Thermoplastic polyurethane elastomer with low internal heat generation as well as preparation method and application of thermoplastic polyurethane elastomer
The thermoplastic polyurethane elastomer is constructed by using a combination of polyols, diisocyanate and 1-benzylpiperidine-derived diol chain extenders, and the high endogenous heat and processing of thermoplastic polyurethane elastomers in high-speed operation and long-term fatigue applications are solved. The problem of instability has achieved a combination of low endogenous heat and high heat resistance, and is suitable for high-speed bicycle inner tubes and other fields.
Patent Information
- Application Number
- CN202411291980.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-14
AI Technical Summary
The existing thermoplastic polyurethane elastomers have problems such as high endogenous heat, thermal stress concentration and unstable processing in high-speed operation and long-term fatigue application scenarios, making it difficult to meet the needs of applications such as high-speed bicycle inner tubes.
The linear polyol is adopted by a combination of 40-70 parts of polyol, 20-50 parts of diisocyanate, 3-25 parts of small molecule glycol chain extender and 0.1-5 parts of 1-benzylpiperidine-derived diol chain extender. Construct the soft segment and introduce large-volume side-based chain extender to improve the rigidity of the hard segment and the thermodynamic compatibility of the soft and hard segments, and reduce endogenous heat.
It achieves low endogenous heat, improves the heat resistance and processing stability of the material, enhances the tensile strength and tear strength of the material, reduces the surface defects of the extruded product, and extends the service life.
Smart Images

Figure BDA0005044875170000051 
Figure BDA0005044875170000052 
Figure BDA0005044875170000062
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane, and in particular relates to a thermoplastic polyurethane elastomer with low endogenous heat, a preparation method and application thereof. Background Art
[0002] Thermoplastic polyurethane elastomer (TPU) is a comprehensive material composed of thermodynamically incompatible soft segments and hard segments with excellent properties such as high strength, high toughness, and high elasticity. TPU can be prepared into a variety of products such as pipes, films, complex molded bodies, etc. through a variety of melt processing methods, such as injection molding and extrusion, and can be widely used in various industries.
[0003] Various high-speed applications and long-term fatigue application scenarios have gradually increased the demand for materials to resist endogenous heat. For example, the inflatable inner tube of a high-speed bicycle needs to maintain low endogenous heat, sufficient strength and airtightness under different and constantly changing frequencies.
[0004] Patent CN113583432A discloses a technology for preparing low endogenous heat polyurethane, which uses terminal hydroxyl polybutadiene to react with polyester polyol and diisocyanate, adjusts the molecular structure to reduce endogenous heat, and introduces Al2O3 modified by silane coupling agent to improve wear resistance. However, the olefin monomer used in this method has the phenomenon of heat aging cross-linking in this application scenario, and thermal stress concentration will occur during subsequent use, greatly reducing the service life and safety. Patent CN111961186A selects diisocyanates and polyols with relatively high molecular rigidity, regularity and symmetry to react, and introduces inorganic fillers to improve the heat resistance of the elastomer and reduce endogenous heat. It belongs to the field of modification and cannot effectively improve the low endogenous heat level of the main structure.
[0005] Patent CN110951034B proposes a technology for preparing high-load-bearing and low-endogenous heat polyurethane elastomers. Through polymethylene polyphenyl polyisocyanate and 1,2,6-hexanetriol, the regularity of the elastomer structure is reduced to reduce endogenous heat, and the cross-linking degree of the material is increased to increase the load strength of the material. However, the polyurethane prepared by this method has high processing temperature, unstable extrusion, and local defects, which makes it difficult to adapt to the processing and application of extruded products.
[0006] Therefore, a new solution needs to be proposed to solve the above problems. Summary of the invention
[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide a thermoplastic polyurethane elastomer with excellent low intrinsic heat, which can be used for extrusion processing and has a long-term low intrinsic heat effect.
[0008] In a first aspect, the present invention provides a thermoplastic polyurethane elastomer with low endogenous heat, which is prepared by using raw materials comprising the following parts by weight:
[0009] 40-70 parts of polyol;
[0010] 20-50 parts of diisocyanate;
[0011] 3-25 parts of small molecule diol chain extender;
[0012] 0.1-5 parts of 1-benzylpiperidine derived diol chain extender, for example, 0.1, 0.5, 1, 2, 3, 4, 5 parts, preferably 0.4-4 parts.
[0013] In the thermoplastic polyurethane elastomer of the present invention, the polyol is selected from at least one of polyester polyol, polyether polyol, polycaprolactone polyol and polycarbonate polyol, and the number average molecular weight of the polyol is preferably 600-4000 g / mol, preferably 1000-2500 g / mol.
[0014] The polyester polyol is a linear polymer polyol prepared by a commonly used synthesis method in the industry, and is prepared from a dibasic acid and a diol; wherein the dibasic acid is one or more of succinic acid, adipic acid, and sebacic acid, and the diol is one or more of ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and diethylene glycol; preferably, the polyester polyol is one or more of polybutylene adipate and polyhexanediol adipate;
[0015] The polyether polyol is prepared by ring-opening polymerization of an epoxy compound containing an active hydrogen compound as an initiator; wherein the active hydrogen compound is selected from one or more of ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, and dipropylene glycol; wherein the epoxy compound is selected from one or more of propylene oxide, tetrahydrofuran, and ethylene oxide; preferably, the polyether polyol is polytetramethylene ether glycol;
[0016] The polycaprolactone polyol is prepared by ring-opening polymerization of ε-caprolactone monomer and an initiator, wherein the initiator is one or more of 1,4-butanediol, 1,6-hexanediol, diethylene glycol, and ethylene glycol; preferably, the initiator is 1,4-butanediol;
[0017] The polycarbonate polyol is prepared by transesterification of a small molecule diol and a small molecule carbonate; wherein the small molecule diol is one or more of 1,6-hexanediol, 1,4-butanediol, 1,4-cyclohexanedimethanol, 1,5-pentanediol, and 3-methylpentanediol; the small molecule carbonate is one or more of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, diphenyl carbonate, ethylene carbonate, or propylene carbonate; more preferably, the small molecule carbonate is dimethyl carbonate;
[0018] The diisocyanate is one or more of aromatic diisocyanate, aliphatic diisocyanate and alicyclic diisocyanate, preferably aromatic diisocyanate, more preferably one or more of diphenylmethane diisocyanate, xylylene diisocyanate, 3,3'-dimethyl-4,4'-biphenyl diisocyanate and 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate;
[0019] In the thermoplastic polyurethane elastomer of the present invention, the small molecule diol chain extender is an aliphatic diol or an aromatic diol, preferably one or more selected from ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, methyl propanediol, 1,4-cyclohexanediol, and terephthalic acid.
[0020] In the thermoplastic polyurethane elastomer of the present invention, the 1-benzylpiperidine-derived diol chain extender has the following structure:
[0021] or its enantiomer
[0022] In a specific embodiment, the thermoplastic polyurethane elastomer may be optionally added with additives such as antioxidants, light stabilizers, ultraviolet absorbers, lubricants, and hydrolysis resistance agents according to actual needs;
[0023] In another specific embodiment, during the preparation process of the thermoplastic polyurethane elastomer, any one of organic tin, organic bismuth, organic potassium, organic zinc and their combinations can be selectively added as polymerization catalysts.
[0024] In a second aspect, the present invention provides a method for preparing the above-mentioned thermoplastic polyurethane elastomer, characterized in that it comprises the following preparation steps:
[0025] 1) Mixing polyol, arbitrary auxiliary agent and 1-benzylpiperidine derived diol chain extender, stirring evenly, the mixing temperature is 50-120° C., preferably 80-110° C.;
[0026] 2) The mixture obtained in 1) is sent to a kneader in proportion with diisocyanate, a small molecule diol chain extender and an optional catalyst, and then sent to a twin-screw extruder for uniform mixing. After reaction extrusion, underwater pelletizing and drying, a thermoplastic polyurethane elastomer is obtained.
[0027] The extrusion temperature is 120-280°C. In view of the fact that the extruder temperature zones cannot be infinite, the specific temperature setting can be a single or repeated point value of 120°C, 150°C, 180°C, 200°C or 220°C. The preferred temperature range is 160°C-200°C.
[0028] The third aspect of the present invention provides the application of the thermoplastic polyurethane elastomer in the fields of pneumatic inner tubes, conveyor belts, pipes, etc.
[0029] The beneficial effects of the present invention are:
[0030] The invention adopts linear polyol to construct the soft segment, thereby ensuring the molding performance and heat resistance of the elastomer. A 1-benzylpiperidine-derived diol chain extender containing a large-volume side group is introduced into the chain extender, and the steric hindrance effect thereof improves the rigidity of the hard segment, improves the heat resistance of the material, and destroys the overall regularity of the hardness to a certain extent, thereby improving the thermodynamic compatibility of the soft and hard segments and reducing the internal heat generated by the soft and hard phases under high-frequency friction. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with examples. The experimental conditions of the present invention can be adjusted accordingly as needed and are not limited to the experimental conditions of this embodiment.
[0032] Unless otherwise specified, the raw materials used in the practice of the present invention are all commercially available conventional products.
[0033] The raw materials used are as follows:
[0034] (A) Polyols:
[0035] PBA (polybutylene adipate glycol), molecular weight 2000 g / mol, Wanhua Chemical Group Co., Ltd.;
[0036] PTMG (polytetramethylene ether glycol), molecular weight 1000 g / mol, Wanhua Chemical Group Co., Ltd.;
[0037] BG-PCL (butanediol-initiated polycaprolactone diol), molecular weight 2000 g / mol, Wanhua Chemical Group Co., Ltd.;
[0038] PCDL (polycarbonate diol, HD200), molecular weight 2000 g / mol, Wanhua Chemical Group Co., Ltd.;
[0039] (B) Diisocyanate:
[0040] MDI (diphenylmethane diisocyanate), Wanhua Chemical Group Co., Ltd.;
[0041] (C) Small molecule diol chain extender:
[0042] BDO (1,4-butanediol), Wanhua Chemical Group Co., Ltd.;
[0043] (D) Synthetic raw materials involved in the 1-benzylpiperidine derived diol chain extender: (5-ethynyl-2,2-dimethyl-1,3-dioxolane-4-)methanol, Aurora; methanesulfonyl chloride, N-(trimethylsilylmethyl)benzylamine, 1,4-dicyanophthalic acid, dichloromethane, potassium carbonate, tetrabutylammonium iodide, acetonitrile, 1,4-naphthalene dinitrile, isopropanol, N-methylmorpholine N-oxide, osmium tetroxide, tert-butyl alcohol, triethylamine, tetrabutylammonium iodide, ethyl acetate, TCI;
[0044] A typical synthesis method of the 1-benzylpiperidine-derived diol chain extender in the present invention can refer to the preparation method described in "Synthesis of polyhydroxy piperidines and their analogues: a novel approach toward selective inhibitors of α-glucosidase", Organic & Biomolecular Chemistry, and is prepared by the following steps: 1) Under an argon atmosphere at 0°C, methanesulfonyl chloride (3.82 mL, 49.35 mmol) is added dropwise to a solution of (5-ethynyl-2,2-dimethyl-1,3-dioxolane-4-)methanol (7.0 g, 44.87 mmol) and triethylamine (6.87 mL, 49.35 mmol) in dichloromethane (100 mL) , and extract product a after heating and stirring for 5 hours; 2) dissolving product a and N-(trimethylsilylmethyl)benzylamine in acetonitrile solution, reflux with anhydrous potassium carbonate and tetrabutylammonium iodide as catalyst, and extracting product b with ethyl acetate; 3) product b and 1,4-dicyanophthalic acid are irradiated with infrared rays to generate product c; 4) N-methylmorpholine N-oxide (50% aqueous solution) and osmium tetroxide are added to the tert-butanol suspension of product c in a volume ratio of 1.2:1, and after stirring at room temperature for 24 hours, 1-benzylpiperidine-derived diol chain extender is obtained by reduced pressure distillation.
[0045] The above-mentioned synthesis route of the 1-benzylpiperidine-derived diol chain extender is only a typical route in the prior art. With technological breakthroughs, the selection of the chain extender is not limited to the products of this synthesis route.
[0046] The raw materials used in the present invention are all added to the reaction system in parts by weight.
[0047] Example 1
[0048] A thermoplastic polyurethane elastomer with low endogenous heat, wherein the raw materials for its preparation include the following components by mass: 233 parts of PBA, 100 parts of diphenylmethane diisocyanate, 25 parts of 1,4-butanediol, and 1.8 parts of 1-benzylpiperidine-derived diol chain extender. The 1-benzylpiperidine-derived diol chain extender and the polyol are mixed evenly in a storage tank, and then the components are mixed evenly in a kneader and sent to a twin-screw extruder. After reaction extrusion, underwater pelletizing, and drying, thermoplastic polyurethane elastomer particles are obtained, wherein the extrusion temperature is set to 185°C.
[0049] Embodiment 2-6
[0050] The formulations of Examples 2-6 are shown in Table 1, and the preparation methods are the same as those of Example 1.
[0051] Comparative Example 1
[0052] A thermoplastic polyurethane elastomer, wherein the raw materials for its preparation include the following components by mass: 214 parts of PBA, 100 parts of diphenylmethane diisocyanate, and 26.4 parts of 1,4-butanediol. The components are mixed evenly in a kneader, and sent to a twin-screw extruder, and thermoplastic polyurethane elastomer particles are obtained after reaction extrusion, underwater pelletizing, and drying, wherein the extrusion temperature is set to 185°C.
[0053] Comparative Examples 2-4
[0054] The formulations of Comparative Examples 2-4 are shown in Table 1, and the preparation methods are the same as those of Comparative Example 1.
[0055] Table 1 Composition of thermoplastic polyurethane elastomer
[0056]
[0057] The thermoplastic polyurethane elastomers in Examples 1-6 and Comparative Examples 1-4 were tested for mechanical properties. The hardness test standard was ASTM D2240-15, the tensile strength test standard was ASTM D412-16, and the tear strength test standard was ASTM D624-00.
[0058] Table 2 Performance test results
[0059]
[0060]
[0061] It can be seen from the test data in Table 2 that, compared with the corresponding comparative examples 1-4, the tensile strength and tear strength of Examples 1-6 are improved while the hardness is controlled to be consistent to the maximum extent, and the elongation at break is not significantly attenuated, that is, after the introduction of the 1-benzylpiperidine-derived diol chain extender, the material has a stronger ability to resist tension during the stress-stretching process, and can withstand greater tensile stress under the same deformation.
[0062] Endogenous heat test method:
[0063] DMA tests were performed on 0.2 mm thick film strips extruded from the elastomers of Examples 1-6 and Comparative Examples 1-4 to study the endogenous heat behavior. The test conditions used a Mettler SDTA861e dynamic mechanical thermoanalyzer set at 100 Hz, tensile mode, and a temperature scan at -50°C-120°C.
[0064] Extrusion performance evaluation method:
[0065] According to the product flow characteristics, set appropriate extrusion parameters and conduct film extrusion test. When the extruded film is stable, randomly take a section of film about 30 cm long and 5 cm wide, and grade the extruded film according to the film appearance grading standard. The film grading standard is as follows:
[0066] Level 1: The film is bright and smooth, with uniform width and thickness, and no obvious gel point within the observation range.
[0067] Level 2: The film is flat, with uniform width and thickness, no large or medium gel points, and the number of gel points in a small observation range is less than 10.
[0068] Level 3: The film is extruded smoothly, without large gel points, with less than or equal to 10 medium gel points within the observation range, or less than or equal to 2 small gel points per square centimeter.
[0069] Large gel point: The area embedded in the extruded film is greater than 0.01mm 2 The crystal point;
[0070] Medium gel point: The area embedded in the extruded film is greater than 0.001mm 2 And less than or equal to 0.01mm 2 The crystal point;
[0071] Small gel point: The area embedded in the extruded film is less than 0.001mm 2 The crystal point;
[0072] The test results of the perfection of the extruded products are included in Tables 3 and 4.
[0073] Table 3 Performance test results of the embodiment
[0074]
[0075] Table 4 Comparative Example Performance Test Results
[0076]
[0077]
[0078] It can be seen from the test data in Tables 3 and 4 that, compared with Comparative Examples 1-4, Examples 1-6 of the present invention have lower loss tangent values tanδ, and less endogenous heat during use. In addition, the extrusion grade of the products in each case after film drawing was determined to be grade three, and Examples 1-6 had fewer gel point defects on the surface of the film strips extruded compared with Comparative Examples 1-4. This shows that the introduction of 1-benzylpiperidine-derived diol chain extender can not only improve the strength of the material, adapt to higher tension environments, but also reduce endogenous heat, and at the same time improve the surface defects of the product, ensure good extrusion effects, and obtain reliable stability in use.
[0079] The applicant declares that the above is only a preferred example of the present invention, and the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement or modification based on the principle of the present invention falls within the protection scope and disclosure scope of the present invention.
Claims
1. A thermoplastic polyurethane elastomer with low endogenous heat, characterized in that: The method is prepared by using the following raw materials in parts by weight: 40-70 parts of polyol; 20-50 parts of diisocyanate; 3-25 parts of small molecule diol chain extender; 0.1-5 parts of 1-benzylpiperidine derived diol chain extender.
2. The thermoplastic polyurethane elastomer according to claim 1, characterized in that The polyol has a number average molecular weight of 600-4000 g / mol, preferably 1000-2500 g / mol.
3. The thermoplastic polyurethane elastomer according to any one of claims 1-2, characterized in that The polyol is selected from at least one of polyester polyol, polyether polyol, polycaprolactone polyol and polycarbonate polyol; Preferably, the polyester polyol is a linear polymer polyol, which is prepared from a dibasic acid and a diol; wherein the dibasic acid is selected from one or more of succinic acid, adipic acid, and sebacic acid, and the diol is selected from one or more of ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and diethylene glycol; more preferably, it is one or more of polybutylene adipate and polyhexanediol adipate; Preferably, the polyether polyol is prepared by ring-opening polymerization of an epoxy compound containing an active hydrogen compound as an initiator; wherein the active hydrogen compound is selected from one or more of ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, and dipropylene glycol; the epoxy compound is selected from one or more of propylene oxide, tetrahydrofuran, and ethylene oxide; more preferably, the polyether polyol is polytetramethylene ether glycol; Preferably, the polycaprolactone polyol is prepared by ring-opening polymerization of ε-caprolactone monomer and an initiator, wherein the initiator is selected from one or more of 1,4-butanediol, 1,6-hexanediol, diethylene glycol, and ethylene glycol; Preferably, the polycarbonate polyol is prepared by an ester exchange reaction between a small molecule diol and a small molecule carbonate; wherein the small molecule diol is selected from one or more of 1,6-hexanediol, 1,4-butanediol, 1,4-cyclohexanedimethanol, 1,5-pentanediol, and 3-methylpentanediol; and the small molecule carbonate is selected from one or more of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, diphenyl carbonate, ethylene carbonate, or propylene carbonate.
4. The thermoplastic polyurethane elastomer according to any one of claims 1 to 3, characterized in that The diisocyanate is one or more of aromatic diisocyanate, aliphatic diisocyanate and alicyclic diisocyanate, preferably aromatic diisocyanate, more preferably one or more of diphenylmethane diisocyanate, xylylene diisocyanate, 3,3'-dimethyl-4,4'-biphenyl diisocyanate and 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate.
5. The thermoplastic polyurethane elastomer according to claim 1, characterized in that: The small molecule diol chain extender is an aliphatic diol or an aromatic diol, preferably one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, methyl propanediol, 1,4-cyclohexanediol and 1,4-diol.
6. The thermoplastic polyurethane elastomer according to any one of claims 1 to 5, characterized in that The 1-benzylpiperidine-derived diol chain extender has the following structure: or its enantiomer 7. The thermoplastic polyurethane elastomer according to any one of claims 1 to 6, characterized in that The thermoplastic polyurethane elastomer also includes one or more of an antioxidant, a light stabilizer, a UV absorber, a lubricant, and a hydrolysis resistance agent.
8. The thermoplastic polyurethane elastomer according to any one of claims 1 to 7, characterized in that The thermoplastic polyurethane elastomer also includes a catalyst, and the catalyst is selected from any one or more of organic tin, organic bismuth, organic potassium and organic zinc.
9. A method for preparing a thermoplastic polyurethane elastomer according to any one of claims 1 to 8, characterized in that: The following steps are involved: The polyol, optional auxiliary agent, and 1-benzylpiperidine derived diol chain extender are mixed; then, the polyol, diisocyanate, small molecule diol chain extender and optional catalyst are sent to a kneader and a twin-screw extruder for mixing, extrusion, underwater pelletization and drying to obtain a thermoplastic polyurethane elastomer; preferably, the extrusion temperature is 120°C-280°C.
10. Use of the thermoplastic polyurethane elastomer according to any one of claims 1 to 8 or the thermoplastic polyurethane elastomer prepared by the preparation method according to claim 9 in the fields of pneumatic inner tubes, conveyor belts and pipes.
Citation Information
Patent Citations
TPU material with high wear resistance and low internal heat generation and preparation method thereof
CN113583432A
High-strength wear-resistant thermoplastic polyurethane elastomer as well as preparation method and application thereof
CN117801214A
Polyurethane forklift wheel material with high environmental adaptability and preparation method thereof
CN118440289A
Polyoxazolidone adhesive resin compoistion prepared from polyepoxides and polyisocyanates
CN1333791A
Block polyisocyanate composition and coating composition containing this
JP2011231306A