Preparation method of zwitterionic hydrophilic chain extender

Through the preparation method of zwitterionic hydrophilic chain extender, the problems of poor hydrolysis stability and limited mechanical properties of aqueous polyurethane chain extender are solved, and the preparation of high-performance water-based polyurethane is realized. It is suitable for multiple industries and reduces production costs and environmental pollution.

CN119019298AInactive Publication Date: 2024-11-26SHANDONG MICHI NEW MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411117524.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing water-based polyurethane chain extenders have problems such as poor hydrolysis stability, limited mechanical properties, high cost and environmental pollution, which are difficult to meet the needs of high-performance applications.

Method used

Using a preparation method of zwitterionic hydrophilic chain extender, the reaction of triethanolamine and methanedisulfonate in ethanol is carried out with heating and reflux reaction, combined with the steps of decompression distillation and recrystallization, the reaction steps are simplified and the production cost is reduced. , and improve hydrolysis stability and mechanical properties.

Benefits of technology

It has achieved high-performance preparation of water-based polyurethane, significantly improved solid content and surface activity, enhanced hydrolysis resistance and mechanical strength, reduced raw material toxicity and environmental pollution, and is suitable for many industries such as coatings, adhesives, leather and textiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019298A_ABST
    Figure CN119019298A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a zwitterionic hydrophilic chain extender, which belongs to the technical field of chain extenders, and comprises the following steps: dissolving triethanolamine and methylene methanedisulfonate in ethanol, and carrying out reflux reaction at 65-80 DEG C for 6-8 hours to obtain a primary product; removing unreacted triethanolamine and ethanol through reduced pressure distillation to obtain a purified product; the preparation method comprises the following steps: dissolving 2-amino-2-methyl-1, 3-pentanediol into acetone, adding naphthalene disulfonic acid ethyl bile ammonium, uniformly mixing, adding an ethanol solution with the concentration of 60%, and reacting at 120-140 DEG C for 6-12 hours to obtain a second-stage product; recrystallizing the secondary product, slowly reducing the temperature, and finally performing vacuum freeze drying to obtain the zwitterionic hydrophilic chain extender. The preparation method provided by the invention is simple in process and high in yield, and the obtained product is excellent in performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chain extenders, and in particular relates to a method for preparing a zwitterionic hydrophilic chain extender. The zwitterionic hydrophilic chain extender combines the properties of anionic and cationic chain extenders and can make the synthesized polyurethane have good surface activity. Background Art

[0002] Polyurethane materials are widely used in coatings, adhesives, leather, textiles and other fields due to their excellent performance. However, traditional solvent-based polyurethane uses volatile organic solvents, which pollutes the environment and is not in line with the concept of sustainable development. Waterborne polyurethane (WPU) uses water as a dispersion medium and has the advantages of being environmentally friendly, safe and non-toxic, and has become a hot spot for research and application in recent years.

[0003] The performance of waterborne polyurethane is closely related to its structure, and chain extender, as one of the key raw materials for synthesizing waterborne polyurethane, has a vital influence on the performance of waterborne polyurethane. Chain extender reacts with polyurethane prepolymer to:

[0004] Increase molecular weight: Improve the mechanical properties, abrasion resistance and chemical resistance of waterborne polyurethane.

[0005] Introducing functional groups: improving the hydrophilicity, surface activity, biocompatibility, etc. of waterborne polyurethane.

[0006] The existing waterborne polyurethane chain extenders mainly have the following technical defects:

[0007] Anionic chain extender:

[0008] Patent document 1 (CN104616263A) discloses a waterborne polyurethane chain extender and a preparation method thereof, which is prepared by esterification reaction using dimethylolpropionic acid (DMPA) as a raw material; however, the chain extender has poor hydrolysis stability and is easily hydrolyzed in a high temperature and high humidity environment, resulting in a decrease in the performance of the waterborne polyurethane.

[0009] Patent document 2 (CN105316586A) discloses a sulfonic acid group-containing waterborne polyurethane chain extender and a preparation method thereof, which is prepared by an etherification reaction using sodium 2-butene-1,4-diol disulfonate as a raw material; although the hydrolysis stability of the chain extender is improved, the mechanical properties of the synthesized waterborne polyurethane are limited and it is difficult to meet the requirements of high-performance applications.

[0010] Cationic chain extender:

[0011] Patent document 3 (CN103750375A) discloses a quaternary ammonium salt type waterborne polyurethane chain extender and a preparation method thereof, which is prepared by quaternization reaction using triethanolamine as a raw material; the chain extender can give the waterborne polyurethane excellent water resistance and adhesion, but its synthesis cost is high, and it is sensitive to pH value, which easily leads to instability of the waterborne polyurethane system.

[0012] Nonionic chain extenders:

[0013] Patent document 4 (CN102776868A) discloses a polyether-type waterborne polyurethane chain extender prepared using polyethylene glycol (PEG) or polypropylene glycol (PPG) as raw materials; the chain extender has good hydrolysis stability and freeze-thaw stability, but its improvement on the mechanical properties of waterborne polyurethane is limited, and it is difficult to meet the needs of high-performance applications.

[0014] Zwitterionic chain extenders:

[0015] Patent document 5 (CN109271165A) discloses a zwitterionic waterborne polyurethane chain extender and a preparation method thereof. The method is prepared by multi-step reaction, the synthesis route is long, the reaction conditions are harsh, and there is an environmental pollution problem, which is not conducive to large-scale industrial production.

[0016] In summary, the existing waterborne polyurethane chain extenders have problems such as poor hydrolysis stability, limited mechanical properties, high cost, and environmental pollution; therefore, it is of great significance to develop a new waterborne polyurethane chain extender with a simple synthesis route, low cost, environmental friendliness, and excellent performance. Summary of the invention

[0017] 1. Problems to be solved

[0018] In view of the problems existing in the prior art, such as poor hydrolysis stability, limited mechanical properties, high cost and environmental pollution of waterborne polyurethane chain extenders, the present invention proposes a novel preparation method of zwitterionic hydrophilic chain extenders to solve these technical defects; compared with the traditional method, the preparation method of the present invention has the following advantages:

[0019] Simple process: The reaction steps are simplified and easy to operate.

[0020] Low cost: The raw materials used are low-priced, reducing the overall production cost.

[0021] Environmentally friendly: reduces the generation of harmful by-products and meets environmental protection requirements.

[0022] Excellent performance: The obtained chain extender has good hydrolysis stability and mechanical properties, and is suitable for the preparation of high-performance waterborne polyurethane.

[0023] This new chain extender can not only be used in the synthesis of polyurethane, but also in multiple industries such as coatings, adhesives, leather and textiles to improve the comprehensive performance of materials.

[0024] 2. Technical solution

[0025] To solve the above problems, the present invention adopts the following technical solutions.

[0026] A method for preparing a zwitterionic hydrophilic chain extender comprises the following steps:

[0027] (1) dissolving triethanolamine and methylene disulfonate in ethanol, heating under reflux for 6-8 hours to obtain a primary product;

[0028] (2) removing unreacted triethanolamine and ethanol from the primary product in step (1) to obtain a purified product, then adding acetone to dissolve it, adding ethyl lactammonium naphthalene disulfonate, mixing well, adding ethanol, and heating the reactor to react to obtain a secondary product;

[0029] (3) The secondary product in step (2) is recrystallized and then dried to obtain a zwitterionic hydrophilic chain extender.

[0030] The following are the chemical substances involved and their CAS numbers:

[0031] Triethanolamine

[0032] CAS No.: 102-71-6

[0033] Methanedisulfonicaciddimethylester

[0034] CAS No.: 99591-74-9

[0035] Acetone

[0036] CAS No.: 67-64-1

[0037] Aclatoniumnapadisilate

[0038] CAS No.: 55077-30-0

[0039] Preferably, in the method for preparing the zwitterionic hydrophilic chain extender described above, the molar ratio between the triethanolamine described in step (1) and the methylene disulfonate described is (1.0-2.0):1.

[0040] Preferably, in the method for preparing the zwitterionic hydrophilic chain extender described above, the molar ratio between the triethanolamine described in step (1) and the methylene disulfonate described is (1.3-1.6):1.

[0041] Preferably, in the method for preparing the zwitterionic hydrophilic chain extender described above, the molar ratio between the triethanolamine described in step (1) and the methylene disulfonate described is 1.4:1.

[0042] Preferably, in the method for preparing the zwitterionic hydrophilic chain extender described above, the ethanol in step (1) is anhydrous ethanol; the amount of ethanol in step (1) is 40mL-50mL per mol of methylene disulfonate; the heating temperature in step (1) is 65°C-80°C; and the reflux equipment in step (1) is a condenser.

[0043] Preferably, in the preparation method of the zwitterionic hydrophilic chain extender described above, the removal method in step (1) is vacuum distillation at a pressure of 1.3-2.0 kPa; wherein the vacuum distillation method first distills out ethanol at 60°C, wherein the ethanol fraction receiving temperature is 40°C, and then gradually raises the temperature to 210°C to distill out triethanolamine, wherein the triethanolamine fraction receiving temperature is 180°C.

[0044] Preferably, in the method for preparing the zwitterionic hydrophilic chain extender described above, the amount of acetone used in step (2) is 30 mL-50 mL per mol of methylene disulfonate; the amount of ethyl lactammonium naphthalene disulfonate used in step (2) is 2 mol-5 mol per mol of methylene disulfonate.

[0045] Preferably, in the method for preparing the zwitterionic hydrophilic chain extender described above, the ethanol in step (2) is an ethanol solution with a mass concentration of 60%; the amount of ethanol in step (2) is 60mL-90mL per mol of methylene disulfonate.

[0046] Preferably, in the method for preparing the zwitterionic hydrophilic chain extender described above, the temperature of heating the reactor in step (2) is 120-140° C.; and the time of heating the reactor in step (2) is 6 h-12 h.

[0047] Preferably, in the method for preparing the zwitterionic hydrophilic chain extender described above, the rate of slowly reducing the temperature of the recrystallization in step (3) is 2° C.-4° C. per minute; and the drying method in step (3) is vacuum freeze-drying.

[0048] 3. Beneficial effects

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] The invention provides a simplified method for synthesizing a zwitterionic hydrophilic chain extender. The method can quickly and efficiently prepare a target product by reacting triethanolamine and methylene disulfonate in ethanol, combined with reduced pressure distillation and recrystallization and other steps. The method not only reduces the reaction steps, but also reduces the production cost, making the method more suitable for large-scale industrial production. The synthesized zwitterionic hydrophilic chain extender shows excellent performance in the preparation of polyurethane. Firstly, it can significantly improve the solid content and surface activity of polyurethane, so that the prepared polyurethane material exhibits better mechanical strength and wear resistance in application; secondly, the introduction of sulfonic acid groups enhances the hydrophilicity of polyurethane, so that it exhibits good stability and hydrolysis resistance in an aqueous system; compared with traditional chain extenders, the raw materials used in the synthesis process of the chain extender of the present invention are less toxic, and the reaction conditions are mild, thereby reducing pollution to the environment; at the same time, water is used as a dispersion medium, thereby avoiding the use of organic solvents, which meets the requirements of modern environmental protection and sustainable development; due to its excellent performance, the chain extender is not only suitable for the synthesis of waterborne polyurethane, but also can be widely used in multiple industries such as coatings, adhesives, leather and textiles; the versatility of this chain extender enables it to meet the needs of different application occasions and broadens its market potential; the preparation method of the present invention not only reduces the raw material and production costs, but also improves the added value of the product; by optimizing the reaction conditions and the raw material ratio, the production efficiency and economic benefits can be maximized under the premise of ensuring product quality; this is of great significance for enterprises to gain advantages in market competition.

[0051] In summary, the present invention solves many deficiencies in the prior art through an innovative synthesis method and excellent product performance, has significant technical and economic advantages, and promotes the further development and application of waterborne polyurethane materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 The schematic diagram of the reaction of triethanolamine and methylene disulfonate;

[0053] Figure 2 3D image of the product of the reaction of triethanolamine and methylene methanedisulfonate;

[0054] Figure 3 is the hydrogen spectrum of the product of the reaction of triethanolamine and methylene methanedisulfonate;

[0055] Figure 4 This is the carbon spectrum of the product of the reaction of triethanolamine and methylene methanedisulfonate;

[0056] Figure 5 is a structural diagram of a zwitterionic hydrophilic chain extender;

[0057] Figure 6 3D diagram of zwitterionic hydrophilic chain extender;

[0058] Figure 7 is the hydrogen spectrum of the zwitterionic hydrophilic chain extender;

[0059] Figure 8 This is the carbon spectrum of zwitterionic hydrophilic chain extender. DETAILED DESCRIPTION

[0060] The present invention is further described below in conjunction with specific embodiments.

[0061] As an environmentally friendly material, waterborne polyurethane (WPU) has been widely used in coatings, adhesives, textiles and other fields due to its excellent performance. In order to further improve its performance, researchers are exploring methods to introduce both anionic and non-ionic functional groups into the polymer. This combination can not only enhance the ionic stability of waterborne polyurethane, but also significantly improve its freeze-thaw stability.

[0062] Synergistic effects of anionic and nonionic functional groups

[0063] The role of anionic functional groups:

[0064] Anionic functional groups, such as sulfonic acid and carboxylic acid groups, provide excellent water solubility and ionic stability. They prevent excessive aggregation between polymer chains through electrostatic repulsion, thereby improving the stability of the emulsion.

[0065] Anionic functional groups can also enhance the hydrolysis resistance of polyurethane, enabling it to maintain excellent mechanical properties in a humid environment.

[0066] The role of non-ionic functional groups:

[0067] Nonionic functional groups, such as polyether segments, can improve the flexibility and low-temperature resistance of polyurethanes. They interact with water molecules through hydrogen bonds and van der Waals forces, enhancing the hydrophilicity and freeze-thaw stability of the polymer.

[0068] The introduction of nonionic functional groups can also reduce the viscosity of the system and improve processing performance.

[0069] Synergy Effect:

[0070] The combination of anionic and nonionic functional groups can form a stable network structure in waterborne polyurethane. This structure not only improves the mechanical strength and wear resistance of polyurethane, but also enhances its stability under extreme temperatures.

[0071] Technical Implementation

[0072] Synthesis method:

[0073] Anionic and nonionic functional groups are introduced into the polyurethane chain through chemical synthesis technology. Commonly used methods include copolymerization and graft polymerization, which can accurately control the amount and position of functional groups introduced, thereby optimizing the properties of polyurethane.

[0074] The specific synthesis steps may include: adding a chain extender containing anionic and nonionic functional groups to the polyurethane prepolymer stage, and combining it with the polyurethane main chain through a chemical reaction.

[0075] Performance optimization:

[0076] The properties of waterborne polyurethane can be further optimized by adjusting the ratio of anionic and nonionic functional groups. For example, increasing the ratio of anionic functional groups can improve water resistance, while increasing the ratio of nonionic functional groups can improve flexibility and low temperature resistance.

[0077] Application prospects

[0078] Coatings and Adhesives:

[0079] The modified waterborne polyurethane exhibits excellent adhesion and weather resistance in the fields of coatings and adhesives, and is suitable for applications requiring high durability.

[0080] Textile and Leather:

[0081] In textile and leather processing, modified waterborne polyurethane can provide soft feel and excellent abrasion resistance while maintaining good breathability and waterproofness.

[0082] Other areas:

[0083] Due to its excellent comprehensive properties, modified waterborne polyurethane can also be used in fields such as building materials, automotive interiors and electronic products to meet the special needs of different application occasions.

[0084] Therefore, by simultaneously introducing anionic and nonionic functional groups into waterborne polyurethane, its ionic stability and freeze-thaw stability can be significantly improved; this modification method not only broadens the application field of waterborne polyurethane, but also provides new possibilities for its application in high-performance materials.

[0085] Technical Solution 1

[0086] The preparation method of a zwitterionic hydrophilic chain extender comprises the following steps:

[0087] (1) dissolving triethanolamine and methylene disulfonate in ethanol, heating under reflux for 6 hours to obtain a primary product;

[0088] It should be noted that the molar ratio between the triethanolamine and the methylene methanedisulfonate is 1.0:1.

[0089] Meanwhile, the ethanol is anhydrous ethanol; the amount of ethanol used is 40 mL per mol of methylene disulfonate; the heating temperature is 80° C.; the reflux equipment in step (1) is a condenser, using an Allihn condenser.

[0090] (2) removing the unreacted triethanolamine and ethanol in the primary product of step (1) to obtain a purified product, then adding acetone to dissolve it, then adding ethyl lactoammonium naphthalene disulfonate, mixing it, adding ethanol, heating the reactor to react, and obtaining a secondary product; the removal method is vacuum distillation, the pressure is 1.3 kPa, and the equipment model name is Pilodist PD300CC; wherein the vacuum distillation method first distills out ethanol at 60° C., wherein the ethanol fraction receiving temperature is 40° C., and then gradually raising the temperature to 210° C. to distill out triethanolamine, wherein the triethanolamine fraction receiving temperature is 180° C.

[0091] In the above-mentioned preparation method of the zwitterionic hydrophilic chain extender, the amount of acetone is 30 mL per mole of methylene disulfonate; the amount of ethyl lactocholine ammonium naphthalene disulfonate is 5 mol per mole of methylene disulfonate; ethanol is an ethanol solution with a mass concentration of 60%; the amount of ethanol is 60 mL per mole of methylene disulfonate. In the above-mentioned preparation method of the zwitterionic hydrophilic chain extender, the temperature of the reaction kettle heating reaction is 120°C; the time of the reaction kettle heating reaction is 12 hours.

[0092] (3) The secondary product in step (2) is recrystallized and then dried to obtain a zwitterionic hydrophilic chain extender. Furthermore, the recrystallization temperature is slowly reduced at a rate of 2° C. per minute; the drying method is vacuum freeze drying using a MartinChrist freeze dryer.

[0093] Technical Solution 2

[0094] The preparation method of a zwitterionic hydrophilic chain extender comprises the following steps:

[0095] (1) dissolving triethanolamine and methylene disulfonate in ethanol, heating under reflux for 8 hours to obtain a primary product;

[0096] It should be noted that the molar ratio between the triethanolamine and the methylene methanedisulfonate is 2.0:1.

[0097] Meanwhile, the ethanol is anhydrous ethanol; the amount of ethanol used is 50 mL per mol of methylene disulfonate; the heating temperature is 65° C.; the reflux equipment in step (1) is a condenser, using an Allihn condenser.

[0098] (2) removing the unreacted triethanolamine and ethanol from the primary product in step (1) to obtain a purified product, then adding acetone to dissolve it, then adding ethyl lactoammonium naphthalene disulfonate, mixing it, adding ethanol, heating the reactor to react, and obtaining a secondary product; the removal method is vacuum distillation, the pressure is 2.0 kPa, and the equipment model name is Pilodist PD300CC; wherein the vacuum distillation method first distills out ethanol at 60° C., wherein the ethanol fraction receiving temperature is 40° C., and then gradually raising the temperature to 210° C. to distill out triethanolamine, wherein the triethanolamine fraction receiving temperature is 180° C.

[0099] The preparation method of the zwitterionic hydrophilic chain extender described above, the amount of acetone is 50mL per mol of methylene disulfonate; the amount of ethyl lactoammonium naphthalene disulfonate is 2mol per mol of methylene disulfonate; ethanol is an ethanol solution with a mass concentration of 60%; the amount of ethanol is 90mL per mol of methylene disulfonate; in the preparation method of the zwitterionic hydrophilic chain extender described above, the temperature of the reactor heating reaction is 140°C; the heating reaction time of the reactor is 6h.

[0100] (3) The secondary product in step (2) is recrystallized and then dried to obtain a zwitterionic hydrophilic chain extender. Furthermore, the recrystallization temperature is slowly reduced at a rate of 4° C. per minute; the drying method is vacuum freeze drying using a MartinChrist freeze dryer.

[0101] Technical Solution 3

[0102] The preparation method of a zwitterionic hydrophilic chain extender comprises the following steps:

[0103] (1) dissolving triethanolamine and methylene disulfonate in ethanol, heating under reflux for 6 hours to obtain a primary product;

[0104] It should be noted that the molar ratio of the triethanolamine in step (1) to the methylene disulfonate is 1.3:1.

[0105] Meanwhile, the ethanol is anhydrous ethanol; the amount of ethanol used is 40 mL / mol of methylene disulfonate; the heating temperature is 65° C.; the reflux equipment in step (1) is a condenser, using an Allihn condenser.

[0106] (2) removing the unreacted triethanolamine and ethanol in the primary product of step (1) to obtain a purified product, then adding acetone to dissolve it, then adding ethyl lactoammonium naphthalene disulfonate, mixing it, adding ethanol, heating the reactor to react, and obtaining a secondary product; the removal method is vacuum distillation, the pressure is 1.3 kPa, and the equipment model name is Pilodist PD300CC; wherein the vacuum distillation method first distills out ethanol at 60° C., wherein the ethanol fraction receiving temperature is 40° C., and then gradually raising the temperature to 210° C. to distill out triethanolamine, wherein the triethanolamine fraction receiving temperature is 180° C.

[0107] In the above-mentioned preparation method of the zwitterionic hydrophilic chain extender, the amount of acetone is 30 mL per mole of methylene disulfonate; the amount of ethyl lactocholine ammonium naphthalene disulfonate is 2 mol per mole of methylene disulfonate; ethanol is an ethanol solution with a mass concentration of 60%; the amount of ethanol is 60 mL per mole of methylene disulfonate. In the above-mentioned preparation method of the zwitterionic hydrophilic chain extender, the temperature of the reaction kettle heating reaction is 120°C; the time of the reaction kettle heating reaction is 6 hours.

[0108] (3) The secondary product in step (2) is recrystallized and then dried to obtain a zwitterionic hydrophilic chain extender. Furthermore, the recrystallization temperature is slowly reduced at a rate of 2° C. per minute; the drying method is vacuum freeze drying using a MartinChrist freeze dryer.

[0109] Technical Solution 4

[0110] The preparation method of a zwitterionic hydrophilic chain extender comprises the following steps:

[0111] (1) dissolving triethanolamine and methylene disulfonate in ethanol, heating under reflux for 8 hours to obtain a primary product;

[0112] The molar ratio of the triethanolamine in step (1) to the methylene disulfonate is 1.6:1.

[0113] Meanwhile, ethanol is anhydrous ethanol; the amount of ethanol is 50 mL per mole of methylene disulfonate; the heating temperature is 80° C.; the reflux device in step (1) is a condenser, using an Allihn condenser,

[0114] (2) removing the unreacted triethanolamine and ethanol from the primary product in step (1) to obtain a purified product, then adding acetone to dissolve it, then adding ethyl lactoammonium naphthalene disulfonate, mixing it, adding ethanol, heating the reactor to react, and obtaining a secondary product; the removal method is vacuum distillation, the pressure is 2.0 kPa, and the equipment model name is Pilodist PD300CC; wherein the vacuum distillation method first distills out ethanol at 60° C., wherein the ethanol fraction receiving temperature is 40° C., and then gradually raising the temperature to 210° C. to distill out triethanolamine, wherein the triethanolamine fraction receiving temperature is 180° C.

[0115] The preparation method of the zwitterionic hydrophilic chain extender described above, the amount of acetone is 50mL per mol of methylene disulfonate; the amount of ethyl lactoammonium naphthalene disulfonate is 5mol per mol of methylene disulfonate; ethanol is an ethanol solution with a mass concentration of 60%; the amount of ethanol is 90mL per mol of methylene disulfonate; in the preparation method of the zwitterionic hydrophilic chain extender described above, the temperature of the reactor heating reaction is 140°C; the heating reaction time of the reactor is 12h.

[0116] (3) The secondary product in step (2) is recrystallized and then dried to obtain a zwitterionic hydrophilic chain extender. Furthermore, the recrystallization temperature is slowly reduced at a rate of 4° C. per minute; the drying method is vacuum freeze drying using a MartinChrist freeze dryer.

[0117] Technical Solution 5

[0118] The preparation method of a zwitterionic hydrophilic chain extender comprises the following steps:

[0119] (1) dissolving triethanolamine and methylene disulfonate in ethanol, heating under reflux for 7 hours to obtain a primary product; the molar ratio of triethanolamine to methylene disulfonate in step (1) is 1.4:1.

[0120] Meanwhile, the ethanol is anhydrous ethanol; the amount of ethanol used is 45 mL per mol of methylene disulfonate; the heating temperature is 74° C.; the reflux equipment in step (1) is a condenser, using an Allihn condenser.

[0121] (2) removing the unreacted triethanolamine and ethanol from the primary product in step (1) to obtain a purified product, then adding acetone to dissolve it, then adding ethyl lactoammonium naphthalene disulfonate, mixing it, adding ethanol, heating the reactor to react, and obtaining a secondary product; the removal method is vacuum distillation, the pressure is 1.7 kPa, and the equipment model name is Pilodist PD300CC; wherein the vacuum distillation method first distills out ethanol at 60° C., wherein the ethanol fraction receiving temperature is 40° C., and then gradually raising the temperature to 210° C. to distill out triethanolamine, wherein the triethanolamine fraction receiving temperature is 180° C.

[0122] The preparation method of the zwitterionic hydrophilic chain extender described above, the amount of acetone used is 40mL per mol of methylene disulfonate; the amount of ethyl lactoammonium naphthalene disulfonate used is 4mol per mol of methylene disulfonate; ethanol is an ethanol solution with a mass concentration of 60%; the amount of ethanol used is 70mL per mol of methylene disulfonate; in the preparation method of the zwitterionic hydrophilic chain extender described above, the temperature of the reactor heating reaction is 130°C; the heating reaction time of the reactor is 10h.

[0123] (3) The secondary product in step (2) is recrystallized and then dried to obtain a zwitterionic hydrophilic chain extender. Furthermore, the recrystallization temperature is slowly reduced at a rate of 3° C. per minute; the drying method is vacuum freeze drying using a MartinChrist freeze dryer.

[0124] Comparison plan 1

[0125] The preparation method of a zwitterionic hydrophilic chain extender comprises the following steps:

[0126] (1) dissolving triethanolamine and methylene disulfonate in ethanol, heating under reflux for 7 hours to obtain a primary product; the molar ratio of triethanolamine to methylene disulfonate in step (1) is 1.4:1.

[0127] Meanwhile, the ethanol is anhydrous ethanol; the amount of ethanol used is 45 mL per mol of methylene disulfonate; the heating temperature is 74° C.; the reflux equipment in step (1) is a condenser, using an Allihn condenser.

[0128] (2) removing the unreacted triethanolamine and ethanol in the primary product of step (1) to obtain a purified product, and then adding acetone to dissolve it to obtain a secondary product; the removal method is vacuum distillation, the pressure is 1.7 kPa, and the equipment model name is Pilodist PD300CC; wherein the vacuum distillation method first distills out ethanol at 60° C., wherein the ethanol fraction receiving temperature is 40° C., and then gradually increases the temperature to 210° C. to distill out triethanolamine, wherein the triethanolamine fraction receiving temperature is 180° C.

[0129] The above-mentioned preparation method of the zwitterionic hydrophilic chain extender, the amount of acetone is added to each mol of methylene disulfonate 40mL.

[0130] (3) The secondary product in step (2) is recrystallized and then dried to obtain a zwitterionic hydrophilic chain extender. Furthermore, the recrystallization temperature is slowly reduced at a rate of 3° C. per minute; the drying method is vacuum freeze drying using a MartinChrist freeze dryer.

[0131] Comparison plan 2

[0132] The preparation method of a zwitterionic hydrophilic chain extender comprises the following steps:

[0133] (1) dissolving N-methyldiethanolamine and methylene disulfonate in ethanol, heating under reflux for 7 hours to obtain a primary product; the molar ratio of the N-methyldiethanolamine to the methylene disulfonate in step (1) is 1.4:1.

[0134] Meanwhile, the ethanol is anhydrous ethanol; the amount of ethanol used is 45 mL per mol of methylene disulfonate; the heating temperature is 74° C.; the reflux equipment in step (1) is a condenser, using an Allihn condenser.

[0135] (2) removing the unreacted N-methyldiethanolamine and ethanol in the primary product of step (1) to obtain a purified product, then adding acetone to dissolve it, then adding ethyl lactoammonium naphthalene disulfonate, mixing it, adding ethanol, heating the reactor to react, and obtaining a secondary product; the removal method is vacuum distillation, the pressure is 1.7 kPa, and the equipment model name is Pilodist PD300CC; wherein the vacuum distillation method first distills out ethanol at 60° C., wherein the ethanol fraction receiving temperature is 40° C., and then gradually raising the temperature to 210° C. to distill out N-methyldiethanolamine, wherein the N-methyldiethanolamine fraction receiving temperature is 180° C.

[0136] The preparation method of the zwitterionic hydrophilic chain extender described above, the amount of acetone used is 40mL per mol of methylene disulfonate; the amount of ethyl lactoammonium naphthalene disulfonate used is 4mol per mol of methylene disulfonate; ethanol is an ethanol solution with a mass concentration of 60%; the amount of ethanol used is 70mL per mol of methylene disulfonate; in the preparation method of the zwitterionic hydrophilic chain extender described above, the temperature of the reactor heating reaction is 130°C; the heating reaction time of the reactor is 10h.

[0137] (3) The secondary product in step (2) is recrystallized and then dried to obtain a zwitterionic hydrophilic chain extender. Furthermore, the recrystallization temperature is slowly reduced at a rate of 3° C. per minute; the drying method is vacuum freeze drying using a MartinChrist freeze dryer.

[0138] Comparison plan 3

[0139] The preparation method of a zwitterionic hydrophilic chain extender comprises the following steps:

[0140] (1) dissolving triethanolamine and 1,3-propane sultone in ethanol, heating under reflux for 7 hours to obtain a primary product; the molar ratio of the triethanolamine to the 1,3-propane sultone in step (1) is 1.4:1.

[0141] Meanwhile, the ethanol is anhydrous ethanol; the amount of ethanol used is 45 mL per mole of 1,3-propane sultone; the heating temperature is 74° C.; the reflux equipment in step (1) is a condenser, and an Allihn condenser is used.

[0142] (2) removing the unreacted triethanolamine and ethanol from the primary product in step (1) to obtain a purified product, then adding acetone to dissolve it, then adding ethyl lactoammonium naphthalene disulfonate, mixing it, adding ethanol, heating the reactor to react, and obtaining a secondary product; the removal method is vacuum distillation, the pressure is 1.7 kPa, and the equipment model name is Pilodist PD300CC; wherein the vacuum distillation method first distills out ethanol at 60° C., wherein the ethanol fraction receiving temperature is 40° C., and then gradually raising the temperature to 210° C. to distill out triethanolamine, wherein the triethanolamine fraction receiving temperature is 180° C.

[0143] The preparation method of the zwitterionic hydrophilic chain extender described above, the amount of acetone is 40mL per mol of 1,3-propane sultone; the amount of ethyl lactammonium naphthalene disulfonate is 4mol per mol of 1,3-propane sultone; ethanol is an ethanol solution with a mass concentration of 60%; the amount of ethanol is 70mL per mol of 1,3-propane sultone; the preparation method of the zwitterionic hydrophilic chain extender described above, the temperature of the reactor heating reaction is 130°C; the heating reaction time of the reactor is 10h.

[0144] (3) The secondary product in step (2) is recrystallized and then dried to obtain a zwitterionic hydrophilic chain extender. Furthermore, the recrystallization temperature is slowly reduced at a rate of 3° C. per minute; the drying method is vacuum freeze drying using a MartinChrist freeze dryer.

[0145] Test plan

[0146] For technical solution 5, if Figure 1 , Figure 2 , Figure 3 and Figure 4 , the product of step (1) is shown in the above figure, and the reaction mechanism is as follows:

[0147] The primary hydroxyl group (-CH 2 -OH) reacts with methylene disulfonate to form an ester bond and release methanol molecules. If refluxed in ethanol solvent, the tertiary amine (-N<) on triethanolamine attacks the methylene (-CH 2 -), SN occurs 2 Nucleophilic substitution reaction forms a quaternary ammonium salt structure and releases a second molecule of methanol. The product molecule contains both quaternary ammonium cations and sulfonic acid anion groups, forming an inner salt type zwitterionic structure. The remaining hydroxyethyl groups give the molecule hydrophilicity. This zwitterionic hydrophilic chain extender can improve the surface activity and hydrolysis stability of polyurethane materials and is widely used in coatings, adhesives and other fields. The reaction also identified key groups through infrared spectroscopy. Preliminary laboratory results show that, for example, the C=O stretching vibration peak of the ester group (1736cm -1 ) and the CN stretching vibration peak of quaternary ammonium salt (~1203cm -1 )wait.

[0148] At the same time, the product information of the key step (2) is as follows Figure 5 , Figure 6 , Figure 7 and Figure 8As shown, the reaction process is as follows: the quaternary ammonium salt cation in the primary product O=S(=O)(O)CS(=O)(=O)OCCN(CCOC)CCOC undergoes an ion exchange reaction with the naphthalene disulfonic acid anion to generate a new zwitterionic compound. During the reaction, ethanol, as a solvent and proton donor, may undergo ester exchange or etherification reaction with the reactants, resulting in further changes in the product structure. In this structure, the naphthalene disulfonic acid anion is connected to the quaternary ammonium cation through an alkyl chain to form a new zwitterionic compound. At the same time, the original sulfonate and hydroxyl functional groups are retained. After analysis, the preliminary laboratory infrared spectrum, 3420cm -1 The broad peak in the range corresponds to the primary alcohol (-CH 2 OH) OH stretching vibration. 2800-3000cm -1 The multiple peaks in the range (2832, 2876, 2911, 2968) correspond to the stretching vibration of aliphatic CH, such as methylene (-CH 2 -) and methyl (-CH 3 ). 1730cm -1 The strong peaks on the left and right correspond to sulfonate esters (-SO 3 R) stretching vibration of the S=O double bond. The compound contains multiple sulfonate groups. 1625cm -1 The peaks around 1250cm correspond to the vibration of the aromatic ring skeleton, and the compound contains a naphthalene ring structure. -1 Multiple peaks in the range 950-1225cm correspond to the stretching vibration of CO single bonds (ether bonds and sulfonate bonds). -1 The multiple peaks in the range correspond to sulfonate (-SO 3 -) Symmetrical and asymmetric stretching vibrations of the S=O double bond in 650-900 cm -1 The peaks in the range correspond to the out-of-plane bending vibrations of aromatic CH and are related to the substitution pattern on the naphthalene ring.

[0149] The performance tests of comparative solutions 1-3 and technical solutions 1-5 are as follows:

[0150] Prepolymerization stage

[0151] 27.50 g HMDI, 66.00 g PPG2000, 0.08 g catalyst Bi8108, 13.50 g chain extender, 3.50 g NPG and 15 g acetone were added into the prepolymerization reactor.

[0152] Stirring was started, the temperature was raised to 80° C., and the mixture was kept warm for reaction for 4 hours to obtain a terminal isocyanate prepolymer.

[0153] Add 35 g of acetone, cool to room temperature, and transfer to a dispersion chain extension kettle.

[0154] Decentralized chain expansion stage

[0155] The dispersion chain extension kettle was started to stir, and 3.80 g of triethylamine was slowly added to carry out a neutralization reaction.

[0156] 220 g of deionized water was added to the neutralized prepolymer several times, and the water addition time was controlled within 10 minutes.

[0157] After the addition of water was complete, 3.60 g of IPDA was added and stirring was continued for 30 minutes.

[0158] The temperature was raised to 50°C and acetone was removed under reduced pressure until the acetone content in the system was less than 1%.

[0159] The obtained emulsion was cooled to room temperature to obtain a polyurethane water-based resin with a solid content of 30%.

[0160] Among the above, HMDI-hexamethylene diisocyanate;

[0161] PPG2000-polypropylene glycol 2000 (polypropylene glycol with a number average molecular weight of 2000);

[0162] Catalyst Bi8108-bismuth catalyst Bi8108;

[0163] Chain extender - the type is not specified, but commonly used ones include diol compounds such as ethylene glycol and 1,4-butanediol;

[0164] NPG-neopentyl glycol (chemical name is 2,2-dimethyl-1,3-propanediol);

[0165] Acetone - Acetone, a commonly used organic solvent;

[0166] Triethylamine - Triethylamine, a commonly used organic base;

[0167] Deionized water - Deionized water is treated by ion exchange or reverse osmosis to remove ionic impurities in the water;

[0168] IPDA-isophoronediamine (chemical name is 5-amino-1,3,3-trimethylcyclohexylamine).

[0169] The test results are shown in Table 1:

[0170] plan Solid content (%) Particle size (nm) Viscosity (mPa·s) Tensile strength(MPa) Elongation at break (%) Comparison plan 1 29.2 115 41 12.7 720 Comparison plan 2 30.5 125 52 10.4 650 Comparison plan 3 29.8 110 37 13.9 780 Technical Solution 1 30.2 89 25 18.2 980 Technical Solution 2 30.8 102 34 16.8 910 Technical Solution 3 29.5 95 29 17.9 950 Technical Solution 4 30.5 108 39 15.5 870 Technical Solution 5 30.1 92 27 19.7 1050

[0171] Compared with Scheme 1, the effect of removing ethyl lactoammonium naphthalene disulfonate can be analyzed from the following aspects:

[0172] 1. Formation of zwitterionic structure

[0173] Ethyl lactoammonium naphthalene disulfonate plays a key role in the synthesis of zwitterionic hydrophilic chain extenders. It provides sulfonic acid groups and combines with other reactants to form zwitterionic structures. This structure helps to improve the hydrophilicity and surface activity of polyurethane. If ethyl lactoammonium naphthalene disulfonate is removed, the formation of the zwitterionic structure may be incomplete, thus affecting the performance of the final product.

[0174] 2. Solubility and dispersibility

[0175] The zwitterionic structure can improve the solubility and dispersibility of polyurethane in water. The removal of ethyl lactammonium naphthalene disulfonate may lead to a decrease in the solubility and dispersibility of the product, affecting its stability and application effect in the aqueous system.

[0176] 3. Mechanical properties

[0177] The sulfonic acid groups introduced by ethyl ammonium naphthalene disulfonate can enhance the interaction between polyurethane chains through electrostatic action and improve the mechanical properties of the material. Removal of this component may lead to a decrease in mechanical properties such as tensile strength and elongation at break.

[0178] 4. Chemical stability

[0179] The sulfonic acid group can also improve the chemical stability of polyurethane, especially its hydrolysis resistance in a humid environment. Removal of ethyl lactammonium naphthalene disulfonate may reduce the chemical stability of the product, making it more susceptible to hydrolysis or degradation during use.

[0180] 5. Reaction efficiency and selectivity

[0181] The presence of ethyl lactoammonium naphthalene disulfonate may affect the efficiency and selectivity of the reaction, and the removal of this component may lead to incomplete reaction or increased side reactions, thereby affecting the purity and performance of the product.

[0182] In summary, the removal of ethyl lactammonium naphthalene disulfonate will have a significant impact on the structure and properties of zwitterionic hydrophilic chain extenders. In order to obtain waterborne polyurethane products with excellent performance, it is usually necessary to maintain or optimize the use of this ingredient.

[0183] Comparative Scheme 2: Triethanolamine is replaced with N-methyldiethanolamine. This change has the following effects on the reaction process and product properties:

[0184] Reduced reactivity

[0185] N-methyldiethanolamine is less basic than triethanolamine, which may result in its lower reactivity with methylene methanedisulfonate and ethyl choline ammonium naphthalene disulfonate. The lower reactivity may require longer reaction times or higher reaction temperatures to achieve equivalent conversions.

[0186] Increased steric hindrance

[0187] N-methyldiethanolamine has one more methyl group than triethanolamine, which increases the steric hindrance of the molecule. Larger steric hindrance may hinder the approach and collision of reactant molecules, further reducing the reaction rate. At the same time, steric hindrance may also affect the conformation and stacking of product molecules.

[0188] The number of hydrogen bonds decreases

[0189] N-methyldiethanolamine has one less hydroxyl group than triethanolamine, which means that the number of intermolecular and intramolecular hydrogen bonds is reduced. The reduction of hydrogen bonds may reduce the crystallinity of the product, thereby affecting its physical properties such as melting point and solubility.

[0190] Reduced hydrophilicity

[0191] The reduction in the number of hydroxyl groups will also lead to a decrease in the overall hydrophilicity of the product molecule, which may reduce its performance as a zwitterionic surfactant, such as solubilization ability and emulsification.

[0192] Product structure changes

[0193] The structure of zwitterionic surfactants synthesized using MDEA is different from that of products made from triethanolamine, and this structural change may affect their physical and chemical properties and practical application performance.

[0194] Changes in by-product types

[0195] Due to the different reaction sites and activities between MDEA and methylene methanedisulfonate, some by-products that are not present in the triethanolamine system may be generated, and these impurities may affect the purity of the product.

[0196] Comparative Scheme 3: methanedisulfonic acid methylene ester is replaced with 1,3-propane sultone. This change has the following effects on the reaction process and product performance:

[0197] Different reaction sites

[0198] Methylene disulfonate contains two sulfonate groups (-SO3CH3), while 1,3-propane sultone is a cyclic sulfonate. The former can react with triethanolamine at two sites, while the latter only has one cyclic sulfonate group involved in the reaction, which leads to differences in the structure of the reaction products.

[0199] Steric hindrance effect

[0200] 1,3-Propane sultone is a five-membered ring structure with large steric hindrance, which may affect its reactivity and selectivity with triethanolamine. The ring structure may also affect the conformation and stacking mode of the product molecule.

[0201] Hydrolytic stability

[0202] Cyclic sulfonates have better hydrolytic stability than non-cyclic sulfonates, so the use of 1,3-propane sultone may improve the hydrolytic resistance of the chain extender and its derived polyurethane products.

[0203] Product structure and properties

[0204] Due to the differences in reaction sites and raw material structures, the zwitterionic chain extender obtained using 1,3-propane sultone is structurally different from the product of methylene disulfonate. The connection mode between the sulfonic acid group and the alcohol hydroxyl group or quaternary ammonium salt has changed, which may affect its reactivity as a chain extender and the mechanical properties and hydrophilicity of the polyurethane product.

[0205] Security considerations

[0206] 1,3-Propane sultone has certain toxicity and carcinogenicity, so special attention should be paid to protection when using it, and it should be operated in a fume hood as much as possible. In comparison, methylene disulfonate has lower toxicity and risk.

[0207] Cost Difference

[0208] The price of 1,3-propane sultone may be higher than that of methylene disulfonate, and cost factors need to be considered when using it, but if the performance improvement it brings can offset the cost increase, it still has application value.

[0209] In summary, the use of 1,3-propane sultone to replace methylene disulfonate will have a certain impact on the synthesis route, product structure and properties. According to the test results, the performance of Comparative Scheme 3 is slightly better than that of Comparative Scheme 2, but it is still inferior to the technical scheme using methylene disulfonate.

[0210] This suggests that when designing zwitterionic chain extenders, the introduction of different raw materials and structural units will significantly change the properties of the product; the selection of suitable sulfonate reagents requires comprehensive consideration of factors such as reaction activity, product stability, safety and cost; through systematic experimental optimization and performance evaluation, it is expected to obtain zwitterionic chain extenders with novel structures and excellent performance, providing more possibilities for the modification of polyurethane materials.

[0211] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0212] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a zwitterionic hydrophilic chain extender, characterized in that: The following steps are involved: (1) dissolving triethanolamine and methylene disulfonate in ethanol, heating under reflux for 6-8 hours to obtain a primary product; (2) removing unreacted triethanolamine and ethanol from the primary product in step (1) to obtain a purified product, then adding acetone to dissolve it, adding ethyl lactammonium naphthalene disulfonate, mixing well, adding ethanol, and heating the reactor to react to obtain a secondary product; (3) The secondary product in step (2) is recrystallized and then dried to obtain a zwitterionic hydrophilic chain extender.

2. The method for preparing the zwitterionic hydrophilic chain extender according to claim 1, characterized in that: The molar ratio of the triethanolamine in step (1) to the methylene disulfonate is (1.0-2.0):

1.

3. The method for preparing the zwitterionic hydrophilic chain extender according to claim 2, characterized in that: The molar ratio of the triethanolamine in step (1) to the methylene disulfonate is (1.3-1.6):

1.

4. The method for preparing the zwitterionic hydrophilic chain extender according to claim 3, characterized in that: The molar ratio of the triethanolamine in step (1) to the methylene disulfonate is 1.4:

1.

5. The method for preparing the zwitterionic hydrophilic chain extender according to claim 4, characterized in that: In step (1), the ethanol is anhydrous ethanol; In step (1), the amount of ethanol is 40 mL to 50 mL per mole of methylene disulfonate; The heating temperature in step (1) is 65°C-80°C; The reflux equipment in step (1) is a condenser.

6. The method for preparing the zwitterionic hydrophilic chain extender according to claim 5, characterized in that: The removal method in step (1) is vacuum distillation at a pressure of 1.3-2.0 kPa; In the reduced pressure distillation method, ethanol is first distilled off at 60°C, wherein the receiving temperature of the ethanol fraction is 40°C, and then the temperature is gradually increased to 210°C to distill off triethanolamine, wherein the receiving temperature of the triethanolamine fraction is 180°C.

7. The method for preparing the zwitterionic hydrophilic chain extender according to claim 6, characterized in that: In step (2), the amount of acetone is 30 mL to 50 mL per mol of methylene disulfonate; In step (2), the amount of ethyl lactoammonium naphthalene disulfonate used is 2 mol to 5 mol per mol of methylene methane disulfonate.

8. The method for preparing the zwitterionic hydrophilic chain extender according to claim 7, characterized in that: In step (2), the ethanol is an ethanol solution with a mass concentration of 60%; The amount of ethanol used in step (2) is 60 mL to 90 mL per mol of methylene disulfonate.

9. The method for preparing the zwitterionic hydrophilic chain extender according to claim 8, characterized in that: The temperature of heating the reaction kettle in step (2) is 120-140°C; The heating reaction time of the reactor in step (2) is 6h-12h.

10. The method for preparing the zwitterionic hydrophilic chain extender according to claim 9, characterized in that: The rate of slowly reducing the temperature of the recrystallization in step (3) is 2°C-4°C per minute; The drying method in step (3) is vacuum freeze drying.

Citation Information

Patent Citations

  • Zwitterionic hydrophilic chain extender and preparation method thereof

    CN103665291A

  • Zwitterionic polyester diol and preparation method thereof

    CN104262597A

  • Preparation method of zwitterionic waterborne polyurethane

    CN104371085A