Waterproof and wear-resistant epoxy coating for leather as well as preparation process and application of waterproof and wear-resistant epoxy coating
By combining NPEL-128 and NPEL-128S and using soft and hard polymers in epoxy resin coatings, the lack of flexibility and poor wear resistance in leather finishing is solved. Problem, high-performance waterproof and wear-resistant coatings are realized, suitable for rapid production and low-temperature use.
Patent Information
- Application Number
- CN202411193508.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-28
AI Technical Summary
Existing epoxy resin coatings have problems such as insufficient flexibility, poor water resistance and wear resistance in leather finishing, and the curing process is not suitable for rapid production.
Using the combination of NPEL-128 and NPEL-128S epoxy resins, combined with soft and hard polymers and modified fillers, waterproof and wear-resistant epoxy coatings are prepared through specific mixing and reaction steps to improve the cross-linking of the coatings. Density and three-dimensional network structure to increase the wear resistance and flexibility of the paint.
It realizes excellent waterproof and wear resistance of epoxy coatings, improves its tensile strength and fold resistance, and achieves rapid curing under low temperature conditions, making it suitable for rapid repair and winter use.
Smart Images

Figure BDA0005015724560000121 
Figure BDA0005015724560000131
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and in particular relates to a waterproof and wear-resistant epoxy coating for leather, a preparation process and an application thereof. Background Art
[0002] Leather finishing is a key step in the leather manufacturing process, which involves various physical and chemical treatments of leather to improve its appearance, feel and functional properties. The purpose of leather finishing is to make the leather more beautiful and durable, and to give it specific properties such as water resistance, oil resistance, stain resistance, softness, gloss, etc. Leather coating is a special coating that is mainly used for the surface treatment of leather products to enhance their wear resistance, water resistance and aesthetics. This coating is mainly composed of resin, curing agent and some additives. When it is applied to the leather and cured, it forms a tough protective film.
[0003] Epoxy resin coating is a commonly used leather finishing product that can firmly adhere to the leather surface to form a durable protective layer. However, epoxy resin coating also has some disadvantages in leather finishing applications: (1) Flexibility issues: Compared with the natural elasticity of leather, epoxy resin coatings may be relatively hard, causing the leather to lose its original softness and comfort. (2) Waterproof and wear resistance: Epoxy resin coatings may affect the wear resistance of leather and have poor waterproof properties, which is a disadvantage for leather products that need to maintain their service life (such as shoes). (3) Curing process: Epoxy resin needs to be mixed with a curing agent and takes a certain amount of time to cure. This process may not be suitable for the fast-production leather products industry.
[0004] The paint on the surface of leather shoes is mainly to improve and protect the leather surface, enhance the appearance and durability of the shoes. The paint can make the color of the leather shoes more vivid and uniform, achieving the visual effect that the designer wants. At the same time, the paint can give the leather shoes a glossy feel. For example, patent leather shoes obtain high gloss by coating with resin paint. The paint forms a protective film that prevents moisture and stains from penetrating into the leather and prolongs the life of the leather shoes. The paint can enhance the wear resistance of the leather and reduce scratches and wear during daily use. At the same time, the paint can be used to cover up small flaws on the leather surface, such as scratches, spots, etc., which helps to maintain the shape and structure of the leather and prevent deformation.
[0005] Therefore, there is an urgent need for an epoxy coating that is waterproof, wear-resistant and flexible, which is of great significance for the production and development of leather products. Summary of the invention
[0006] The purpose of the present invention is to provide a waterproof and wear-resistant epoxy coating for leather and a preparation process and application thereof.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] A preparation process of a waterproof and wear-resistant epoxy coating for leather comprises the following steps:
[0009] (1) Weigh the raw materials by mass: 13-17 parts of modified filler, 50-55 parts of epoxy resin, 15-20 parts of polymer, 40-45 parts of polythiol curing agent, 0.2-0.4 parts of antioxidant, 0.1-0.3 parts of defoaming agent, 0.3-0.5 parts of dispersant and 0.2-0.5 parts of leveling agent;
[0010] The epoxy resin is a mixture of NPEL-128 epoxy resin and NPEL-128S epoxy resin in a mass ratio of 2.4-2.8:1;
[0011] The preparation method of the polymer is as follows: by weight:
[0012] Step 1: dissolving 400-420 parts of isophorone diisocyanate in 1500 parts of N-methylpyrrolidone, heating to 52-55° C., adding 1200-1250 parts of polypropylene glycol, and reacting at 52-55° C. for 3-5 hours to obtain an isocyanate-terminated first intermediate;
[0013] Step 2: dissolving 400-420 parts of diaminodiphenylmethane in 900 parts of N-methylpyrrolidone, heating to 52-55° C., adding 180-200 parts of toluene diisocyanate, and reacting at 52-55° C. for 3-5 hours to obtain an amino-terminated second intermediate;
[0014] Step 3: Add 1450-1480 parts of the first intermediate to 750-770 parts of the second intermediate, mix well, and react at 80-84° C. for 3-4 hours to obtain a polymer;
[0015] (2) performing a first mixing of the epoxy resin, the polymer and the modified filler to obtain a first mixture;
[0016] (3) adding an antioxidant, a defoaming agent, a dispersant, and a leveling agent to the first mixture in sequence, and performing a second mixing to obtain a second mixture;
[0017] (4) The second mixture is mixed with a polythiol curing agent to obtain a waterproof and wear-resistant epoxy coating for leather.
[0018] NPEL-128 epoxy resin and NPEL-128S epoxy resin were purchased from Nan Ya Plastics Industrial Co., Ltd.
[0019] Nan Ya Plastics Industry Co., Ltd.'s model NPEL-128 epoxy resin is a liquid epoxy resin generated by the reaction of bisphenol A and epoxy chloride. It is a resin commonly used in leather coatings. Leather shoes will inevitably be rubbed and bumped during daily wear, and the high wear resistance of the coating helps to maintain the beauty of the upper. However, the wear resistance of the NPEL-128 epoxy resin coating is not ideal. The present invention compounds the NPEL-128 epoxy resin with the NPEL-128S epoxy resin and a polymer to improve the wear resistance of the coating. Analysis shows that the mixing of resins with different epoxy equivalents can adjust the cross-linking density of the final cured product, thereby improving the wear resistance of the coating. At the same time, the polymer combined with soft and hard segments is added to the epoxy resin, which can improve the cross-linking network structure of the epoxy resin and form a more complex three-dimensional network. This network structure can better resist wear. The inventor also found that under this condition, the tensile strength of the epoxy coating is improved.
[0020] Furthermore, the preparation method of the modified filler is:
[0021] (1) calcining a mixed filler at a temperature of 800-900° C. for 40-60 minutes to obtain a calcined mixed filler; the mixed filler is a mixture of nano samarium oxide, boron nitride and organic bentonite in a mass ratio of 1:0.2-0.6:1.2-1.5;
[0022] (2) crushing the calcined mixed filler and grinding it into 80-100 mesh mixed filler powder;
[0023] (3) Mixing a mixed filler powder, tetramethylammonium bromide and ethanol aqueous solution in a mass ratio of 10:1-1.2:80-100, stirring evenly, heating at a temperature of 55-60° C. for 3-5 hours, filtering, and drying to obtain a modified mixed filler.
[0024] Furthermore, the mass percentage concentration of the ethanol aqueous solution is 65-70%.
[0025] The inventors found that after adding polymers to the coating system, when the upper of leather shoes is bent during wearing, cracks are more likely to form at the creases. These cracks not only affect the appearance, but also gradually expand, causing greater damage. The analysis is that the ratio of soft and hard segments in the coating affects the elasticity of the coating, which cannot adapt to the bending and stretching of the leather during wearing or use. The inventors tried to add mixed fillers to improve the folding resistance of epoxy coatings, but the effect was not ideal. Through a large number of experiments, it was found that the present invention can improve the folding resistance of epoxy coatings by modifying the mixed fillers. The analysis is that the mixed filler modified with tetramethylammonium bromide is hydrophobic, which can improve its dispersibility in the organic matrix, thereby forming a more uniform distribution in the epoxy resin and the polymer. The layered structure of the mixed filler can expand after modification, allowing epoxy resin and polymer molecules to be inserted between layers, which can increase the flexibility of the coating without sacrificing strength. At the same time, under this condition, the water resistance and thermal storage stability of the coating are improved.
[0026] Furthermore, the polythiol curing agent is GLC-905 polythiol curing agent purchased from Shandong Suihua Biotechnology Co., Ltd.
[0027] After the polythiol curing agent is mixed with the epoxy resin, the present invention can achieve rapid gel curing at low temperature and with a thinner coating, and has obvious advantages over other curing agents in rapid repair, winter and low-temperature working situations.
[0028] Furthermore, the antioxidant is selected from at least one of antioxidant 1010, antioxidant 168, antioxidant BHT, and antioxidant 330.
[0029] Furthermore, the defoaming agent is selected from at least one of TEGO901W defoaming agent, TEGO902W defoaming agent and TEGO801W defoaming agent.
[0030] Furthermore, the dispersant is selected from at least one of TEGODi spers715w, TEGODi spers755w, and TEGOWet280.
[0031] Furthermore, the leveling agent is selected from at least one of BYK300, BYK306 and BYK333.
[0032] The invention also provides epoxy coating prepared by the preparation process.
[0033] The invention also provides application of the epoxy coating in preparing leather products.
[0034] Furthermore, the epoxy coating is used in the preparation of leather shoes.
[0035] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0036] 1. The present invention provides a waterproof and wear-resistant epoxy coating for leather, and a preparation process and application thereof. The epoxy coating has excellent waterproof and wear-resistant properties, excellent comprehensive properties, high thermal storage stability, and can be used to prepare leather products.
[0037] 2. Nan Ya Plastics Industrial Co., Ltd.'s NPEL-128 epoxy resin is a liquid epoxy resin generated by the reaction of bisphenol A and epoxy chloride, and is a resin commonly used in leather coatings. However, the wear resistance of the NPEL-128 epoxy resin coating is not ideal. The present invention compounds the NPEL-128 epoxy resin with the NPEL-128S epoxy resin and a polymer to improve the wear resistance of the coating. The tensile strength of the epoxy coating is improved.
[0038] 3. The inventors found that after adding polymers to the coating system, when the upper of leather shoes is bent during wearing, cracks are more likely to form at the creases. These cracks not only affect the appearance, but also gradually expand, leading to greater damage. Analysis shows that the ratio of soft and hard segments in the coating affects the elasticity of the coating, which cannot adapt to the bending and stretching of the leather during wearing or use. The present invention can improve the folding resistance of epoxy coatings by modifying the mixed filler. At the same time, under this condition, the water resistance and thermal storage stability of the coating are improved. DETAILED DESCRIPTION
[0039] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Some of the raw materials in the embodiments are purchased from the following manufacturers:
[0041] The particle size of nano samarium oxide is 40-60nm. Zhejiang Zhiti Nano Micro New Materials Co., Ltd.
[0042] Boron nitride, average particle size 100nm, specific surface area 10-20m 2 / g. Zhejiang Zhiti Nano-Micro New Materials Co., Ltd.
[0043] Organic bentonite: 94wt% can pass through a 200-mesh sieve. Hemmingsdeqian organic modified bentonite BENTONE EW-NA.
[0044] Example 1
[0045] This embodiment provides a waterproof and wear-resistant epoxy coating for leather, and its preparation process includes the following steps:
[0046] (1) Weigh the following raw materials by mass: 15 parts of modified filler, 52 parts of epoxy resin, 17 parts of polymer, 43 parts of polythiol curing agent, 0.3 parts of antioxidant, 0.2 parts of defoaming agent, 0.4 parts of dispersant, and 0.3 parts of leveling agent;
[0047] The epoxy resin is a mixture of NPEL-128 epoxy resin and NPEL-128S epoxy resin in a mass ratio of 2.6:1;
[0048] The preparation method of the polymer is as follows: by weight:
[0049] Step 1: dissolving 410 parts of isophorone diisocyanate in 1500 parts of N-methylpyrrolidone, heating to 53° C., adding 1220 parts of polypropylene glycol, and reacting at 53° C. for 4 hours to obtain an isocyanate-terminated first intermediate;
[0050] Step 2: Dissolve 410 parts of diaminodiphenylmethane in 900 parts of N-methylpyrrolidone, heat to 53° C., add 190 parts of toluene diisocyanate, and react at 53° C. for 4 hours to obtain an amino-terminated second intermediate;
[0051] Step 3: 1470 parts of the first intermediate were added to 760 parts of the second intermediate, mixed evenly, and reacted at 82° C. for 3.5 hours to obtain a polymer;
[0052] (2) performing a first mixing of the epoxy resin, the polymer and the modified filler to obtain a first mixture;
[0053] (3) adding an antioxidant, a defoaming agent, a dispersant, and a leveling agent to the first mixture in sequence, and performing a second mixing to obtain a second mixture;
[0054] (4) The second mixture is mixed with a polythiol curing agent to obtain a waterproof and wear-resistant epoxy coating for leather.
[0055] NPEL-128 epoxy resin and NPEL-128S epoxy resin were purchased from Nan Ya Plastics Industrial Co., Ltd.
[0056] The preparation method of the modified filler is:
[0057] (1) calcining a mixed filler at a temperature of 850° C. for 50 minutes to obtain a calcined mixed filler; the mixed filler is a mixture of nano samarium oxide, boron nitride and organic bentonite in a mass ratio of 1:0.4:1.3;
[0058] (2) crushing the calcined mixed filler and grinding it into 80-100 mesh mixed filler powder;
[0059] (3) Mixing a mixed filler powder, tetramethylammonium bromide and an ethanol aqueous solution in a mass ratio of 10:1.1:90, stirring evenly, heating at 57° C. for 4 hours, filtering, and drying to obtain a modified mixed filler.
[0060] The mass percentage concentration of the ethanol aqueous solution is 70%.
[0061] The polythiol curing agent is GLC-905 polythiol curing agent, which was purchased from Shandong Suihua Biotechnology Co., Ltd.
[0062] The antioxidant is antioxidant 1010.
[0063] The defoaming agent is TEGO901W defoaming agent.
[0064] The dispersant is TEGOD ispers715w.
[0065] The leveling agent is BYK300.
[0066] Example 2
[0067] This embodiment provides a waterproof and wear-resistant epoxy coating for leather, and its preparation process includes the following steps:
[0068] (1) Weigh the following raw materials by mass: 17 parts of modified filler, 55 parts of epoxy resin, 15 parts of polymer, 45 parts of polythiol curing agent, 0.2 parts of antioxidant, 0.3 parts of defoaming agent, 0.3 parts of dispersant, and 0.5 parts of leveling agent;
[0069] The epoxy resin is a mixture of NPEL-128 epoxy resin and NPEL-128S epoxy resin in a mass ratio of 2.4:1;
[0070] The preparation method of the polymer is as follows: by weight:
[0071] Step 1: dissolving 420 parts of isophorone diisocyanate in 1500 parts of N-methylpyrrolidone, heating to 52° C., adding 1200 parts of polypropylene glycol, and reacting at 52° C. for 5 hours to obtain an isocyanate-terminated first intermediate;
[0072] Step 2: dissolving 400 parts of diaminodiphenylmethane in 900 parts of N-methylpyrrolidone, heating to 52° C., adding 180 parts of toluene diisocyanate, and reacting at 52° C. for 5 hours to obtain an amino-terminated second intermediate;
[0073] Step 3: Add 1450 parts of the first intermediate to 750 parts of the second intermediate, mix well, and react at 80° C. for 4 hours to obtain a polymer;
[0074] (2) performing a first mixing of the epoxy resin, the polymer and the modified filler to obtain a first mixture;
[0075] (3) adding an antioxidant, a defoaming agent, a dispersant, and a leveling agent to the first mixture in sequence, and performing a second mixing to obtain a second mixture;
[0076] (4) The second mixture is mixed with a polythiol curing agent to obtain a waterproof and wear-resistant epoxy coating for leather.
[0077] NPEL-128 epoxy resin and NPEL-128S epoxy resin were purchased from Nan Ya Plastics Industrial Co., Ltd.
[0078] The preparation method of the modified filler is:
[0079] (1) calcining a mixed filler at a temperature of 900° C. for 40 minutes to obtain a calcined mixed filler; the mixed filler is a mixture of nano samarium oxide, boron nitride and organic bentonite in a mass ratio of 1:0.6:1.2;
[0080] (2) crushing the calcined mixed filler and grinding it into 80-100 mesh mixed filler powder;
[0081] (3) Mixing a mixed filler powder, tetramethylammonium bromide and an ethanol aqueous solution in a mass ratio of 10:1.3:100, stirring evenly, heating at 60° C. for 3 hours, filtering, and drying to obtain a modified mixed filler.
[0082] The mass percentage concentration of the ethanol aqueous solution is 65%.
[0083] The polythiol curing agent is GLC-905 polythiol curing agent, which was purchased from Shandong Suihua Biotechnology Co., Ltd.
[0084] The antioxidant is antioxidant 168.
[0085] The defoaming agent is TEGO902W defoaming agent.
[0086] The dispersant is TEGOD ispers755w.
[0087] The leveling agent is BYK306.
[0088] Example 3
[0089] This embodiment provides a waterproof and wear-resistant epoxy coating for leather, and its preparation process includes the following steps:
[0090] (1) Weigh the following raw materials by mass: 13 parts of modified filler, 50 parts of epoxy resin, 15 parts of polymer, 40 parts of polythiol curing agent, 0.2 parts of antioxidant, 0.1 parts of defoaming agent, 0.3 parts of dispersant, and 0.2 parts of leveling agent;
[0091] The epoxy resin is a mixture of NPEL-128 epoxy resin and NPEL-128S epoxy resin in a mass ratio of 2.8:1;
[0092] The preparation method of the polymer is as follows: by weight:
[0093] Step 1: dissolving 400 parts of isophorone diisocyanate in 1500 parts of N-methylpyrrolidone, heating to 52° C., adding 1250 parts of polypropylene glycol, and reacting at 52° C. for 5 hours to obtain an isocyanate-terminated first intermediate;
[0094] Step 2: Dissolve 420 parts of diaminodiphenylmethane in 900 parts of N-methylpyrrolidone, heat to 52° C., add 200 parts of toluene diisocyanate, and react at 52° C. for 5 hours to obtain an amino-terminated second intermediate;
[0095] Step 3: Add 1480 parts of the first intermediate to 770 parts of the second intermediate, mix well, and react at 80° C. for 4 hours to obtain a polymer;
[0096] (2) performing a first mixing of the epoxy resin, the polymer and the modified filler to obtain a first mixture;
[0097] (3) adding an antioxidant, a defoaming agent, a dispersant, and a leveling agent to the first mixture in sequence, and performing a second mixing to obtain a second mixture;
[0098] (4) The second mixture is mixed with a polythiol curing agent to obtain a waterproof and wear-resistant epoxy coating for leather.
[0099] NPEL-128 epoxy resin and NPEL-128S epoxy resin were purchased from Nan Ya Plastics Industrial Co., Ltd.
[0100] The preparation method of the modified filler is:
[0101] (1) calcining a mixed filler at a temperature of 850° C. for 50 minutes to obtain a calcined mixed filler; the mixed filler is a mixture of nano samarium oxide, boron nitride and organic bentonite in a mass ratio of 1:0.6:1.3;
[0102] (2) crushing the calcined mixed filler and grinding it into 80-100 mesh mixed filler powder;
[0103] (3) Mixing a mixed filler powder, tetramethylammonium bromide and an ethanol aqueous solution in a mass ratio of 10:1:95, stirring evenly, heating at 57° C. for 4 hours, filtering, and drying to obtain a modified mixed filler.
[0104] The mass percentage concentration of the ethanol aqueous solution is 70%.
[0105] The polythiol curing agent is GLC-905 polythiol curing agent, which was purchased from Shandong Suihua Biotechnology Co., Ltd.
[0106] The antioxidant is antioxidant 1010.
[0107] The defoaming agent is TEGO901W defoaming agent.
[0108] The dispersant is TEGOD ispers715w.
[0109] The leveling agent is BYK300.
[0110] Comparative Example 1
[0111] The difference between this comparative example and Example 1 is that the epoxy resin is a mixture of NPEL-128 epoxy resin and NPEL-128S epoxy resin in a mass ratio of 1:1.
[0112] Comparative Example 2
[0113] The difference between this comparative example and Example 1 is that NPEL-128S epoxy resin is replaced by NPEL-134 epoxy resin purchased from Nan Ya Plastics Industrial Co., Ltd.
[0114] Comparative Example 3
[0115] The difference between this comparative example and Example 1 is that the proportions of the polymer and the epoxy resin are different.
[0116] The raw materials were weighed according to the mass proportions: 15 parts of modified filler, 44 parts of epoxy resin, 25 parts of polymer, 43 parts of polythiol curing agent, 0.3 parts of antioxidant, 0.2 parts of defoaming agent, 0.4 parts of dispersant and 0.3 parts of leveling agent.
[0117] Comparative Example 4
[0118] The difference between this comparative example and Example 1 is that the polymer is replaced by NPEL-127 epoxy resin purchased from Nan Ya Plastics Industrial Co., Ltd.
[0119] Comparative Example 5
[0120] The difference between this comparative example and Example 1 is that the preparation method of the modified filler is: mixing a mixed filler, a silane coupling agent KH560, and a 70wt% ethanol aqueous solution in a mass ratio of 1:0.02:8, and the mixed filler is a mixture of nano samarium oxide, boron nitride and organic bentonite in a mass ratio of 1:0.4:1.3; reacting at 70°C for 6h, filtering, washing, and drying to obtain a modified filler.
[0121] Comparative Example 6
[0122] The difference between this comparative example and Example 1 is that the mass ratio of nano samarium oxide, boron nitride and organic bentonite is 1:1:1.
[0123] Comparative Example 7
[0124] The difference between this comparative example and Example 1 is:
[0125] The particle size of nano samarium oxide is 100-150nm. Zhejiang Zhiti Nano Micro New Materials Co., Ltd.
[0126] Boron nitride, average particle size 180nm, specific surface area 4-7m 2 / g. Zhejiang Zhiti Nano-Micro New Materials Co., Ltd.
[0127] Organic bentonite: particle size ≤1μm. Model: Deqian Hemmings BENTONE SD-2 organic bentonite.
[0128] Performance Testing
[0129] The coatings of Examples 1-3 and Comparative Examples 1-7 were tested for performance:
[0130] 1. Tensile strength: GB / T2567-2008, 25℃×7 days (humidity 50%);
[0131] 2. Folding resistance at room temperature: refer to GB / T3903.41-2019, use leather flexural resistance tester, 23°C, 100,000 cycles;
[0132] 3. Low temperature folding resistance: refer to GB / T3903.41-2019, use leather flexural resistance tester, -10℃, 50,000 cycles;
[0133] 4. Gakushin type friction value: tested using Japan Yasuda (Gakushin type) color fastness friction tester;
[0134] 5. Thermal storage stability: 50℃ thermal storage for 20 days.
[0135] 6. Water resistance: Spray the epoxy coating onto the surface of the leather embryo and let it stand at 50℃ for 2 hours;
[0136] 7. The roller coating is: apply the epoxy coating to the surface of the leather embryo with a spraying amount of 8g /
[0137] square feet of embryonic skin, dry; then refer to GJB2589.7-1996 to determine the water penetration times.
[0138] The performance test results of each example are shown in Table 1.
[0139] Table 1 Performance test results
[0140]
[0141]
[0142] The results show that the epoxy coatings of Examples 1-2 have excellent comprehensive performance, and the performance decreases to varying degrees when the raw materials and conditions for preparation are changed. Comparative Example 3 shows that when the amount of polymer added increases, the folding resistance of the coating decreases.
[0143] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A process for preparing a waterproof and wear-resistant epoxy coating for leather, It is characterized in that The following steps are involved: (1) Weigh the raw materials by mass: 13-17 parts of modified filler, 50-55 parts of epoxy resin, 15-20 parts of polymer, 40-45 parts of polythiol curing agent, 0.2-0.4 parts of antioxidant, 0.1-0.3 parts of defoaming agent, 0.3-0.5 parts of dispersant and 0.2-0.5 parts of leveling agent; The epoxy resin is a mixture of NPEL-128 epoxy resin and NPEL-128S epoxy resin in a mass ratio of 2.4-2.8:1; The preparation method of the polymer is as follows: by weight: Step 1: dissolving 400-420 parts of isophorone diisocyanate in 1500 parts of N-methylpyrrolidone, heating to 52-55° C., adding 1200-1250 parts of polypropylene glycol, and reacting at 52-55° C. for 3-5 hours to obtain an isocyanate-terminated first intermediate; Step 2: dissolving 400-420 parts of diaminodiphenylmethane in 900 parts of N-methylpyrrolidone, heating to 52-55° C., adding 180-200 parts of toluene diisocyanate, and reacting at 52-55° C. for 3-5 hours to obtain an amino-terminated second intermediate; Step 3: Add 1450-1480 parts of the first intermediate to 750-770 parts of the second intermediate, mix well, and react at 80-84° C. for 3-4 hours to obtain a polymer; (2) performing a first mixing of the epoxy resin, the polymer and the modified filler to obtain a first mixture; (3) adding an antioxidant, a defoaming agent, a dispersant, and a leveling agent to the first mixture in sequence, and performing a second mixing to obtain a second mixture; (4) The second mixture is mixed with a polythiol curing agent to obtain a waterproof and wear-resistant epoxy coating for leather.
2. The preparation process of the waterproof and wear-resistant leather epoxy coating according to claim 1, It is characterized in that The preparation method of the modified filler is: (1) calcining a mixed filler at a temperature of 800-900° C. for 40-60 minutes to obtain a calcined mixed filler; the mixed filler is a mixture of nano samarium oxide, boron nitride and organic bentonite in a mass ratio of 1:0.2-0.6:1.2-1.5; (2) crushing the calcined mixed filler and grinding it into 80-100 mesh mixed filler powder; (3) Mixing a mixed filler powder, tetramethylammonium bromide and ethanol aqueous solution in a mass ratio of 10:1-1.2:80-100, stirring evenly, heating at a temperature of 55-60° C. for 3-5 hours, filtering, and drying to obtain a modified mixed filler.
3. The preparation process of the waterproof and wear-resistant leather epoxy coating according to claim 2, It is characterized in that The mass percentage concentration of the ethanol aqueous solution is 65-70%.
4. The preparation process of the waterproof and wear-resistant leather epoxy coating according to claim 1, It is characterized in that The antioxidant is selected from at least one of antioxidant 1010, antioxidant 168, antioxidant BHT, and antioxidant 330.
5. The preparation process of the waterproof and wear-resistant leather epoxy coating according to claim 1, It is characterized in that The defoaming agent is selected from at least one of TEGO901W defoaming agent, TEGO902W defoaming agent and TEGO801W defoaming agent.
6. The preparation process of the waterproof and wear-resistant leather epoxy coating according to claim 1, It is characterized in that The dispersant is selected from at least one of TEGODispers715w, TEGODispers755w, and TEGOWet280.
7. The preparation process of the waterproof and wear-resistant leather epoxy coating according to claim 1, It is characterized in that The leveling agent is selected from at least one of BYK300, BYK306 and BYK333.
8. An epoxy coating obtained by the preparation process according to any one of claims 1 to 7.
9. Use of the epoxy coating according to claim 8 in the preparation of leather products.
10. The use according to claim 9, It is characterized in that The epoxy coating is applied to the preparation of leather shoes.
Citation Information
Patent Citations
Modified packing for aviation cable material and preparation method of modified packing
CN104151610A
Preparation method of wear-resistant and tear-resistant finishing auxiliary agent for leather
CN115304991A
Elastic coating composition with IPN structure and preparation method of elastic coating composition
CN115612385A
Super-wear-resistant polyurethane floor coating suitable for low-temperature environment