Novel sunscreen material with ultraviolet ray and near infrared ray double-blocking effect as well as preparation method and application of novel sunscreen material
By covering the porous structure of the titanium dioxide shell and the second shell of the tanninic acid derivative on the gold nanorod, double barriers to ultraviolet and near-infrared are achieved, and the problem of difficulty in blocking sunscreen materials in the prior art is solved. , improves sun protection effect and antioxidant ability.
Patent Information
- Application Number
- CN202411119570.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-31
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
Existing sunscreen materials are difficult to block ultraviolet rays (UVA/UVB) and near-infrared (NIR) at the same time, and commonly used inorganic sunscreen agents such as TiO2 and ZnO are not effective in blocking near-infrared rays, and it is difficult to improve the sunscreen effect.
New sun protection materials with multi-layered cladding structures, including gold nanorods, titanium dioxide shells coated on gold nanorods, and a second shell of tannin or its derivatives, through the specific aspect ratio of gold nanorods and the porous structure of the shell, achieving effective absorption and scattering of ultraviolet and near-infrared rays.
The dual barrier ability of ultraviolet and near-infrared rays is achieved, the antioxidant effect is enhanced, the reactive oxygen species is eliminated, and the sun protection performance is improved. In particular, the barrier ability of conventional inorganic sunscreen agents is significantly improved under a smaller amount of addition.
Smart Images

Figure CN119015139A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of daily chemical products, and in particular to a novel sunscreen material with dual ultraviolet and near infrared blocking effects, and a preparation method and application thereof. Background Art
[0002] The sun can provide heat and energy for human life, but it can also have acute and chronic adverse effects on human skin. Due to the protection of the atmosphere, the sunlight reaching the earth's surface contains about 5% ultraviolet light (UV), 50% visible light (VL) and 45% infrared light (IR). The ultraviolet rays reaching the earth contain about 10% medium-wave ultraviolet rays (UVB 290-320nm) and 90% long-wave ultraviolet rays (UVA 320-400nm). UVB is mainly absorbed by the epidermis, causing inflammatory reactions of sunburn and directly damaging DNA; UVA can penetrate into the dermis and induce DNA damage through the production of melanin and its byproduct reactive oxygen species (ROS), causing oxidative damage and photoaging. Infrared rays can be divided into near-infrared region (IR-A, 700-1400nm), mid-infrared region (IR-B, 1400-3000nm) and far-infrared region (IR-C, 3000nm-1mm) according to their wavelength. Water molecules in the earth's atmosphere have a significant impact on the intensity of IR reaching the earth's surface. Water molecules have a certain absorption of IR-B and IR-C, which greatly reduces the radiation intensity when they reach the earth's surface. In contrast, due to the principles of quantum physics, the IR-A radiation with higher energy is less likely to be absorbed through the vibration mode of water molecules. The above phenomenon also applies to the human body. The water content of the skin accounts for about 18%-20% of the total water content of the human body. The vibration mode of water molecules in the skin prevents IR-B and IR-C radiation from penetrating the skin, but more than 65% of IR-A radiation can reach the dermis and subcutaneous tissue. Skin exposed to IR-A radiation for a long time may cause thermal stress due to increased skin temperature, produce reactive oxygen and trigger the production of matrix metalloproteinases (MMPs), change colloid balance, cause collagen degradation, etc., thereby damaging the skin and causing thermal aging. In addition, repeated exposure to IR-A radiation will not only reduce the thickness of the epidermal cell layer of human skin, but also increase the thickness of the stratum corneum, which also indicates that repeated exposure to IR-A may cause skin aging. Therefore, if you want to reduce the negative impact of sunlight radiation on the skin, you need to consider blocking both ultraviolet rays (UVA / UVB) and near infrared rays (NIR). However, little is known about the physical and chemical blocking methods of near infrared rays. The principle of protecting the skin from damage by near infrared rays is also different from that of ultraviolet rays. It is difficult to produce the same effect using inorganic sunscreens such as TiO2, ZnO or organic sunscreens commonly used in sunscreen cosmetics. At the same time, the sunscreen effect needs to be improved. Summary of the invention
[0003] The object of the present invention is to overcome one or more deficiencies in the prior art and to provide a new type of sunscreen material with dual ultraviolet and near infrared blocking effects, which has good sunscreen effects. For example, it can simultaneously block ultraviolet rays (UVA / UVB) and near infrared rays (NIR), remove reactive oxygen species (ROS) and enhance the antioxidant effect.
[0004] The present invention also provides a method for preparing the novel sunscreen material having dual ultraviolet and near infrared blocking effects, and its application in preparing sunscreen compositions and cosmetics.
[0005] In order to achieve the above object, a technical solution adopted by the present invention is:
[0006] A sunscreen material comprises gold nanorods, a first shell layer coated on the gold nanorods and a second shell layer coated on the first shell layer, wherein the material of the first shell layer comprises titanium dioxide, and the material of the second shell layer comprises tannic acid or its derivatives.
[0007] According to some preferred aspects of the present invention, the aspect ratio of the gold nanorods is 3-10. Under this aspect ratio, the gold nanorods can better absorb infrared rays with a wavelength of 700-1400 nm.
[0008] In some specific embodiments of the present invention, the first shell layer is a titanium dioxide shell.
[0009] According to some preferred aspects of the present invention, the first shell layer has a porous structure, which is more conducive to significant absorption and scattering in the ultraviolet region.
[0010] In some embodiments, in addition to the coating-coated relationship, the second shell layer and the first shell layer may be connected by chemical bonds due to the surface functionalization and etching effects of tannic acid, and the chemical bonds include covalent bonds, coordination bonds, etc.
[0011] According to some preferred aspects of the present invention, the preparation of the first shell layer satisfies the following conditions:
[0012] (1) using the gold nanorods and the first shell layer precursor as raw materials, respectively, wherein the first shell layer precursor refers to a substance that can generate the first shell layer through one or more steps of conversion treatment;
[0013] (2) The one-step or multi-step conversion treatment includes a precipitation treatment in the presence of a precipitant, and a calcination treatment.
[0014] Furthermore, the first shell layer precursor includes titanium halide, which may be titanium tetrachloride, titanium tetrabromide, etc. In some other embodiments, the first shell layer may include titanium dioxide as the main material and other inorganic materials with sunscreen effects such as zinc oxide as auxiliary materials.
[0015] Furthermore, the precipitant includes carbonate and / or bicarbonate. Carbonate and / or bicarbonate can be precipitated on the gold nanorods to obtain carbonate precipitate, which is coated on the gold nanorods and then calcined to convert the carbonate precipitate into a sunscreen substance in the form of a corresponding oxide, such as titanium dioxide. In addition, the first shell material in the form of a precursor is subjected to one or more steps of conversion treatment to prepare the coating structure, so that the first shell can be uniformly coated on the gold nanorods.
[0016] According to some preferred aspects of the present invention, in the sunscreen material, the total mass of the gold nanorods and the first shell layer accounts for 90%-99%, and the second shell layer accounts for 1%-10%. Further, in the sunscreen material, the total mass of the gold nanorods and the first shell layer accounts for 94%-97%, and the second shell layer accounts for 3%-6%.
[0017] According to some preferred aspects of the present invention, the mass ratio of the gold nanorods to the first shell layer is 1:0.8-4.1.
[0018] Another technical solution provided by the present invention is a method for preparing the sunscreen material described above, the method for preparing the sunscreen material comprising:
[0019] Dispersing the gold nanorods and the first shell precursor in a solvent, adding a precipitant capable of reacting with the first shell precursor to generate a first intermediate, and calcining the first intermediate to obtain a second intermediate;
[0020] The second intermediate and the material of the second shell layer are mixed and stirred to obtain the sunscreen material.
[0021] In some embodiments of the present invention, the method for preparing the gold nanorods comprises:
[0022] In the presence of a first surfactant, a gold precursor is reacted with a reducing agent to generate gold nanoparticles;
[0023] mixing a second surfactant, a gold precursor, silver nitrate and ascorbic acid to prepare a growth solution;
[0024] The gold nanoparticles are added into the growth solution to react and generate gold nanorods.
[0025] Furthermore, the first surfactant may be cetyltrimethylammonium bromide (CTAB) or the like.
[0026] Furthermore, the gold precursor may be a gold halide acid, and the gold halide acid may be tetrachloroauric acid (HAuCl4), tetrabromoauric acid, or the like.
[0027] Furthermore, the reducing agent may be sodium borohydride (NaBH4) or the like.
[0028] According to some specific embodiments of the present invention, the method for preparing gold nanoparticles includes: mixing an aqueous solution of a first surfactant (the concentration may be 0.001-0.5 mol / L, for example, 0.005-0.2 mol / L) and an aqueous solution of a gold precursor (the concentration may be 0.0001-0.2 mol / L, for example, 0.0005-0.05 mol / L), and then adding a low temperature (for example, 0-10°C, further 0-5°C) sodium borohydride aqueous solution (the concentration may be 0.001-0.2 mol / L, for example, 0.005-0.1 mol / L), reacting to generate gold nanoparticles.
[0029] In some embodiments, the average particle size of the gold nanoparticles is about 3-5 nm.
[0030] In some embodiments, the molar ratio of the first surfactant to the gold precursor is 1-100:1, further 20-80:1.
[0031] In some embodiments, the molar ratio of the gold precursor to the reducing agent is 1:0.1-10, for example, 1:1-8, or 1:1-5.
[0032] Further, the second surfactant is composed of hexadecyltrimethylammonium bromide (CTAB) and benzylhexadecylammonium chloride (BDAC). In some embodiments, the molar ratio of the benzylhexadecylammonium chloride (BDAC) to the hexadecyltrimethylammonium bromide (CTAB) is 0.01-10:1, for example, 0.02-8:1, or 0.05-5:1, or 0.07-3:1.
[0033] In the present invention, silver nitrate can catalyze the growth of gold nanorods, and ascorbic acid can play a reducing role, for example, reducing gold particles to gold element.
[0034] Furthermore, in the process of preparing the growth solution, the molar ratio of the gold precursor, the silver nitrate and the ascorbic acid is 1:0.005-5:0.005-3, for example, it can be 1:0.005-2:0.005-2, or 1:0.08-1:0.08-1.5, or 1:0.08-0.3:0.09-0.3.
[0035] Furthermore, in the process of preparing the growth solution, the molar ratio of the gold precursor to the second surfactant is 1:10-200, for example, 1:30-180, or 1:50-150.
[0036] In some embodiments of the present invention, the method for preparing the growth solution includes: adding hexadecyltrimethylammonium bromide (CTAB) and benzylhexadecylammonium chloride (BDAC) into a container respectively, stirring and dissolving at 25-40° C., and then adding a gold precursor, silver nitrate and ascorbic acid respectively, mixing, to obtain the growth solution.
[0037] Furthermore, in the process of preparing the gold nanorods, the gold nanoparticles are added in the form of a gold nanoseed solution.
[0038] Furthermore, in the process of preparing the gold nanorods, after the gold nanoseeds are added to the growth solution, when the color of the solution changes from brown to transparent, it means the growth of the gold nanorods (GNRs). Depending on the ratio of BDAC / CTAB, the color changes for a short period of several minutes or up to 10 minutes, a long period of several hours, or about 10 hours or even longer. The longer the time required for the color change, the greater the aspect ratio of the gold nanorods (GNRs).
[0039] In some embodiments of the present invention, the preparation method of the second intermediate comprises: dispersing the first shell precursor in an aqueous solution of gold nanorods, adding an aqueous solution of a precipitant under stirring conditions until the pH value reaches 7.5-9.0, continuing stirring, separating the precipitate, i.e., the first intermediate, and then calcining to obtain the second intermediate.
[0040] In some embodiments of the present invention, the calcination is controlled to be carried out at 200-700°C, further 300-500°C.
[0041] In some embodiments of the present invention, the calcination time is controlled to be 5-20 hours, further 8-16 hours.
[0042] According to a specific aspect of the present invention, the preparation method of the second intermediate comprises: adding titanium tetrachloride to an aqueous solution of gold nanorods, adding an aqueous solution of carbonate and / or bicarbonate under stirring conditions until the pH value reaches 7.5-9.0, continuing stirring, separating a carbonate precipitate, i.e., the first intermediate, and then calcining to obtain the second intermediate.
[0043] In some embodiments of the present invention, the molar ratio of the first shell layer precursor to the gold nanorods is 2-10:1, for example, 2-6:1, or 2-4:1.
[0044] In some embodiments of the present invention, the method for preparing the sunscreen material comprises: adding the second intermediate to an aqueous solution of tannic acid, mixing and dispersing (the temperature can be controlled to be 20-40° C.), centrifuging, and washing to obtain the sunscreen material.
[0045] Another technical solution provided by the present invention is a blocking agent having dual blocking effects of ultraviolet rays and near-infrared rays, which comprises the sunscreen material mentioned above, water and a selective alcohol substance.
[0046] Furthermore, the alcohol substance includes but is not limited to 1,2-hexanediol and the like.
[0047] Furthermore, in the blocking agent, the above-mentioned sunscreen material accounts for 0.001%-5%, alcohol substances account for 0.5%-5%, and water accounts for 90%-99%, calculated by mass percentage.
[0048] Furthermore, in terms of mass percentage, in the blocking agent, the above-mentioned sunscreen material accounts for 0.001%-2%, alcohol substances account for 0.8%-4%, and water accounts for 94%-99%.
[0049] In some embodiments of the present invention, in the blocking agent, the sunscreen material mentioned above accounts for 0.001%-0.5%, alcohols account for 1.5%-4%, and water accounts for 95.5%-98.4%, calculated by weight percentage.
[0050] According to some specific aspects of the present invention, in the blocking agent, the sunscreen material mentioned above accounts for 0.001%-0.1%, alcohols account for 1.5%-4%, and water accounts for 95.9%-98.4%, calculated by mass percentage.
[0051] Another technical solution provided by the present invention is a sunscreen composition, which includes nano titanium dioxide and / or nano zinc oxide, and the above-mentioned sunscreen material or the above-mentioned blocking agent with dual ultraviolet and near-infrared blocking effects.
[0052] Furthermore, the sunscreen composition is composed of nano titanium dioxide, nano zinc oxide and the above-mentioned blocking agent.
[0053] Furthermore, the nano titanium dioxide is added by pre-treated nano titanium dioxide, and the pre-treated nano titanium dioxide is obtained by coating nano titanium dioxide with aluminum hydroxide and / or stearic acid. In some embodiments, nano titanium dioxide is coated with aluminum hydroxide and stearic acid, and the mass ratio of the aluminum hydroxide, the stearic acid and the nano titanium dioxide is 70-86:6-16:6-16, and the total amount of the three is 100 parts.
[0054] Furthermore, the nano zinc oxide is added by pre-treated nano zinc oxide, and the pre-treated nano zinc oxide is obtained by coating with silane such as triethoxyoctylsilane, polydimethylsiloxane, dimethoxydiphenylsilane / triethoxyoctylsilane cross-linked copolymer, etc. In some embodiments, the mass ratio of the silane to the nano zinc oxide is 90-98:2-10, and the total amount of the two is 100 parts.
[0055] Furthermore, the particle size of the nano titanium dioxide may be 10-15 nm, and it is spindle-shaped and has a rutile crystal structure.
[0056] Furthermore, the particle size of the nano zinc oxide can be 20-40 nm, and it has an isometric shape and a wurtzite crystal structure.
[0057] Furthermore, the mass ratio of the nano titanium dioxide, the nano zinc oxide and the blocking agent is 1:1.1-3:0.01-2.
[0058] Another technical solution provided by the present invention is: use of the sunscreen material described above, or the blocking agent described above with dual ultraviolet and near-infrared blocking effects, or the sunscreen composition described above in cosmetics.
[0059] Another technical solution provided by the present invention is a sunscreen cosmetic comprising a solvent, an emollient, a humectant, a suspending agent, a dispersing agent, a skin feel regulator, an emulsifying stabilizer, and nano titanium dioxide, nano zinc oxide and the above-mentioned blocking agent.
[0060] Furthermore, the solvent includes water, siloxane (for example, one or both of cyclopentasiloxane and methyl trimethicone), and butylene glycol dicaprylate / dicaprate.
[0061] Furthermore, the emollient includes glyceryl caprylate, caprylyl glycol, ethylhexylglycerin and the like.
[0062] Furthermore, the moisturizing agent includes butylene glycol and the like.
[0063] Furthermore, the suspending agent includes disteardimethylammonium hectorite and the like.
[0064] Furthermore, the dispersant includes polyglycerol-6 polyricinoleate and the like.
[0065] Furthermore, the skin feel regulator includes methyl methacrylate cross-linked polymer and the like.
[0066] Furthermore, the emulsion stabilizer includes magnesium sulfate and the like.
[0067] Furthermore, the sunscreen cosmetics also contain preservatives, etc., and the preservatives include 1,2-hexanediol, etc.
[0068] In some embodiments of the present invention, the sunscreen cosmetic is a sunscreen, which comprises phase A, phase B, phase C, phase D and phase E;
[0069] Wherein, phase A includes cyclopentasiloxane and disteardimethylammonium hectorite;
[0070] Phase B includes Butylene Glycol Dicaprylate / Dicaprate, Glyceryl Caprylate, and Caprylyl Glycol;
[0071] Phase C includes PEG-10 dimethicone, polyglyceryl-6 polyricinoleate, ethylhexylglycerin, and methyl trimethicone;
[0072] Phase D includes pretreated nano titanium dioxide, pretreated nano zinc oxide and methyl methacrylate cross-linked polymer;
[0073] Phase E includes water, butylene glycol, magnesium sulfate, 1,2-hexanediol, and a blocking agent having dual blocking effects of ultraviolet rays and near infrared rays.
[0074] Furthermore, in terms of mass percentage, in the sunscreen:
[0075]
[0076]
[0077] Furthermore, in some embodiments of the present invention, the method for preparing the sunscreen comprises:
[0078] (1) After measuring the raw materials of phase B, heat to 45-55°C, mix and stir evenly, then cool to 25-35°C;
[0079] (2) The raw materials of phase C and phase D are measured and put into the phase B container in sequence;
[0080] (3) Disperse the raw materials of phase A separately and put them into the container of phase B and stir evenly;
[0081] (4) separately measuring and evenly dispersing the raw materials of phase E;
[0082] (5) Pre-dispersing the AD phase mixture at room temperature, slowly adding the E phase for emulsification;
[0083] (6) Degassing and filtering.
[0084] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0085] Based on the problem that existing sunscreen materials are difficult to block ultraviolet rays (UVA / UVB) and near infrared rays (NIR) at the same time, the present invention innovatively provides a new type of sunscreen material with dual ultraviolet and near infrared blocking effects. The sunscreen material is a multi-layer coating structure, based on gold nanorods, which are sequentially coated with a first shell layer containing titanium dioxide and a second shell layer containing tannic acid or its derivatives. It is found in practice that the sunscreen material can simultaneously have excellent ultraviolet (UVA / UVB) and near infrared (NIR) blocking capabilities, especially can enhance the ultraviolet (UVA / UVB) blocking capabilities of conventional inorganic sunscreens such as TiO2 and ZnO on the basis of a relatively small amount of addition. In addition, it also has a good antioxidant effect, such as the ability to scavenge reactive oxygen species (ROS) and free radicals. BRIEF DESCRIPTION OF THE DRAWINGS
[0086] Figure 1 This is a transmission electron microscopy image of the titanium dioxide@gold nanorod core-shell composite (GNR@TiO2) prepared in Example 1 of the present invention;
[0087] Figure 2 This is the energy spectrum of the titanium dioxide@gold nanorod core-shell composite (GNR@TiO2) prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0088] The above scheme is further described below in conjunction with specific embodiments; it should be understood that these embodiments are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following embodiments; the implementation conditions adopted in the embodiments can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in conventional experiments.
[0089] In the following examples and comparative examples, "a M" means the molar amount per liter is a, for example, "1 M" means the molar content is 1 mol / L. In the following examples and comparative examples, unless otherwise specified, the raw materials are commercially available or prepared by conventional methods in the art.
[0090] Example 1
[0091] This example provides a sunscreen material and a preparation method thereof, the preparation method of the sunscreen material comprising:
[0092] 1. Preparation of Gold Nanorods (GNRs)
[0093] (1) Gold seed synthesis
[0094] 5 mL of 0.02 M hexadecyltrimethylammonium bromide (CTAB) aqueous solution and 5 mL of 0.0005 M HAuCl4 aqueous solution were placed in a vial and vortexed vigorously for about 1 minute; thereafter, 900 μL of 0.01 M NaBH4 aqueous solution at about 3°C was added as a reducing agent and vortexed for 3 minutes. As a result, the color of the solution was brown, and gold nanoparticles of about 3 to 5 nm were formed, forming gold seeds.
[0095] (2) Synthesis of growth solution
[0096] 50 mL of 0.15 M CTAB aqueous solution and 50 mL of 0.0495 M benzyl hexadecyl ammonium chloride (BDAC) aqueous solution were added to a 250 mL conical flask, respectively, so that the molar ratio of BDAC / CTAB was 0.33:1. The conical flask was placed in a prepared water bath, the temperature was maintained at 30°C and stirred to completely dissolve CTAB and BDAC. 100 mL of 0.001 M HAuCl4 aqueous solution, 2.4 mL of 0.004 M AgNO3 aqueous solution and 1.4 mL of 0.00788 M ascorbic acid aqueous solution were added to the conical flask, mixed well, and a growth solution was prepared. The color of the solution became transparent due to the reducing effect of ascorbic acid.
[0097] (3) Synthesis of gold nanorods
[0098] 240 μL of the gold seeds prepared according to step (1) were added to the growth solution prepared according to step (2). When the color of the solution changed from transparent to wine red, it meant the growth of gold nanorods (GNR). After the color change, the solution was stirred for more than 12 hours to complete the crystal growth reaction of gold nanorods (GNR). After the reaction, the solution was centrifuged at 15000 rpm for 30 minutes, washed with distilled water for about 2 times, and then dispersed in distilled water. Among them, the aspect ratio of the gold nanorods was measured to be about 4.
[0099] 2. Preparation of Titanium Dioxide@Gold Nanorod Core-Shell Composite (GNR@TiO2)
[0100] 3 mol TiCl4 was slowly dripped into 1000 mL 1M GNR aqueous solution, and the solution was stirred continuously. A 5% NaHCO3 aqueous solution was added to adjust the pH value to about 8.0, and the solution was stirred for 2 h and allowed to stand at low temperature for 12 h. The obtained hydrolysis precipitate (i.e., the first intermediate) was filtered, washed, dried in a thermostat at 80 ° C for 6 h, and then moved into a muffle furnace and calcined at 400 ° C for 12 h to obtain a titanium dioxide @ gold nanorod core-shell complex (GNR@TiO2), i.e., the second intermediate.
[0101] See also Figure 1 As shown, it is a transmission electron microscopy image of the titanium dioxide @ gold nanorod core-shell composite (GNR@TiO2) prepared in this example. Figure 2 is its energy spectrum; Figure 1-Figure 2 It can be seen that titanium dioxide is successfully coated on the gold nanorods.
[0102] 3. Preparation of sunscreen material (TA-GNR@TiO2)
[0103] 2.2g of titanium dioxide@gold nanorod core-shell composite (GNR@TiO2) was put into an aqueous solution containing 0.1g of TA (tannic acid, also known as tannic acid), and placed in a 25°C water bath constant temperature oscillator (vibration frequency of 450r / min) for 1h. Centrifuged and washed twice with deionized water to obtain a sunscreen material (TA-GNR@TiO2).
[0104] Example 2
[0105] This example provides a sunscreen material and a preparation method thereof, the preparation method of the sunscreen material comprising:
[0106] 1. Preparation of Gold Nanorods (GNRs)
[0107] (1) Gold seed synthesis
[0108] 5 mL of 0.02 M hexadecyltrimethylammonium bromide (CTAB) aqueous solution and 5 mL of 0.0005 M HAuCl4 aqueous solution were placed in a vial and vortexed vigorously for about 1 minute; thereafter, 900 μL of 0.01 M NaBH4 aqueous solution at about 3°C was added as a reducing agent and vortexed for 3 minutes. As a result, the color of the solution was brown, and gold nanoparticles of about 3 to 5 nm were formed, forming gold seeds.
[0109] (2) Synthesis of growth solution
[0110] 50 mL of 0.15 M CTAB aqueous solution and 50 mL of 0.0105 M benzyl hexadecyl ammonium chloride (BDAC) aqueous solution were added to a 250 mL conical flask, respectively, so that the molar ratio of BDAC / CTAB was 0.07:1. The conical flask was placed in a prepared water bath, the temperature was maintained at 30°C and stirred to completely dissolve CTAB and BDAC. 100 mL of 0.001 M HAuCl4 aqueous solution, 2.4 mL of 0.004 M AgNO3 aqueous solution and 1.4 mL of 0.00788 M ascorbic acid aqueous solution were added to the above conical flask, mixed well, and a growth solution was prepared. The color of the solution became transparent due to the reduction effect of ascorbic acid.
[0111] (3) Synthesis of gold nanorods
[0112] 240 μL of the gold seeds prepared according to step (1) were added to the growth solution prepared according to step (2). When the color of the solution changed from transparent to wine red, it meant the growth of gold nanorods (GNR). After the color change, the solution was stirred for more than 12 hours to complete the crystal growth reaction of gold nanorods (GNR). After the reaction, the solution was centrifuged at 15000 rpm for 30 minutes, washed with distilled water for about 2 times, and then dispersed in distilled water. Among them, the aspect ratio of the gold nanorods was measured to be about 3.
[0113] 2. Preparation of Titanium Dioxide@Gold Nanorod Core-Shell Composite (GNR@TiO2)
[0114] 3 mol TiCl4 was slowly dripped into 1000 mL 1M GNR aqueous solution, and the solution was stirred continuously. A 5% NaHCO3 aqueous solution was added to adjust the pH value to about 8.0, and the solution was stirred for 2 h and allowed to stand at low temperature for 12 h. The obtained hydrolysis precipitate (i.e., the first intermediate) was filtered, washed, dried in a thermostat at 80 ° C for 6 h, and then moved into a muffle furnace and calcined at 400 ° C for 12 h to obtain a titanium dioxide @ gold nanorod core-shell complex (GNR@TiO2), i.e., the second intermediate.
[0115] 3. Preparation of sunscreen material (TA-GNR@TiO2)
[0116] 2.2g of titanium dioxide@gold nanorod core-shell composite (GNR@TiO2) was put into an aqueous solution containing 0.1g of TA (tannic acid, also known as tannic acid), and placed in a 25°C water bath constant temperature oscillator (vibration frequency of 450r / min) for 1h. Centrifuged and washed twice with deionized water to obtain a sunscreen material (TA-GNR@TiO2).
[0117] Example 3
[0118] This example provides a sunscreen material and a preparation method thereof, the preparation method of the sunscreen material comprising:
[0119] 1. Preparation of Gold Nanorods (GNRs)
[0120] (1) Gold seed synthesis
[0121] 5 mL of 0.02 M hexadecyltrimethylammonium bromide (CTAB) aqueous solution and 5 mL of 0.0005 M HAuCl4 aqueous solution were placed in a vial and vortexed vigorously for about 1 minute; thereafter, 900 μL of 0.01 M NaBH4 aqueous solution at about 3°C was added as a reducing agent and vortexed for 3 minutes. As a result, the color of the solution was brown, and gold nanoparticles of about 3 to 5 nm were formed, forming gold seeds.
[0122] (2) Synthesis of growth solution
[0123] 50 mL of 0.15 M CTAB aqueous solution and 50 mL of 0.1005 M benzyl hexadecyl ammonium chloride (BDAC) aqueous solution were added to a 250 mL conical flask, respectively, so that the molar ratio of BDAC / CTAB was 0.67:1. The conical flask was placed in a prepared water bath, the temperature was maintained at 30°C and stirred to completely dissolve CTAB and BDAC. 100 mL of 0.001 M HAuCl4 aqueous solution, 2.4 mL of 0.004 M AgNO3 aqueous solution and 1.4 mL of 0.00788 M ascorbic acid aqueous solution were added to the conical flask, mixed well, and a growth solution was prepared. The color of the solution became transparent due to the reduction of ascorbic acid.
[0124] (3) Synthesis of gold nanorods
[0125] 240 μL of the gold seeds prepared according to step (1) were added to the growth solution prepared according to step (2). When the color of the solution changed from transparent to wine red, it meant the growth of gold nanorods (GNR). After the color change, the solution was stirred for more than 12 hours to complete the crystal growth reaction of gold nanorods (GNR). After the reaction, the solution was centrifuged at 15000 rpm for 30 minutes, washed with distilled water for about 2 times, and then dispersed in distilled water. Among them, the aspect ratio of the gold nanorods was measured to be about 5.
[0126] 2. Preparation of Titanium Dioxide@Gold Nanorod Core-Shell Composite (GNR@TiO2)
[0127] 3 mol TiCl4 was slowly dripped into 1000 mL 1M GNR aqueous solution, and the solution was stirred continuously. A 5% NaHCO3 aqueous solution was added to adjust the pH value to about 8.0, and the solution was stirred for 2 h and allowed to stand at low temperature for 12 h. The obtained hydrolysis precipitate (i.e., the first intermediate) was filtered, washed, dried in a thermostat at 80 ° C for 6 h, and then moved into a muffle furnace and calcined at 400 ° C for 12 h to obtain a titanium dioxide @ gold nanorod core-shell complex (GNR@TiO2), i.e., the second intermediate.
[0128] 3. Preparation of sunscreen material (TA-GNR@TiO2)
[0129] 2.2g of titanium dioxide@gold nanorod core-shell composite (GNR@TiO2) was put into an aqueous solution containing 0.1g of TA (tannic acid, also known as tannic acid), and placed in a 25°C water bath constant temperature oscillator (vibration frequency of 450r / min) for 1h. Centrifuged and washed twice with deionized water to obtain a sunscreen material (TA-GNR@TiO2).
[0130] Example 4
[0131] This example provides a sunscreen material and a preparation method thereof, the preparation method of the sunscreen material comprising:
[0132] 1. Preparation of Gold Nanorods (GNRs)
[0133] (1) Gold seed synthesis
[0134] 5 mL of 0.02 M hexadecyltrimethylammonium bromide (CTAB) aqueous solution and 5 mL of 0.0005 M HAuCl4 aqueous solution were placed in a vial and vortexed vigorously for about 1 minute; thereafter, 900 μL of 0.01 M NaBH4 aqueous solution at about 3°C was added as a reducing agent and vortexed for 3 minutes. As a result, the color of the solution was brown, and gold nanoparticles of about 3 to 5 nm were formed, forming gold seeds.
[0135] (2) Synthesis of growth solution
[0136] 50 mL of 0.15 M CTAB aqueous solution and 50 mL of 0.15 M benzyl hexadecyl ammonium chloride (BDAC) aqueous solution were added to a 250 mL conical flask, respectively, so that the molar ratio of BDAC / CTAB was 1:1. The conical flask was placed in a prepared water bath, the temperature was maintained at 30°C and stirred to completely dissolve CTAB and BDAC. 100 mL of 0.001 M HAuCl4 aqueous solution, 2.4 mL of 0.004 M AgNO3 aqueous solution and 1.4 mL of 0.00788 M ascorbic acid aqueous solution were added to the conical flask, mixed well, and a growth solution was prepared. The color of the solution became transparent due to the reduction effect of ascorbic acid.
[0137] (3) Synthesis of gold nanorods
[0138] 240 μL of the gold seeds prepared according to step (1) were added to the growth solution prepared according to step (2). When the color of the solution changed from transparent to wine red, it meant the growth of gold nanorods (GNR). After the color change, the solution was stirred for more than 12 hours to complete the crystal growth reaction of gold nanorods (GNR). After the reaction, the solution was centrifuged at 15000 rpm for 30 minutes, washed with distilled water for about 2 times, and then dispersed in distilled water. Among them, the aspect ratio of the gold nanorods was measured to be about 6.
[0139] 2. Preparation of Titanium Dioxide@Gold Nanorod Core-Shell Composite (GNR@TiO2)
[0140] 3 mol TiCl4 was slowly dripped into 1000 mL 1M GNR aqueous solution, and the solution was stirred continuously. A 5% NaHCO3 aqueous solution was added to adjust the pH value to about 8.0, and the solution was stirred for 2 h and allowed to stand at low temperature for 12 h. The obtained hydrolysis precipitate (i.e., the first intermediate) was filtered, washed, dried in a thermostat at 80 ° C for 6 h, and then moved into a muffle furnace and calcined at 400 ° C for 12 h to obtain a titanium dioxide @ gold nanorod core-shell complex (GNR@TiO2), i.e., the second intermediate.
[0141] 3. Preparation of sunscreen material (TA-GNR@TiO2)
[0142] 2.2g of titanium dioxide@gold nanorod core-shell composite (GNR@TiO2) was put into an aqueous solution containing 0.1g of TA (tannic acid, also known as tannic acid), and placed in a 25°C water bath constant temperature oscillator (vibration frequency of 450r / min) for 1h. Centrifuged and washed twice with deionized water to obtain a sunscreen material (TA-GNR@TiO2).
[0143] Example 5
[0144] This example provides a sunscreen material and a preparation method thereof, the preparation method of the sunscreen material comprising:
[0145] 1. Preparation of Gold Nanorods (GNRs)
[0146] (1) Gold seed synthesis
[0147] 5 mL of 0.02 M hexadecyltrimethylammonium bromide (CTAB) aqueous solution and 5 mL of 0.0005 M HAuCl4 aqueous solution were placed in a vial and vortexed vigorously for about 1 minute; thereafter, 900 μL of 0.01 M NaBH4 aqueous solution at about 3°C was added as a reducing agent and vortexed for 3 minutes. As a result, the color of the solution was brown, and gold nanoparticles of about 3 to 5 nm were formed, forming gold seeds.
[0148] (2) Synthesis of growth solution
[0149] 50 mL of 0.15 M CTAB aqueous solution and 50 mL of 0.45 M benzyl hexadecyl ammonium chloride (BDAC) aqueous solution were added to a 250 mL conical flask, respectively, so that the molar ratio of BDAC / CTAB was 3:1. The conical flask was placed in a prepared water bath, the temperature was maintained at 30°C and stirred to completely dissolve CTAB and BDAC. 100 mL of 0.001 M HAuCl4 aqueous solution, 2.4 mL of 0.004 M AgNO3 aqueous solution and 1.4 mL of 0.00788 M ascorbic acid aqueous solution were added to the above conical flask, mixed well, and a growth solution was prepared. The color of the solution became transparent due to the reduction effect of ascorbic acid.
[0150] (3) Synthesis of gold nanorods
[0151] 240 μL of the gold seeds prepared according to step (1) were added to the growth solution prepared according to step (2). When the color of the solution changed from transparent to wine red, it meant the growth of gold nanorods (GNR). After the color change, the solution was stirred for more than 12 hours to complete the crystal growth reaction of gold nanorods (GNR). After the reaction, the solution was centrifuged at 15000 rpm for 30 minutes, washed with distilled water for about 2 times, and then dispersed in distilled water. Among them, the aspect ratio of the gold nanorods was measured to be about 10.
[0152] 2. Preparation of Titanium Dioxide@Gold Nanorod Core-Shell Composite (GNR@TiO2)
[0153] 3 mol TiCl4 was slowly dripped into 1000 mL 1M GNR aqueous solution, and the solution was stirred continuously. A 5% NaHCO3 aqueous solution was added to adjust the pH value to about 8.0, and the solution was stirred for 2 h and allowed to stand at low temperature for 12 h. The obtained hydrolysis precipitate (i.e., the first intermediate) was filtered, washed, dried in a thermostat at 80 ° C for 6 h, and then moved into a muffle furnace and calcined at 400 ° C for 12 h to obtain a titanium dioxide @ gold nanorod core-shell complex (GNR@TiO2), i.e., the second intermediate.
[0154] 3. Preparation of sunscreen material (TA-GNR@TiO2)
[0155] 2.2g of titanium dioxide@gold nanorod core-shell composite (GNR@TiO2) was put into an aqueous solution containing 0.1g of TA (tannic acid, also known as tannic acid), and placed in a 25°C water bath constant temperature oscillator (vibration frequency of 450r / min) for 1h. Centrifuged and washed twice with deionized water to obtain a sunscreen material (TA-GNR@TiO2).
[0156] Example 6
[0157] This example provides a sunscreen material and a preparation method thereof, which is basically the same as Example 1, with the only difference being that during the preparation of the titanium dioxide@gold nanorod core-shell composite (GNR@TiO2), the amount of TiCl4 added is 4 mol.
[0158] Example 7
[0159] This example provides a sunscreen material and a preparation method thereof, which is basically the same as Example 1, with the only difference being that during the preparation of the sunscreen material (TA-GNR@TiO2), the amount of TA added is 0.2 g.
[0160] Performance Test 1
[0161] (1) Cytotoxicity test
[0162] The purpose of the experiment was to investigate the effect of the presence or absence of tannic acid on cytotoxicity. Human fibroblasts (CCD-986sk purchased from ATCC (Manassas, VA, USA)) were used as a normal cell model. Human fibroblasts were cultured in a medium consisting of Iscove's modified Dulbecco's medium (IMDM), 10% fetal bovine serum, and 100 U / mL penicillin-streptomycin sulfate at 37°C in a humidified, 5% CO2 environment. 4 Each well was inoculated in a 32-well culture plate, and 1 g of GNR@TiO2 and TA-GNR@TiO2 aqueous solution with concentrations of 0 / 1 / 5 / 10 / 20 / 30 / 40 / 50 ppm was added to the culture plate and cultured overnight. The culture dish was irradiated with IR-A for 30 min, and the cell viability of human fibroblasts exposed to IR-A through the slide was evaluated using the Epoch microplate spectrophotometer (BioTek, USA) by colorimetric MTT meta-bolic activity assay. The test results are shown in Table 1.
[0163] Table 1
[0164]
[0165] As shown in Table 1, the cell survival rate of the samples without tannic acid (tannic acid) added decreased as the concentration in the culture plate increased; the cell survival rate of the samples with tannic acid (tannic acid) added increased as the concentration in the formula plate increased. It can be seen that the addition of tannic acid (tannic acid) helps to protect the survival of cells.
[0166] (2) Photocatalytic activity test
[0167] When the unwrapped inorganic sunscreen TiO2 / ZnO absorbs ultraviolet rays, it can generate hole-electron pairs, which can reduce-oxidize the surrounding organic matter, thereby generating reactive oxygen. Tannic acid (tannic acid) belongs to phenolic substances and can remove free radicals and reactive oxygen through the photocatalytic action of inorganic sunscreens. When reactive oxygen is generated, the unique blue color of methylene blue at 600nm will become transparent, so a standard curve of methylene blue content and photocatalytic activity can be obtained. By measuring the photocatalytic degradation amount of methylene blue in the methylene blue solution containing the sample under ultraviolet light irradiation of different lengths, the inhibition of tannic acid (tannic acid) on photocatalysis is determined. The test results are shown in Table 2 below.
[0168] Table 2
[0169]
[0170] From Table 2, it can be seen that for the sample without tannic acid (tannic acid) added (titanium dioxide @ gold nanorod core-shell composite (GNR@TiO2)), the concentration of methylene blue dropped from 10 mg / L to 4.0 mg / L after 180 minutes of ultraviolet irradiation, and the degradation rate was about 60.0%; for the sample with tannic acid (tannic acid) added (i.e., the sunscreen material of the present invention (TA-GNR@TiO2)), the concentration of methylene blue dropped from 9.7 mg / L to 8.8 mg / L after 180 minutes of ultraviolet irradiation, and the degradation rate was about 9.28%. It can be seen that the addition of tannic acid (tannic acid) helps to inhibit the photocatalytic activity of titanium dioxide.
[0171] (3) Skin safety test
[0172] In order to ensure the safety of TA-TiO2@GNR applied to the human body, a skin occlusion patch test was conducted in accordance with the "Technical Rules for Safety of Cosmetics". First, according to the subject selection criteria specified in the "Technical Rules for Safety of Cosmetics", 30 people were selected to participate in the test. Then, a patch tester containing 300ppm TA-TiO2@GNR aqueous solution was applied to the curved side of the subject's forearm with a low-allergenic tape, and the palm of the hand was gently pressed to evenly apply it to the skin for 24 hours. The skin reaction was observed according to the standards in Appendix 3 30 minutes (after the indentation disappears), 24 hours and 48 hours after the removal of the test patch tester, and the observation results were recorded. As shown in the results in Table 4, 0 of the 30 people had adverse skin reactions.
[0173] Table 3 Skin reaction grading standards for occlusive patch test (Technical Specifications for Safety of Cosmetics (2015 Edition))
[0174]
[0175] Table 4 Summary of human patch test results
[0176]
[0177] Example 8
[0178] This example provides a blocking agent with dual blocking effects of ultraviolet rays and near-infrared rays and a preparation method thereof. The preparation method comprises: adding the sunscreen material prepared in Example 1 into water, and adding 1,2-hexanediol, mixing and dispersing to prepare a blocking agent; wherein, in terms of mass percentage, the sunscreen material accounts for 0.0069%, 1,2-hexanediol accounts for 2.5%, and water accounts for 97.4931%.
[0179] Example 9
[0180] This example provides a blocking agent with dual blocking effects of ultraviolet rays and near-infrared rays and a preparation method thereof, which is basically the same as Example 8, with the only difference being that "the sunscreen material prepared in Example 1" is replaced by "the sunscreen material prepared in Example 2".
[0181] Example 10
[0182] This example provides a blocking agent with dual blocking effects of ultraviolet rays and near-infrared rays and a preparation method thereof, which is basically the same as Example 8, with the only difference being that "the sunscreen material prepared in Example 1" is replaced by "the sunscreen material prepared in Example 3".
[0183] Embodiment 11
[0184] This example provides a blocking agent with dual blocking effects of ultraviolet rays and near-infrared rays and a preparation method thereof, which is basically the same as Example 8, with the only difference being that "the sunscreen material prepared in Example 1" is replaced by "the sunscreen material prepared in Example 4".
[0185] Example 12
[0186] This example provides a blocking agent with dual blocking effects of ultraviolet rays and near-infrared rays and a preparation method thereof, which is basically the same as Example 8, with the only difference being that "the sunscreen material prepared in Example 1" is replaced by "the sunscreen material prepared in Example 5".
[0187] Example 13
[0188] This example provides a blocking agent with dual blocking effects of ultraviolet rays and near-infrared rays and a preparation method thereof, which is basically the same as Example 8, with the only difference being that "the sunscreen material prepared in Example 1" is replaced by "the sunscreen material prepared in Example 6".
[0189] Embodiment 14
[0190] This example provides a blocking agent with dual blocking effects of ultraviolet rays and near-infrared rays and a preparation method thereof, which is basically the same as Example 8, with the only difference being that "the sunscreen material prepared in Example 1" is replaced by "the sunscreen material prepared in Example 7".
[0191] Application Example 1
[0192] This example provides a sunscreen and a preparation method thereof, and the raw material formula thereof is shown in Table 5.
[0193] Table 5
[0194]
[0195] The preparation method of the sunscreen comprises:
[0196] (1) After measuring the raw materials of phase B, heat to 50°C, mix and stir evenly, then cool to 30°C;
[0197] (2) The raw materials of phase C and phase D are measured and put into the phase B container in sequence;
[0198] (3) Disperse the raw materials of phase A separately and put them into the container of phase B and stir evenly;
[0199] (4) separately measuring and evenly dispersing the raw materials of phase E;
[0200] (5) Pre-dispersing the AD phase mixture at room temperature, slowly adding the E phase for emulsification;
[0201] (6) degassing and filtering to obtain a water-in-oil formulation of sunscreen.
[0202] Application Example 2
[0203] This example provides a sunscreen and a preparation method thereof. This example is basically the same as Application Example 1, with the only difference being that the amount of the blocking agent added is 0.5% (containing 15 ppm GNR).
[0204] Application Example 3
[0205] This example provides a sunscreen and a preparation method thereof. This example is basically the same as Application Example 1, with the only difference being that the amount of the blocking agent added is 1% (containing 30 ppm GNR).
[0206] Application Example 4
[0207] This example provides a sunscreen and a preparation method thereof. This example is basically the same as Application Example 1, with the only difference being that the amount of blocking agent added is 1.67% (including 50 ppm GNR).
[0208] Application Example 5
[0209] This example provides a sunscreen and a preparation method thereof. This example is basically the same as Application Example 1, with the only difference being that the amount of the blocking agent added is 3.33% (including 100 ppm GNR).
[0210] Application Example 6
[0211] This example provides a sunscreen and a preparation method thereof. This example is basically the same as Application Example 1, with the only difference being that the amount of the blocking agent added is 5% (containing 150 ppm GNR).
[0212] Application Example 7
[0213] This example provides a sunscreen and a preparation method thereof. This example is basically the same as Application Example 1, with the only difference being that the amount of the blocking agent added is 10% (containing 300 ppm GNR).
[0214] Application Example 8
[0215] This example provides a sunscreen and a preparation method thereof. This example is basically the same as Application Example 1, with the only difference being that the amount of the blocking agent added is 20% (containing 600 ppm GNR).
[0216] Application Example 9
[0217] This example provides a sunscreen and a preparation method thereof. This example is basically the same as Application Example 1, with the only difference being that the amount of blocking agent added is 30% (including 900 ppm GNR).
[0218] Application Comparative Example 1
[0219] This example provides a sunscreen and a preparation method thereof, and the raw material formula thereof is shown in Table 6.
[0220] Table 6
[0221]
[0222]
[0223] The preparation method is the same as that of Application Example 1.
[0224] Application Comparative Example 2
[0225] This example provides a sunscreen and a preparation method thereof, and the raw material formula thereof is shown in Table 7.
[0226] Table 7
[0227]
[0228]
[0229] The preparation method is the same as that of Application Example 1.
[0230] Application Comparative Example 3
[0231] This example provides a sunscreen and a preparation method thereof, and the raw material formula thereof is shown in Table 8.
[0232] Table 8
[0233]
[0234] The preparation method is the same as that of Application Example 7.
[0235] Performance Test 2
[0236] (1) Near infrared heat blocking effect test
[0237] The sunscreens prepared in Comparative Examples 1-3 and Application Examples 1-7 were respectively 2 The dose was evenly applied on the slide, with an area of 8.5 cm 2 (1.7×5.0cm 2 ) and dried for 10 min. Except for the hole the size of the slide, the rest of the area is made of thick paper. The heating zone for measuring the temperature rise caused by IR-A through the transmission window is a petri dish covered with a nitrile synthetic rubber cover. The slide coated with sunscreen is placed on the transmission window 15 cm away from the IR lamp (250 W, BR125 red, Phi-lips, The Netherlands), and the heating zone for measuring the temperature is 10 cm away from the slide. The temperature change ΔT (℃) on the surface of the nitrile synthetic rubber cover (referred to as the heating zone) caused by IR radiation through the slide during the 10 min IR irradiation is recorded.
[0238] Temperature change ΔT(℃) = T final -T initial (T final : Temperature after IR irradiation for 10 minutes, T initial : Temperature before IR irradiation)
[0239] The change in the temperature rise suppression rate of the comparative example and the embodiment is calculated by the following formula, %.
[0240] Temperature rise suppression rate ΔTRI (%) = TRI sample - TRI carrier {TRI sample (%) = [(T(f) slide - T(f) sample) / (T(f) slide - T(i) slide)] × 100%, TRI carrier (%) = [(T(f) slide - T(f) carrier) / (T(f) slide - T(i) slide)] × 100%}
[0241] T(f)slide is the temperature of the glass slide after IR radiation passes through the glass slide without sunscreen, °C; T(f)sample is the temperature of the glass slide after IR radiation passes through the glass slide with sunscreen sample, °C; T(i)slide is the temperature of the glass slide before IR radiation passes through the glass slide without sunscreen, °C; T(f)carrier is the temperature of the glass slide after IR radiation passes through the glass slide with sunscreen matrix, °C;
[0242] TRI 载体 In the sunscreen, the base material used is the sunscreen matrix, which is the base material without sunscreen and blocking agents.
[0243] The results are shown in Table 9.
[0244] Table 9 In vitro evaluation of IR-A blocking performance
[0245]
[0246] It can be seen from Table 9 that as the content of TA-TiO2@GNR in the sunscreen increases, the temperature change decreases from 7.9℃ to 4.4℃, and the temperature rise inhibition rate increases from 8.7% to 35.5%, indicating that TA-TiO2@GNR has a thermal blocking effect. When 50ppm GNR is added to the formula, the temperature change increases from 7.9℃ to 9.1℃, and the temperature rise inhibition rate decreases from 8.7 to 5.8%, which may be due to the IR-A SPR (surface plasmon resonance effect) absorption of GNR causing photothermal conversion, thereby increasing the skin temperature, while TA-TiO2@GNR can absorb IR-A and has a high scattering rate, which can show a good thermal resistance effect.
[0247] At the same time, from the comparison between Application Example 7 and Application Comparative Example 3, it can be seen that even if the same amount of gold nanorods, titanium dioxide and tannic acid are added, if the product does not present the specific structure of the present invention, its infrared blocking effect is relatively poor.
[0248] (2) In vitro sunscreen effect test
[0249] The UV-2000S COLIPA method was used to determine the in vitro sunscreen effect of the sunscreen base: the sunscreens prepared in Comparative Examples 1-3 and Application Examples 1-7 were heated to 1.3 mg / cm 2 Apply evenly on a 5cm*5cm PMMA plate, spread evenly with your fingers, and store in a dark place for 15 minutes to form a film. Place the PMMA plate after light protection treatment in UV-2000S for analysis to obtain the in vitro sun protection value.
[0250] The results are shown in Table 10.
[0251] Table 10 Evaluation of in vitro sunscreen effect
[0252]
[0253] Note: The sun protection factor (SPF) is a specific value that indicates the ability of a product to protect against UVB rays. It is an indicator for evaluating the ability of sunscreen cosmetics to protect the skin from sunburn. SPF is the abbreviation of Sun Protection Factor. The larger the SPF value, the better the effect of preventing sunburn.
[0254] PFA (Protection Factor of UVA) refers to the ability to protect against long-wave ultraviolet rays. The calculation formula is PFA = MPPD value of skin with sunscreen applied / MPPD value of skin without sunscreen applied. The higher the PFA value, the better the effect of preventing skin from tanning.
[0255] It can be seen from Table 10 that there is not much difference in the in vitro sun protection values of the sunscreens of Comparative Examples 1-2 and Application Examples 1-4. This should be caused by the very small amount of TA-TiO2@GNR added. Taking GNR as the benchmark, once the addition amount reaches a relatively large amount of 100 ppm and above, referring to Application Examples 5-7, it can be found that the sun protection values are significantly improved. For example, the in vitro sun protection value of Example 7 increases from SPF27.9 / PFA13.5 to SPF 37.8 / PFA 17.3.
[0256] In particular, from the comparison between Application Example 7 and Application Comparative Example 3, it can be seen that even if the same amount of gold nanorods, titanium dioxide and tannic acid are added, if the specific structure of the present invention is not presented in the product, the blocking effect of ultraviolet rays is relatively poor.
[0257] (3) User experience evaluation
[0258] The sunscreen cover labels prepared by using comparative examples 1-3 and application examples 5-7 were evaluated by 10 consumers for their use experience. Each skin feeling experience can be scored between 1 and 5 points. The higher the score, the more recognized it is. For example, a high moisturizing sense score indicates that the moisturizing feeling is strong. The evaluation results of the 10 consumers were summarized and the average was calculated. The results are shown in Table 11 below.
[0259] Table 11 Evaluation of usage experience
[0260]
[0261]
[0262] It can be seen from Table 11 that, compared with the control examples without the addition of the sunscreen material or blocker of the present invention, the addition of the sunscreen material or blocker of the present invention has no negative impact on the fit, spreadability, sliding feel, and durability; in particular, TA-TiO2@GNR exhibits a heat blocking effect that slightly enhances the moisturizing and refreshing feel.
[0263] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
[0264] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A sunscreen material, characterized in that: The sunscreen material comprises gold nanorods, a first shell layer coated on the gold nanorods, and a second shell layer coated on the first shell layer, wherein the material of the first shell layer comprises titanium dioxide, and the material of the second shell layer comprises tannic acid or its derivatives.
2. The sunscreen material according to claim 1, characterized in that: The aspect ratio of the gold nanorods is 3-10; and / or the gold nanorods absorb infrared rays with a wavelength of 700-1400nm.
3. The sunscreen material according to claim 1, characterized in that: The first shell layer is a titanium dioxide shell.
4. The sunscreen material according to claim 1, characterized in that: The preparation of the first shell layer meets the following conditions: (1) using the gold nanorods and the first shell layer precursor as raw materials, respectively, wherein the first shell layer precursor refers to a substance that can generate the first shell layer through one or more steps of conversion treatment; (2) The one-step or multi-step conversion treatment includes a precipitation treatment in the presence of a precipitant, and a calcination treatment.
5. The sunscreen material according to claim 4, characterized in that: The first shell layer precursor comprises titanium halide; and / or the precipitant comprises carbonate and / or bicarbonate.
6. The sunscreen material according to claim 1, characterized in that: In terms of mass percentage, in the sunscreen material, the total mass of the gold nanorods and the first shell layer accounts for 90%-99%, and the second shell layer accounts for 1%-10%; and / or the mass ratio of the gold nanorods to the first shell layer is 1:0.8-4.
1.
7. A method for preparing the sunscreen material according to any one of claims 1 to 6, characterized in that: The preparation method comprises: Dispersing the gold nanorods and the first shell precursor in a solvent, adding a precipitant capable of reacting with the first shell precursor to generate a first intermediate, and calcining the first intermediate to obtain a second intermediate; The second intermediate and the material of the second shell layer are mixed and stirred to obtain the sunscreen material.
8. A blocking agent having dual blocking effects of ultraviolet rays and near infrared rays, characterized in that: The blocking agent comprises the sunscreen material according to any one of claims 1 to 6, water and an optional alcohol substance.
9. A sunscreen composition, characterized in that: The sunscreen composition comprises nano titanium dioxide and / or nano zinc oxide, and the sunscreen material according to any one of claims 1 to 6 or the blocking agent having dual ultraviolet and near infrared blocking effects according to claim 8.
10. Use of the sunscreen material according to any one of claims 1 to 6, or the blocking agent with dual ultraviolet and near infrared blocking effects according to claim 8, or the sunscreen composition according to claim 9 in cosmetics.
Citation Information
Cited By
Cosmetic composition for sunscreen comprising core-shell NANO composite
KR102959079B1