, the few-walled carbon nanotubes with a wall number in the range of 2 to 7 can be effectively adsorbed on the surface of a single particle and / or a pseudo single particle, and the conductivity of the first lithium composite transition metal oxide can be significantly improved. In addition, the single-walled carbon nanotubes can maintain the electrical connection between the first lithium composite transition metal oxide. Therefore, since the resistance of the positive electrode can be significantly reduced, the resistance of the secondary battery can be reduced, and the capacity, life and storage performance can be improved.
[0015] In addition, in the case of using a combination of few-walled carbon nanotubes and single-walled carbon nanotubes having a wall number in the range of 2 to 7, since the binder in the positive electrode can be uniformly dispersed and present, the binder content for ensuring the adhesiveness of the positive electrode can be low. Therefore, since the amount of the positive electrode active material can be relatively increased, the capacity of the positive electrode can be improved. DETAILED DESCRIPTION
[0016] Hereinafter, the present invention will be described in more detail.
[0017] It is to be understood that the words or terms used in the specification and claims should not be interpreted as the meanings defined in commonly used dictionaries, and it is to be further understood that based on the principle that the inventor can appropriately define the meanings of words or terms to best illustrate the present invention, the words or terms should be interpreted as having a meaning consistent with their meanings in the context of the relevant technology and the technical concept of the invention.
[0018] In the present invention, the expression "primary particle" means a particle unit in which no grain boundary exists in appearance when observed by using a scanning electron microscope with a field of view of 5000 to 20000 times. The expression "average particle size of primary particles" means the arithmetic mean of particle sizes calculated after measuring the particle sizes of primary particles observed in a scanning electron microscope image.
[0019] In the present invention, the expression "secondary particle" is a particle formed by aggregating a plurality of primary particles. In the present invention, a secondary particle in which 10 or less primary particles are aggregated is called a pseudo single particle to distinguish it from a conventional secondary particle formed by aggregating tens to hundreds of primary particles.
[0020] The expression "average particle size D" in the present invention is 50" means the particle size of 50% based on the volume cumulative particle size distribution of the lithium composite transition metal oxide powder or the positive electrode active material powder, wherein, in the case where the lithium composite transition metal oxide is a secondary particle, it means the average particle size of the secondary particle. The average particle size D 50 It can be measured by using a laser diffraction method. For example, after dispersing the lithium composite transition metal oxide powder or the positive electrode active material powder in a dispersion medium, the dispersion medium is introduced into a commercial laser diffraction particle size measuring instrument (e.g., Microtrac MT 3000), and then irradiated with an ultrasonic wave of about 28 kHz with an output of 60 W to obtain a volume cumulative particle size distribution diagram, and then the average particle size D can be measured by obtaining the particle size corresponding to 50% volume cumulative amount. 50 .
[0021] The "specific surface area" in the present invention is measured by the Brunauer-Emmett-Teller (BET) method, wherein, specifically, the specific surface area can be calculated from the nitrogen adsorption amount at liquid nitrogen temperature (77K) using BELSORP-mino II of BEL Japan Inc.
[0022] In the present invention, carbon nanotubes refer to allotropes of carbon that have a columnar nanostructure and include walls that constitute the side surfaces of the column and are formed of carbon atoms. Tubular carbon nanotubes having a wall number of 1 are called single-walled carbon nanotubes, carbon nanotubes having a wall number of 2 to 7 are classified as few-walled carbon nanotubes, and carbon nanotubes having a wall number of 8 or more are classified as multi-walled carbon nanotubes.
[0023] <Positive electrode>
[0024] According to one embodiment of the present invention, a positive electrode includes a positive electrode active material layer, wherein the positive electrode active material layer contains a positive electrode active material and a conductive agent, wherein the positive electrode active material includes a first lithium composite transition metal oxide in the form of a single particle composed of one primary particle or in the form of a pseudo-single particle as an aggregate of 10 or less primary particles, and the conductive agent includes few-walled carbon nanotubes and single-walled carbon nanotubes, wherein the number of walls of the few-walled carbon nanotubes can be in the range of 2 to 7.
[0025] The positive electrode may include a positive electrode active material layer. Specifically, the positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, or the positive electrode may be composed of only the positive electrode active material layer without the positive electrode current collector.
[0026] The positive electrode current collector is not particularly limited as long as it has conductivity without causing adverse chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, fired carbon, or aluminum or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can generally have a thickness of 3 μm to 500 μm, and microscopic irregularities can be formed on the surface of the current collector to improve the adhesion of the positive electrode active material. The positive electrode current collector can be used in various shapes, such as films, sheets, foils, nets, porous bodies, foams, non-woven fabric bodies, etc.
[0027] The positive electrode active material layer may include a positive electrode active material and a conductive agent.
[0028] (1) Positive electrode active material
[0029] The positive electrode active material may include the first lithium composite transition metal oxide in a single particle form composed of one primary particle or in a pseudo single particle form as an aggregate of 10 or less primary particles. Specifically, the positive electrode active material may be formed of the first lithium composite transition metal oxide.
[0030] The first lithium composite transition metal oxide may be in the form of a single particle composed of one primary particle, or in the form of a pseudo-single particle as an aggregate of 10 or less, preferably 2 to 10, and more preferably 2 to 8 primary particles.
[0031] Conventionally, spherical secondary particles in which tens to hundreds of primary particles are gathered are generally used as positive electrode active materials for lithium secondary batteries. However, with respect to the positive electrode active material in the form of secondary particles in which many primary particles are gathered as described above, there is a problem that particle rupture in which the primary particles fall off during the rolling process during the preparation of the positive electrode may occur, and cracks may appear in the particles during charging and discharging. In the case of particle rupture or cracking of the positive electrode active material, due to the increase in the contact area with the electrolyte solution, the side reaction with the electrolyte solution increases, resulting in transition metal dissolution and gas generation, and therefore the battery performance may be rapidly reduced, or in severe cases, the battery may explode or catch fire.
[0032] In contrast, since the first lithium composite transition metal oxide in the form of a single particle composed of one primary particle or a pseudo-single particle form in which 10 or fewer primary particles are aggregated has a higher particle strength than the conventional positive electrode active material in the form of a secondary particle in which dozens to hundreds of primary particles are aggregated, particle breakage hardly occurs during roll pressing. In addition, regarding the positive electrode active material in the single particle form or the pseudo-single particle form, since the number of primary particles constituting the particles is small, the change caused by the volume expansion and contraction of the primary particles during charging and discharging is small, and thus, the occurrence of cracks in the particles is significantly reduced. Therefore, since the amount of gas generation during battery operation can be reduced, the stability of the battery can be improved.
[0033] The first lithium composite transition metal oxide may include a compound represented by the following [Formula 1].
[0034] [Formula 1]
[0035] Li a1 [Ni b1 Co c1 M 1 d1 M 2 e1 O2
[0036] In Formula 1, M 1 may be at least one selected from manganese (Mn) and aluminum (Al), M 2 may be at least one selected from zirconium (Zr), tungsten (W), yttrium (Y), barium (Ba), calcium (Ca), titanium (Ti), magnesium (Mg), tantalum (Ta), and niobium (Nb), and 0.8 ≤ a1 ≤ 1.2, 0.8 ≤ b1 < 1, 0 < c1 < 0.2, 0 < d1 < 0.2, and 0 ≤ e1 ≤ 0.1.
[0037] In Formula 1, M 1 may be at least one selected from Mn and Al, and may specifically be Mn or Mn and Al.
[0038] M 2 may be at least one selected from Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb, may specifically be at least one selected from Zr, Y, Mg, and Ti, and may be more preferably Zr, Y, or a combination thereof. The element M 2 is not necessarily included, but when it is included in an appropriate amount, it may play a role in promoting grain growth or improving crystal structure stability during sintering.
[0039] a1 represents the molar ratio of lithium in the first lithium composite transition metal oxide, where a1 can satisfy 0.8 ≤ a1 ≤ 1.2, 0.85 ≤ a1 ≤ 1.15, or 0.9 ≤ a1 ≤ 1.2. When the molar ratio of lithium satisfies the above ranges, the crystal structure of the lithium-based nickel oxide can be stably formed.
[0040] b1 represents the molar ratio of nickel in all metals other than lithium in the first lithium composite transition metal oxide, where b1 can satisfy 0.8 ≤ b1 < 1, 0.82 ≤ b1 < 1, or 0.83 ≤ b1 < 1. When the molar ratio of nickel satisfies the above ranges, high energy density can be exhibited to achieve high capacity.
[0041] c1 represents the molar ratio of cobalt in all metals other than lithium in the first lithium composite transition metal oxide, where c1 can satisfy 0 < c1 < 0.2, 0 < c1 < 0.18, or 0.01 ≤ c1 ≤ 0.17. When the molar ratio of cobalt satisfies the above ranges, good resistance characteristics and output characteristics can be achieved.
[0042] d1 represents the molar ratio of element M in all metals other than lithium in the first lithium composite transition metal oxide 1 where d1 can satisfy 0 < d1 < 0.2, 0 < d1 < 0.18, or 0.01 ≤ d1 ≤ 0.17. When the molar ratio of element M 1 satisfies the above ranges, the structural stability of the positive electrode active material is excellent.
[0043] e1 represents the molar ratio of element M in all metals other than lithium in the first lithium composite transition metal oxide 2 where e1 can satisfy 0 ≤ e1 ≤ 0.1 or 0 ≤ e1 ≤ 0.05.
[0044] The compound represented by [Equation 1] contains a large amount of nickel. As the amount of nickel increases, the cracking phenomenon of the positive electrode active material during the process of preparing the positive electrode (for example, the rolling process) increases, and the amount of small-sized positive electrode active material (fine powder) increases. The surface of the positive electrode active material must be sufficiently covered by a conductive agent to improve the conductivity of the positive electrode. Among them, if the fine powder increases as described above, there is a problem that the surface of the positive electrode active material to be covered by the conductive agent increases excessively. Since the amount of multi-walled carbon nanotubes increases excessively in order to sufficiently cover the increased surface of the positive electrode active material with conventional multi-walled carbon nanotubes, the capacity of the positive electrode may decrease. In contrast, if the few-walled carbon nanotubes with 2 to 7 walls of the present invention are used, since a relatively large number of carbon nanotubes can be included for the same amount, the total surface area increased by the fine powder of the positive electrode active material can be sufficiently and effectively covered. Therefore, the conductivity of the positive electrode can be improved while maintaining the capacity of the positive electrode.
[0045] The average particle size of the primary particles (the primary particles contained in single particles or pseudo single particles) included in the first lithium composite transition metal oxide may be in the range of 1 μm to 10 μm, particularly 2 μm to 7 μm, and more particularly 3 μm to 5 μm. When the average particle size of the primary particles satisfies the above range, even during roll pressing, the breakage of the first lithium composite transition metal oxide can be suppressed, and the output characteristics can be improved by ensuring the lithium diffusion path.
[0046] The Brunauer-Emmett-Teller (BET) specific surface area of the first lithium composite transition metal oxide may be from 0.1 m 2 / g to 3 m 2 / g, particularly 0.3 m 2 / g to 2 m 2 / g, and more particularly 0.5 m 2 / g to 1.0 m 2 / g. When the above range is satisfied, since the breakage phenomenon of the positive electrode active material during the roll pressing process can be reduced, the amount of fine positive electrode active material powder can be reduced, and thus the gas generation during battery operation can be minimized.
[0047] The positive electrode active material may further include a second lithium composite transition metal oxide. The second lithium composite transition metal oxide may include a compound represented by the following [Formula 2].
[0048] [Formula 2]
[0049] Li a2 [Ni b2 Co c2 M 3 d2 M 4 e2 O2
[0050] In Formula 1, M 3 may be at least one selected from Mn and Al, M 4 may be at least one selected from Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb, and 0.8 ≤ a2 ≤ 1.2, 0.8 ≤ b2 < 1, 0 < c2 < 0.17, 0 < d < 0.17, and 0 ≤ e2 ≤ 0.1.
[0051] a2 represents the molar ratio of lithium in the second lithium composite transition metal oxide, where a2 may satisfy 0.8 ≤ a2 ≤ 1.2, 0.85 ≤ a2 ≤ 1.15, or 0.9 ≤ a2 ≤ 1.2. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium nickel-based oxide can be stably formed.
[0052] b2 represents the molar ratio of nickel among all metals other than lithium in the second lithium composite transition metal oxide, where b2 can satisfy 0.8 ≤ b2 < 1, 0.82 ≤ b2 < 1, or 0.83 ≤ b2 < 1. When the molar ratio of nickel satisfies the above ranges, high energy density can be exhibited to achieve high capacity.
[0053] c2 represents the molar ratio of cobalt among all metals other than lithium in the second lithium composite transition metal oxide, where c2 can satisfy 0 < c2 < 0.2, 0 < c2 < 0.18, or 0.01 ≤ c2 ≤ 0.17. When the molar ratio of cobalt satisfies the above ranges, good resistance characteristics and output characteristics can be achieved.
[0054] d2 represents the molar ratio of element M among all metals other than lithium in the second lithium composite transition metal oxide 3 where d2 can satisfy 0 < d2 < 0.2, 0 < d2 < 0.18, or 0.01 ≤ d2 ≤ 0.17. When the molar ratio of element M 3 satisfies the above ranges, the structural stability of the positive electrode active material is excellent.
[0055] e2 represents the molar ratio of element M among all metals other than lithium in the second lithium composite transition metal oxide 4 where e2 can satisfy 0 ≤ e2 ≤ 0.1 or 0 ≤ e2 ≤ 0.05.
[0056] The second lithium composite transition metal oxide can be secondary particles having a form in which dozens or hundreds of primary particles are bound to each other by granulation. Specifically, the second lithium composite transition metal oxide can be secondary particles in which more than 10 primary particles are granulated.
[0057] Since the second lithium composite transition metal oxide is used in combination with the first lithium composite transition metal oxide, the positive electrode active material can have a bimodal particle size distribution. The bimodal particle size distribution can mean that particles having different particle size distributions are mixed with each other to have a particle size distribution including at least two peaks during particle size analysis by the laser diffraction method mentioned in the specification.
[0058] When the second lithium composite transition metal oxide is used in combination with the first lithium composite transition metal oxide, since the filling rate of the positive electrode active material layer increases, the desired thickness of the positive electrode can be achieved even with a smaller force during roll pressing, and thus, the breakage of the positive electrode active material can be minimized, and the energy density of the battery can be improved. In addition, since the total specific surface area of the positive electrode active material can be reduced compared to the case of using only the first lithium composite transition metal oxide, the same level of battery output performance can be obtained even with a small amount of conductive agent, and the capacity of the battery can be improved.
[0059] The average particle size D of the second lithium composite transition metal oxide 50 It may be in the range of 10 μm to 20 μm, particularly 12 μm to 18 μm, and more particularly 13 μm to 17 μm. When the above range is satisfied, since the filling rate of the positive electrode active material layer is increased, the desired thickness of the positive electrode can be achieved even with a smaller force during rolling, and thus, the cracking of the positive electrode active material can be minimized, and the energy density of the battery can be improved. The above average particle size D in this paragraph 50 Means the average particle size D of the secondary particles 50 .
[0060] When the first lithium composite transition metal oxide and the second lithium composite transition metal oxide are used in combination, since the filling rate of the positive electrode active material layer is increased, the desired thickness of the positive electrode can be achieved even with a smaller force during rolling, and therefore, the rupture of the positive electrode active material can be minimized, and the energy density of the battery can be improved. In addition, when the first lithium composite transition metal oxide and the second lithium composite transition metal oxide are used in combination, since the rupture phenomenon of the positive electrode active material can be improved, the level of gas generation in the battery can be reduced. In addition, since the total specific surface area of the positive electrode active material can be at an appropriate level when the first lithium composite transition metal oxide and the second lithium composite transition metal oxide are used in combination, the same level of battery output can be obtained even with a small amount of conductive agent, and therefore, the battery capacity can be improved by relatively increasing the amount of positive electrode active material.
[0061] The weight ratio of the first lithium composite transition metal oxide to the second lithium composite transition metal oxide may be in the range of 1:9 to 5:5, particularly 2:8 to 4:6, and more particularly 3:7 to 4:6. When the above range is met, the space between the second lithium composite transition metal oxides can be effectively filled with the fine powder of the second lithium composite transition metal oxide and the first lithium composite transition metal oxide. Therefore, since the desired thickness of the positive electrode can be achieved even with less force during the rolling process, the cracking of the positive electrode active material can be further minimized, and the energy density of the battery can be further improved.
[0062] (2) Conductive agent
[0063] The conductive agent may include few-walled carbon nanotubes having a wall number of 2 to 7; and single-walled carbon nanotubes.
[0064] The number of walls of conventional multi-walled carbon nanotubes commonly used is 8 or more (e.g., 8 to 11). In the case of a typical positive electrode active material in the form of secondary particles, sufficient conductivity can be achieved even if conventional multi-walled carbon nanotubes are used in a small amount (e.g., 0.4 wt % to 0.6 wt %). However, with respect to the first lithium composite transition metal oxide in the form of a single particle or a pseudo-single particle, since it has a higher resistance and a larger surface area than the conventional positive electrode active material in the form of secondary particles, when the same amount of multi-walled carbon nanotubes as in the case of using the positive electrode active material in the form of secondary particles is used, the surface of the first lithium composite transition metal oxide is not fully covered by the multi-walled carbon nanotubes, and thus the problem of reduced conductivity of the positive electrode occurs. Therefore, in order to achieve sufficient conductivity by using conventional multi-walled carbon nanotubes having a wall number of 8 or more, the amount of the conductive agent must be high, wherein, if the amount of the multi-walled carbon nanotubes increases, agglomeration of the positive electrode slurry occurs and the viscosity increases, and thus the coating characteristics deteriorate. Therefore, in order to smoothly coat the characteristics, the viscosity of the positive electrode slurry must be reduced by reducing the solid content in the positive electrode slurry. However, if the solid content in the positive electrode slurry is reduced, there is a problem that the amount of active material is reduced, thereby reducing the capacity characteristics. In addition, since the amount of the first lithium composite transition metal oxide is relatively reduced when the amount of multi-walled carbon nanotubes is increased, there is also a problem of reduced capacity.
[0065] As a result of a large number of studies conducted to solve these problems, the present inventors have confirmed that, in the case of using a few-walled carbon nanotube and a single-walled carbon nanotube having a wall number of 2 to 7 as a conductive agent together with a first lithium composite transition metal oxide in a single particle form or a pseudo-single particle form, since the number of carbon nanotubes contained in the positive electrode active material layer increases even if the same or less amount of carbon nanotubes as in the related art is used, the surface of the positive electrode active material can be fully covered with the carbon nanotubes, and thus the resistance of the positive electrode is significantly reduced. In addition, in this case, the present inventors found that even if the solid content of the positive electrode slurry is high (e.g., 70 wt % to 80 wt %), the viscosity of the positive electrode slurry can be kept low, and the coating characteristics of the positive electrode slurry can be improved to increase the capacity of the positive electrode.
[0066] 1) Few-walled carbon nanotubes with 2 to 7 walls
[0067] The few-walled carbon nanotubes having a wall number of 2 to 7 may exist by being adsorbed on the surface of the positive electrode active material (e.g., the surface of the first lithium composite transition metal oxide and / or the second lithium composite transition metal oxide to be described later). The few-walled carbon nanotubes improve the conductivity of the positive electrode by covering the surface of the positive electrode active material or connecting the positive electrode active material.
[0068] The wall number of the few-walled carbon nanotubes may be in the range of 2 to 7, preferably 2 to 6, and more preferably 3 to 6. In the case where the wall number is less than 2, the packing density of the carbon nanotubes may be reduced, so that the transportation and input of the carbon nanotubes may not be smooth, and the productivity of the positive electrode may be reduced due to excessive increase in the viscosity of the positive electrode slurry composition. In the case where the wall number is greater than 7, the effect of improving the resistance characteristics of the positive electrode and the slurry viscosity is reduced.
[0069] In the present invention, by using a few-walled carbon nanotube with a wall number of 2 to 7, the productivity of the positive electrode can be ensured, and at the same time, the conductivity of the positive electrode can be effectively improved. More specifically, when a first lithium composite transition metal oxide in a single particle form or a pseudo-single particle form with a large surface area is used, a sufficient number of carbon nanotubes is required to fully cover the surface of the first lithium composite transition metal oxide. Regarding the few-walled carbon nanotube with a wall number of 2 to 7, since the number of carbon nanotubes of the same amount is greater than the number of multi-walled carbon nanotubes, even a relatively small amount can effectively cover the surface of the first lithium composite transition metal oxide, and thus the conductivity of the positive electrode can be significantly improved. In addition, since the conductivity is ensured without increasing the amount of carbon nanotubes, a relatively large amount of positive electrode active material can be included, and thus the capacity of the positive electrode can be ensured.
[0070] The BET specific surface area of few-walled carbon nanotubes can be 300 m 2 / g to 500m 2 / g, preferably 330m 2 / g to 500m 2 / g, and more preferably 400m 2 / g to 500m 2 In the case of satisfying the above range, since the transportation and input of the few-walled carbon nanotubes are smooth, the productivity of the positive electrode can be improved. In addition, since the few-walled carbon nanotubes can effectively cover the surface of the first lithium composite transition metal oxide, the conductivity of the positive electrode can be effectively improved.
[0071] The average diameter of the few-walled carbon nanotubes can be in the range of 3nm to 7nm, particularly 4nm to 6nm, and more particularly 4.5nm to 5.5nm. When the above range is met, since the transportation and input of the few-walled carbon nanotubes are smooth, the productivity of the positive electrode can be improved, and since the few-walled carbon nanotubes can effectively cover the surface of the first lithium composite transition metal oxide with high specific surface area and low lithium ion diffusion resistance, the conductivity of the positive electrode can be effectively improved. The average diameter means the average value of the diameters of the first 30 few-walled carbon nanotubes and the last 30 few-walled carbon nanotubes with larger diameters in the few-walled carbon nanotubes when the positive electrode active material layer of the prepared positive electrode is examined by a scanning electron microscope (SEM) at a magnification of 10000.
[0072] The average length of the few-walled carbon nanotubes may be in the range of 0.2 μm to 5 μm, particularly 0.5 μm to 3 μm, and more particularly 0.7 μm to 1.5 μm. When the above range is met, even with a small amount, the surface of the positive electrode active material can be effectively covered, and therefore, the conductivity of the positive electrode can be improved. The average length means the average value of the lengths of the first 30 few-walled carbon nanotubes and the last 30 few-walled carbon nanotubes having a larger length among the few-walled carbon nanotubes when the positive electrode active material layer of the prepared positive electrode is examined by SEM at a magnification of 10,000.
[0073] Based on the total weight of the positive electrode active material layer, the few-walled carbon nanotubes may be included in an amount of 0.1 wt % to 3 wt %, particularly 0.2 wt % to 2 wt %, and more particularly 0.3 wt % to 1 wt %, for example 0.45 wt % to 1 wt %. When the above range is met, sufficient conductivity can be achieved, the solid content in the positive electrode slurry can be kept high, so that the amount of the positive electrode active material in the positive electrode active material layer can be increased, and thus excellent capacity characteristics can be achieved.
[0074] 2) Single-walled carbon nanotubes
[0075] The single-walled carbon nanotubes can play a role in electrically connecting the positive electrode active materials to each other in the positive electrode active material layer. The single-walled carbon nanotubes can exist in the positive electrode active material layer strand by strand, or can exist in the form of a small bundle (rope) in which a plurality of single-walled carbon nanotubes are bound side by side.
[0076] The BET specific surface area of single-walled carbon nanotubes can be 800 m 2 / g to 1600m 2 / g, preferably 1000m 2 / g to 1400m 2 / g, and more preferably 1100m 2 / g to 1300m 2 When the above range is satisfied, the conductivity of the positive electrode can be effectively improved even if a small amount of single-walled carbon nanotubes is used.
[0077] The average diameter of the single-walled carbon nanotubes can be in the range of 1 nm to 2.5 nm, particularly 1.3 nm to 2 nm, and more particularly 1.5 nm to 2 nm. When the above range is met, due to the large specific surface area of the single-walled carbon nanotubes, even if the amount of the conductive agent is low, the conductivity of the positive electrode can be effectively improved. The average diameter means the average value of the diameters of the first 30 single-walled carbon nanotubes and the last 30 single-walled carbon nanotubes with larger diameters in the single-walled carbon nanotubes when the positive electrode active material layer of the prepared positive electrode is examined by SEM at a magnification of 10,000.
[0078] The average length of the single-walled carbon nanotubes may be in the range of 0.5 μm to 30 μm, particularly 2 μm to 20 μm, and more particularly 3 μm to 15 μm. When the above range is met, the resistance of the positive electrode can be effectively reduced due to the excellent conductive connection between the positive electrode active materials. In addition, since the connection between the positive electrode active materials can be effectively maintained even when the volume of the positive electrode active materials changes during battery operation, the life characteristics of the battery can be improved. The average length means the average value of the lengths of the first 30 single-walled carbon nanotubes and the last 30 single-walled carbon nanotubes having a larger length in the single-walled carbon nanotubes when the positive electrode active material layer of the prepared positive electrode is examined by SEM at a magnification of 10,000.
[0079] Based on the total weight of the positive electrode active material layer, the single-walled carbon nanotubes may be included in an amount of 0.005 wt % to 0.15 wt %, particularly 0.01 wt % to 0.1 wt %, and more particularly 0.02 wt % to 0.07 wt %. When the above range is met, the initial resistance of the positive electrode can be reduced, and the life characteristics of the battery can be improved. In addition, since the conductivity can be improved even if the amount of the positive electrode active material is low, the energy density of the battery can be increased.
[0080] The weight ratio of the few-walled carbon nanotubes to the single-walled carbon nanotubes may be in the range of 5:1 to 50:1, particularly 7:1 to 40:1, and more particularly 10:1 to 30:1. When the above range is met, since the surface of the positive electrode active material is effectively covered by the few-walled carbon nanotubes, and the single-walled carbon nanotubes can be conductively and effectively connected to the positive electrode active material, a conductive network in the positive electrode can be more effectively formed. Therefore, the resistance of the positive electrode is reduced, and the capacity and life characteristics of the battery can be further improved.
[0081] In the positive electrode active material layer, the total amount of the few-walled carbon nanotubes and the single-walled carbon nanotubes can be in the range of 0.2 wt % to 2.0 wt %, particularly 0.3 wt % to 1.5 wt %, and more particularly 0.4 wt % to 1.0 wt %, based on the total weight of the positive electrode active material layer. When the above range is met, the capacity of the positive electrode can be maintained at a high level while improving the conductivity of the positive electrode. In addition, when the weight ratio range of the few-walled carbon nanotubes to the single-walled carbon nanotubes is met while the above range is met, the resistance reduction of the battery and the improvement of the initial capacity and capacity retention rate can be more effectively achieved.
[0082] (3) Others
[0083] The positive electrode active material layer may further include a binder.
[0084] Binder improves the adhesion between the positive active material particles and the adhesion between the positive active material and the positive current collector. Specific examples of binders can be polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or its various copolymers, and any one of them or a mixture of two or more thereof can be used. Based on the total weight of the positive active material layer, the binder can be included in an amount of 1% to 30% by weight, preferably 1% to 20% by weight, and more preferably 1% to 10% by weight.
[0085] The positive electrode according to the present invention may have an A value defined by the following equation (1) of 3 or more, preferably 3 to 7, and more preferably 4 to 6.
[0086] Equation (1): A = (BET1×W1+BET2×W2) / (BET3×W3+BET4×W4)
[0087] In equation (1), BET1 is the specific surface area of the few-walled carbon nanotubes, BET2 is the specific surface area of the single-walled carbon nanotubes, BET3 is the specific surface area of the first lithium composite transition metal oxide, BET4 is the specific surface area of the second lithium composite transition metal oxide, W1 is the weight % of the few-walled carbon nanotubes relative to the total weight of the positive electrode active material layer, W2 is the weight % of the single-walled carbon nanotubes relative to the total weight of the positive electrode active material layer, W3 is the weight % of the first lithium composite transition metal oxide relative to the total weight of the positive electrode active material layer, and W4 is the weight % of the second lithium composite transition metal oxide relative to the total weight of the positive electrode active material layer. In this case, the unit of the specific surface area is m 2 / g.
[0088] The A value of equation (1) represents the ratio of the total specific surface area of the conductive agent contained in the positive electrode active material layer to the total specific surface area of the positive electrode active material, wherein, since the contact area between the positive electrode active material and the conductive agent increases when the A value is 3 or greater, the effect of improving the resistance characteristics, capacity characteristics and life characteristics of the positive electrode is more excellent.
[0089] The positive electrode can be prepared according to a typical method for preparing a positive electrode. For example, after preparing a positive electrode slurry by mixing a positive electrode active material, a binder, and / or a conductive agent in a solvent and coating the positive electrode slurry on a positive electrode current collector, the positive electrode can be prepared by drying and rolling the coated positive electrode current collector. In this case, the types and amounts of the positive electrode active material, the binder, and the conductive agent are the same as those previously described.
[0090] The solvent may be a commonly used solvent in the art. The solvent may include dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone, or water, and any one thereof or a mixture of two or more thereof may be used. Considering the coating thickness and manufacturing yield of the slurry, if the solvent can dissolve or disperse the positive electrode active material, the conductive agent, and the binder, the amount of the solvent used may be sufficient, and may allow for a viscosity that can provide excellent thickness uniformity during subsequent coating for preparing the positive electrode.
[0091] As another method, the positive electrode may be prepared by casting a positive electrode slurry on a separate support and then laminating a film separated from the support on a positive electrode current collector.
[0092] Secondary battery
[0093] A secondary battery according to another embodiment of the present invention may include the positive electrode of the above embodiment. The secondary battery may be a lithium secondary battery. Specifically, the secondary battery includes a positive electrode, a negative electrode arranged to face the positive electrode, a separator arranged between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is as described above. In addition, the lithium secondary battery may also optionally include a battery container for accommodating an electrode assembly of a positive electrode, a negative electrode and a separator, and a sealing member for sealing the battery container.
[0094] In a lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector.
[0095] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing adverse chemical changes in the battery, and for example, copper; stainless steel; aluminum; nickel; titanium; fired carbon; copper or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc.; and aluminum-cadmium alloys can be used. In addition, the negative electrode current collector may generally have a thickness of 3 μm to 500 μm, and similar to the positive electrode current collector, microscopic irregularities may be formed on the surface of the current collector to improve the adhesion of the negative electrode active material. The negative electrode current collector may be used in various shapes, such as films, sheets, foils, nets, porous bodies, foams, non-woven fabric bodies, and the like.
[0096] The negative electrode active material layer optionally contains a negative electrode binder and a negative electrode conductor in addition to the negative electrode active material.
[0097] A compound capable of reversibly inserting and deinserting lithium can be used as the negative electrode active material. Specific examples of the negative electrode active material may be carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fibers, and amorphous carbon; metal compounds that can be alloyed with lithium, such as silicon (Si), aluminum (Al), tin (Sn), lead (Pb), zinc (Zn), bismuth (Bi), indium (In), magnesium (Mg), gallium (Ga), cadmium (Cd), Si alloys, Sn alloys, or Al alloys; metal oxides that may be doped and undoped with lithium, such as SiO β (0<β<2), SnO2, vanadium oxide, and lithium vanadium oxide; or a composite material comprising a metal compound and a carbon-containing material, such as a Si-C composite material or a Sn-C composite material, and any one of them or a mixture of two or more thereof can be used.
[0098] In addition, a metallic lithium film can be used as a negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon can be used as carbon materials. Typical examples of low-crystalline carbon can be soft carbon and hard carbon, and typical examples of high-crystalline carbon can be irregular, planar, flaky, spherical or fibrous natural graphite or artificial graphite, crystalline graphite (Kishgraphite), pyrolytic carbon, carbon fiber based on mesophase pitch, mesophase carbon microspheres, mesophase pitch, and high-temperature sintered carbon such as coke derived from petroleum or coal tar pitch.
[0099] The negative electrode conductive agent is used to provide conductivity to the electrode, wherein any conductive agent can be used without particular limitation, as long as it has suitable electronic conductivity without causing adverse chemical changes in the battery. Specific examples of negative electrode conductive agents can be: graphite, such as natural graphite or artificial graphite; carbon-based materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal (such as copper, nickel, aluminum and silver) powder or fiber; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives, and any one thereof or a mixture of two or more thereof can be used. Based on the total weight of the negative electrode active material layer, the negative electrode conductive agent can generally be included in an amount of 1% to 30% by weight, preferably 1% to 20% by weight, and more preferably 1% to 10% by weight.
[0100] The negative electrode binder improves the adhesion between the negative electrode active material particles and the adhesion between the negative electrode active material and the negative electrode current collector. Specific examples of the negative electrode binder can be polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or its various copolymers, and any one of them or a mixture of two or more thereof can be used. Based on the total weight of the negative electrode active material layer, the negative electrode binder can be included in an amount of 1% to 30% by weight, preferably 1% to 20% by weight, and more preferably 1% to 10% by weight.
[0101] The negative electrode active material layer can be prepared, for example, by coating a negative electrode slurry containing a negative electrode active material and optionally a negative electrode binder and a negative electrode conductor on a negative electrode collector and drying the coated negative electrode collector, or by casting the negative electrode slurry on a separate support and then laminating a film separated from the support on the negative electrode collector.
[0102] In lithium secondary batteries, separators separate the negative electrode from the positive electrode and provide a path for the movement of lithium ions, wherein any separator can be used as a separator without particular limitation, as long as it is commonly used in lithium secondary batteries, and in particular, separators having high moisture retention capacity for electrolytes and low resistance to the transfer of electrolyte ions can be used. Specifically, porous polymer films can be used, such as porous polymer films prepared by polyolefin-based polymers (such as ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers), or laminated structures having two or more layers thereof. In addition, typical porous nonwoven fabrics can be used, such as nonwoven fabrics formed by high melting point glass fibers or polyethylene terephthalate fibers. In addition, a coated separator comprising a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and a separator with a monolayer or multilayer structure can be optionally used.
[0103] In addition, the electrolyte used in the present invention may include an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, or a molten inorganic electrolyte that can be used to prepare a lithium secondary battery, but the present invention is not limited thereto.
[0104] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0105] Any organic solvent can be used as the organic solvent without particular limitation, as long as it can act as a medium through which ions participating in the electrochemical reaction of the battery can move. Specifically, as the organic solvent, ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone can be used; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; or carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethanol and isopropanol; nitrile such as R-CN (wherein R is a linear, branched or cyclic C2-C20 hydrocarbon group, and may include a double bond aromatic ring or an ether bond); amide such as dimethylformamide; dioxolane such as 1,3-dioxolane; or cyclopentane sulfone. Among these solvents, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant (which can improve the charge / discharge performance of the battery) and a low-viscosity linear carbonate-based compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred.
[0106] Lithium salts can be used without particular limitation, as long as they are compounds that can provide lithium ions used in lithium secondary batteries. Specifically, as lithium salts, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI or LiB(C2O4)2 can be used. Lithium salts can be used in a concentration range of 0.1 M to 5.0 M, preferably 0.1 M to 3.0 M. If the concentration of the lithium salt is included in the above range, since the electrolyte can have appropriate conductivity and viscosity, excellent electrolyte performance can be obtained, and lithium ions can be effectively moved.
[0107] In order to improve the life characteristics of the battery, suppress the reduction of the battery capacity, and improve the discharge capacity of the battery, the electrolyte may further contain additives. For example, as additives, compounds based on halogenated alkylene carbonates (e.g., difluoroethylene carbonate), pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted The additive may be 0.1 wt % to 10 wt %, preferably 0.1 wt % to 5 wt %, based on the total weight of the electrolyte.
[0108] As described above, since the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent capacity characteristics, output characteristics and life characteristics, the lithium secondary battery is suitable for portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEV).
[0109] Therefore, according to another embodiment of the present invention, a battery module including a lithium secondary battery as a unit battery and a battery pack including the battery module are provided.
[0110] The battery module or battery pack can be used as a power source for: at least one of medium and large devices of power tools; electric vehicles, including electric vehicles (EV), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEV); or energy storage systems.
[0111] Embodiments of the invention
[0112] Hereinafter, embodiments of the present invention will be described in detail in a manner that can be easily implemented by those skilled in the art. However, the present invention may be presented in many different forms and should not be construed as being limited to the embodiments set forth herein.
[0113] Example 1
[0114] Using Li[Ni 0.86 Co 0.08 Mn 0.06 ]O2 as the positive electrode active material, Li[Ni 0.86 Co 0.08 Mn 0.06 ]O2 is in the form of a single particle consisting of one primary particle, has a monomodal particle size distribution, and has an average particle size D of 3.7 μm. 50 and 0.7m 2 / g BET specific surface area. The specific surface area used is 400m 2 / g and a few-walled carbon nanotube with a wall number of 5 and a specific surface area of 1200m 2 / g of single-walled carbon nanotubes as a conductive agent. Polyvinylidene fluoride is used as a binder. A positive electrode slurry with a solid content of 70 wt% is prepared by adding a positive electrode active material, a conductive agent and a binder to N-methylpyrrolidone and mixing them. One surface of an aluminum current collector having a width of 340 mm and a thickness of 15 mm is coated with the positive electrode slurry, and then dried and rolled at 130°C to prepare a positive electrode including a positive electrode active material layer.
[0115] In this case, the weight ratio of the positive electrode active material, few-walled carbon nanotubes, single-walled carbon nanotubes and binder in the positive electrode active material layer is 97.37:0.6:0.03:2.0, which is also the same as the amount (weight %) of each component.
[0116] Example 2
[0117] The positive electrode was prepared in the same manner as in Example 1, except that the weight ratio of the positive electrode active material, few-walled carbon nanotubes, single-walled carbon nanotubes and binder in the positive electrode active material layer was changed to 97.37:0.615:0.015:2.0. This is also the same as the amount (weight %) of each component.
[0118] Example 3
[0119] The positive electrode was prepared in the same manner as in Example 1, except that the weight ratio of the positive electrode active material, few-walled carbon nanotubes, single-walled carbon nanotubes and binder in the positive electrode active material layer was changed to 97.685:0.3:0.015:2.0. This is also the same as the amount (weight %) of each component.
[0120] Example 4
[0121] The positive electrode was prepared in the same manner as in Example 1, except that Li[Ni 0.86 Co 0.08 Mn 0.06 ]O2 and Li[Ni 0.92 Co 0.04 Mn 0.02 Al 0.02 ]O2 as the positive electrode active material, Li[Ni 0.86 Co 0.08 Mn 0.06 ]O2 is in the form of a single particle consisting of one primary particle and has an average particle size D of 3.7 μm. 50 and 0.7m 2 / g BET specific surface area, Li[Ni 0.92 Co 0.04 Mn 0.02 Al 0.02 ]O2 is in the form of secondary particles and has an average particle size of 15 μm 50and 0.5m 2 / g BET specific surface area.
[0122] Comparative Example 1
[0123] The positive electrode was prepared in the same manner as in Example 1, except that a positive electrode having a specific surface area of 260 m 2 / g and multi-walled carbon nanotubes with a wall number of 10 have a specific surface area of 400m 2 / g and few-walled carbon nanotubes with a wall number of 5.
[0124] Comparative Example 2
[0125] The positive electrode was prepared in the same manner as in Example 1, except that only the positive electrode having a specific surface area of 400 m 2 / g and 5-walled carbon nanotubes as the conductive agent, instead of single-walled carbon nanotubes. In this case, the weight ratio of the positive electrode active material, the few-walled carbon nanotubes and the binder in the positive electrode active material layer is 97.4:0.6:2.0. This is also the same as the amount (weight %) of each component.
[0126] Comparative Example 3
[0127] The positive electrode was prepared in the same manner as in Example 1, except that only single-walled carbon nanotubes were used as the conductive agent instead of the nanostructured carbon nanotubes having a specific surface area of 400 m 2 / g and a few-walled carbon nanotube with a wall number of 5. In this case, the weight ratio of the positive electrode active material, the single-walled carbon nanotube and the binder in the positive electrode active material layer is 97.97:0.03:2.0. This is also the same as the amount (weight %) of each component.
[0128] Comparative Example 4
[0129] The positive electrode was prepared in the same manner as in Example 1, except that a positive electrode having a specific surface area of 600 m 2 / g and multi-walled carbon nanotubes with a wall number of 10 have a specific surface area of 400m 2 / g and few-walled carbon nanotubes with a wall number of 5, but since the positive electrode slurry composition is extremely difficult to apply due to the excessively high viscosity of the positive electrode slurry composition, it may be impossible to prepare a positive electrode.
[0130] The average diameter and average length of the few-walled carbon nanotubes, single-walled carbon nanotubes, and multi-walled carbon nanotubes were respectively checked by measuring the positive electrodes of the embodiments and comparative examples with a magnification of 10000 using SEM. This corresponds to the average value of the diameter (or length) of the first 30 carbon nanotubes and the last 30 carbon nanotubes.
[0131] 1) Specific surface area is 400m 2 / g of few-walled carbon nanotubes
[0132] Average diameter: 5nm, average length: 1μm
[0133] 2) Single-walled carbon nanotubes
[0134] Average diameter: 1.5nm, average length: 5μm
[0135] 3) Specific surface area is 260m 2 / g multi-walled carbon nanotubes
[0136] Average diameter: 10nm, average length: 1μm
[0137] [Table 1]
[0138]
[0139] Experimental Example 1: Battery Resistance Evaluation
[0140] (1) Preparation of batteries
[0141] A mixture of artificial graphite, natural graphite, and SiO as a negative electrode active material, superC as a conductive agent, and SBR / CMC as a binder were mixed in a weight ratio of 96:1:3 to prepare a negative electrode slurry, and one surface of a copper current collector was coated with the negative electrode slurry, dried at 130° C., and then roll-pressed to prepare a negative electrode.
[0142] The lithium secondary battery is prepared by preparing an electrode assembly by arranging a separator between a positive electrode and a negative electrode, arranging the electrode assembly in a battery box, and then injecting an electrolyte solution into the box. The electrolyte solution is prepared by dissolving 1M LiPF6 in a mixed organic solvent in which ethylene carbonate / dimethyl carbonate / diethyl carbonate are mixed in a volume ratio of 1:2:1 and adding 2 wt % of vinylene carbonate (VC).
[0143] (2) Battery resistance evaluation
[0144] After charging and discharging the battery three times at a 0.3C rate at room temperature, the battery resistance was evaluated by checking the resistance value when a current was applied at a 2.5C rate for 10 seconds at a state of charge (SOC) of 50. The measurement results are shown in Table 2 below.
[0145] Experimental Example 2: Evaluation of initial discharge capacity and capacity retention rate
[0146] After each of the lithium secondary batteries prepared in Experimental Example 1 was charged to 4.25V at 1C in a constant current-constant voltage (CC-CV) mode at 45°C and each lithium secondary battery was discharged to 2.5V at a constant current of 0.5C as one cycle and 200 charge and discharge cycles were performed, the initial discharge capacity and the capacity retention rate were measured to evaluate the life characteristics. The measurement results are shown in Table 2 below.
[0147] [Table 2]
[0148]
Claims
1. A positive electrode comprising a positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode active material and a conductive agent, wherein the positive electrode active material includes a first lithium composite transition metal oxide in a single particle form consisting of one primary particle or in a pseudo-single particle form as an aggregate of 10 or less primary particles, and The conductive agent includes few-walled carbon nanotubes and single-walled carbon nanotubes. The number of walls of the few-walled carbon nanotubes is in the range of 2 to 7. 2 . The positive electrode according to claim 1 , wherein the average diameter of the few-walled carbon nanotubes is 3 nm to 7 nm.
3. The positive electrode according to claim 1, wherein the Brunauer-Emmett-Teller (BET) specific surface area of the few-walled carbon nanotubes is 300 m 2 / g to 500m 2 / g.
4. The positive electrode according to claim 1, wherein the first lithium composite transition metal oxide comprises a compound represented by [Formula 1], [Formula 1] Li a1 [Ni b1 Co c1 M 1 d1 M 2 e1 ]O2 in, In Formula 1, M 1 is at least one selected from manganese (Mn) and aluminum (Al), and M 2 is at least one selected from zirconium (Zr), tungsten (W), yttrium (Y), barium (Ba), calcium (Ca), titanium (Ti), magnesium (Mg), tantalum (Ta), and niobium (Nb), and 0.8 ≤ a1 ≤ 1.2, 0.8 ≤ b1 < 1, 0 < c1 < 0.2, 0 < d1 < 0.2, and 0 ≤ e1 ≤ 0.
1. 5 . The positive electrode according to claim 1 , wherein an average particle diameter of the primary particles contained in the first lithium composite transition metal oxide is in the range of 1 μm to 10 μm.
6. The positive electrode according to claim 1, wherein the BET specific surface area of the first lithium composite transition metal oxide is 0.1 m 2 / g to 3m 2 / g. 7 . The positive electrode according to claim 1 , wherein the few-walled carbon nanotubes are contained in an amount of 0.1 wt % to 3 wt % based on the total weight of the positive electrode active material layer.
8. The positive electrode according to claim 1, wherein the BET specific surface area of the single-walled carbon nanotube is 800 m 2 / g to 1600m 2 / g. 9 . The positive electrode according to claim 1 , wherein the single-walled carbon nanotube is included in an amount of 0.005 wt % to 0.15 wt % based on the total weight of the positive electrode active material layer. 10 . The cathode according to claim 1 , wherein a weight ratio of the few-walled carbon nanotubes to the single-walled carbon nanotubes is in a range of 5:1 to 50:
1. 11 . The cathode according to claim 1 , wherein a weight ratio of the few-walled carbon nanotubes to the single-walled carbon nanotubes is in a range of 10:1 to 30:
1.
12. The positive electrode according to claim 1, wherein In the positive electrode active material layer, The total amount of the few-walled carbon nanotubes and the single-walled carbon nanotubes is in a range of 0.2 wt % to 2.0 wt % based on the total weight of the positive electrode active material layer.
13. The positive electrode according to claim 1, wherein the positive electrode active material comprises a second lithium composite transition metal oxide, The average particle size of the second lithium composite transition metal oxide is D 50 10μm to 20μm.
14. The positive electrode according to claim 13, wherein the second lithium composite transition metal oxide comprises a compound represented by [Formula 2], [Formula 2] Li a2 [Ni b2 Co c2 M 3 d2 M 4 e2 ]O2 in, In Formula 2, M 3 is at least one selected from Mn and Al, and M 4 is at least one selected from Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb, and 0.8 ≤ a2 ≤ 1.2, 0.8 ≤ b2 < 1, 0 < c2 < 0.17, 0 < d < 0.17, and 0 ≤ e2 ≤ 0.
1.
15. The positive electrode according to claim 1, wherein the positive electrode has an A value defined by equation (1) of 3 or more, Equation (1): A = (BET1×W1+BET2×W2) / (BET3×W3+BET4×W4) in, In equation (1), BET1 is the specific surface area of the few-walled carbon nanotubes, BET2 is the specific surface area of the single-walled carbon nanotubes, BET3 is the specific surface area of the first lithium composite transition metal oxide, BET4 is the specific surface area of the second lithium composite transition metal oxide, W1 is the weight % of the few-walled carbon nanotubes relative to the total weight of the positive electrode active material layer, W2 is the weight % of the single-walled carbon nanotubes relative to the total weight of the positive electrode active material layer, W3 is the weight % of the first lithium composite transition metal oxide relative to the total weight of the positive electrode active material layer, and W4 is the weight % of the second lithium composite transition metal oxide relative to the total weight of the positive electrode active material layer. 16 . A secondary battery comprising the positive electrode according to claim 1 .