Knife coating dynamics design method based on stress wave propagation
Through stress wave propagation simulation and finite element model, the material and structure of the tool coating are optimized, which solves the problem that the static method in the existing technology cannot conform to the dynamic environment of high-speed cutting, and achieves the improvement of the dynamic performance of the coating and the cutting effect. Stability extended.
Patent Information
- Application Number
- CN202411293206.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-26
AI Technical Summary
The existing technology relies on static methods when designing and evaluating tool coatings, and cannot effectively fit the dynamic environment of high-speed cutting, resulting in large differences in static properties and cutting performance. The traditional test methods are cumbersome and inefficient, so it is impossible to design the coating power from scratch. Learn performance.
Using a design method based on stress wave propagation, the basic load data is obtained through cutting experiments, a finite element model is established for stress wave simulation, the stress waveform structure and attenuation rate are calculated, the coating material and structure are optimized, and the appropriate modulation period is designed to enhance the coating. kinetic properties.
It effectively avoids fatigue cracking and layered fallout caused by the inability to quickly balance stress waves in high-speed cutting, and extends the service life of the tool coating and the stability of the cutting effect.
Smart Images

Figure CN119026275A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mechanical processing, and in particular relates to a tool coating dynamics design method based on stress wave propagation. Background Art
[0002] As modern material structures continue to become more refined, barrier materials are welcoming new opportunities. As a key barrier material at the micro-nano scale, coatings are widely used in the field of surface protection of materials. Coated tools are known as the "teeth" of modern industry and play an irreplaceable and important role in advanced manufacturing fields such as aerospace, new energy vehicles, consumer electronics, and cutting processing. However, extremely harsh cutting environments and stringent processing requirements have put forward increasingly higher mechanical performance requirements for tool coating materials.
[0003] At present, static performance is the main indicator for designing and judging tool coatings, and the cutting performance of tool coatings is improved by pursuing higher hardness and toughness. However, the designed coated tools still have obvious shortcomings, mainly the following problems:
[0004] First, the static properties of tool coatings do not match the high-speed cutting service environment. Using static data such as hardness and toughness to evaluate dynamic behavior is biased and ineffective. The high-speed cutting process is a dynamic strong loading process, which belongs to the category of dynamics. Its loading load changes with time and produces high strain in a very short time at a very small scale. Therefore, the dynamic response process caused by the inertial effect must be considered, and it cannot be simply blurred as a static problem. Secondly, the failure of tool coatings is often not due to insufficient static indicators, but poor dynamic impact resistance. Failure analysis after high-speed cutting shows that although coating wear is inevitable, cracking, delamination and shedding caused by strong load impact are more common forms of catastrophic damage to the coating and ultimately lead to protection failure. The intermittent impact load of the "petal-shaped" edge of the milling cutter and the cyclic impact of the jagged chips produced by turning on the coating surface will cause high strain and inertia effects on the tool coating surface, thereby exciting stress waves. Before the stress is balanced, the dynamic propagation process of the stress wave in the tool coating, such as transmission, reflection and scattering, will lead to severe stress concentration at the interface of the tool coating, which can easily cause fatigue cracking, tensile fracture and delamination of the coating, making it difficult for the functional characteristics of the tool coating to be exerted.
[0005] The design and evaluation of tool coatings at home and abroad still rely on statics methods, which are inconsistent with the dynamic environment of actual high-speed cutting. The statics performance and cutting performance have a large deviation, and the conclusions are even opposite. The use of reciprocating impact tests to evaluate coating performance is based on experimental trial and error, and cannot design the dynamic performance of the coating from scratch. It also has cumbersome steps, complex equipment, high prices, and low efficiency. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a tool coating dynamics design method based on stress wave propagation, which can be compatible with the dynamic environment of actual high-speed cutting and has a simple and clear design process.
[0007] The technical solution of the present invention to solve the above technical problems is:
[0008] A tool coating dynamics design method based on stress wave propagation includes the following steps:
[0009] Design material selection: determine the tool base material and cutting material according to the actual lathe model, and select the coating material based on the projection coefficient of the coating material;
[0010] Cutting experiment: Use the traditional static performance evaluation method to select the coating modulation cycle of the tool, select the corresponding tool, and install the corresponding tool on the lathe to actually cut the selected cutting material. And obtain the basic load data in the actual cutting process through in-situ detection;
[0011] A simulation model is established, with basic load data as data input, the upper boundary as the self-owned boundary, the left, right and lower boundaries as semi-infinite boundaries, and fixed constraints are applied, the mesh is refined, and a finite element model for stress wave simulation is established;
[0012] Cutting simulation: input the material properties of the selected tool substrate, cutting material and tool coating material into the simulation model, use the simulation model to simulate the cutting of at least one coated tool with a modulation period between 75 and 1200 nm, perform data settlement on the stress wave propagation process at the moment of high-speed cutting impact, and obtain the corresponding stress waveform structure;
[0013] Results analysis: The corresponding stress waveform structure is calculated and analyzed, and the normal stress time-space cloud diagram is drawn to evaluate the dynamic response behavior of the coating to the high-speed cutting stress wave. The dynamic performance of different coating systems and structures is evaluated by calculating the stress wave attenuation rate.
[0014] Tool design, according to the dynamic properties of the coating and the lathe application, select the corresponding cutting tool with a suitable modulation period for preparation, and obtain the cutting coating tool with tool coating dynamics design based on stress wave propagation.
[0015] Specifically, in the design material selection step, the coating material is selected by the formula Obtain, where T is the transmission coefficient of the coating material with K sublayers, is the impedance ratio between the jth layer and the (j+1)th layer; The specific calculation method is ,in is the mass density of the coating material, is the longitudinal wave velocity under plane stress conditions.
[0016] Preferably, in the step of establishing a simulation model, the finite element model established is a two-dimensional explicit finite element model.
[0017] Specifically, in the cutting experiment, the in-situ detection obtains the cutting pressure of each cutting in the cutting process, obtains the average cutting load force by counting the cutting pressure at least once, calculates the impact stress based on the average cutting load force, and uses the impact stress as the basic load data.
[0018] Preferably, the calculation formula of the average cutting load force is N p =(N1+N2+……N n ) / n, where N is the cutting pressure detected by in-situ detection during cutting, n is the number of cutting times, n≥1;
[0019] The impact stress calculation formula is: , where S is the actual contact area of the cutting, which is calculated from the scanning electron microscope photograph of the surface morphology after impact.
[0020] Specifically, in the cutting simulation step, the stress waveform structure includes the transmission, reflection and scattering behaviors of the internal interface of the coating and the interface between the substrate and the coating; wherein the material properties of the cutting material are elastic, elastoplastic or viscoelastic-plastic.
[0021] Specifically, in the design material selection step, the material of the tool substrate includes one of high-speed steel, stainless steel, cemented carbide and titanium alloy, and the thickness y2 is 0.002~20 mm; the coating material is one of transition metal, transition metal nitride, transition metal carbide, BN, diamond and diamond-like carbon, and the thickness y1 is 0.1~500 μm.
[0022] Preferably, the transition metal includes Ti, Cr, and Zr; the transition metal nitride includes TiN, CrN, AlN, TaN, TiAlN, and TiSiN; and the transition metal carbide includes TiC, CrC, TaC, CrAlC, and TiSiC.
[0023] Preferably, the coating structure in the coated tool in the cutting simulation step includes one of single layer, multi-layer, nano multi-layer, nano composite and gradient structure or a composite structure formed by a combination of two.
[0024] Specifically, in the result calculation step, the calculation formula of the stress wave attenuation rate is: ,in is the maximum compressive stress at the membrane-base interface, extracted from the normal stress time-space cloud map. is the input impact pressure.
[0025] The present invention has the following beneficial effects: by analyzing the impact stress generated during the cutting process, cutting simulation, and combining it with stress wave analysis, a tool coating that is compatible with the dynamic environment of actual high-speed cutting is screened out, effectively avoiding problems such as fatigue cracking, tensile fracture, and delamination of the tool coating caused by the inability of the stress wave to quickly reach a stress equilibrium state during intermittent impact loads, thereby effectively extending the service life of the tool coating and the stability of the cutting effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the explicit dynamics finite element simulation model of stress wave propagation in the present invention.
[0027] Figure 2 Schematic diagram of the structure of multilayer Ti / TiN with a modulation period of 1200 nm and the corresponding cross-sectional SEM image in the present invention.
[0028] Figure 3 Schematic diagram of the stress wave propagation structure of multilayer Ti / TiN with a modulation period of 1200 nm in the present invention, wherein 1 is the input load length, 2 is the edge effect release wave, 3 is the maximum tensile stress, 4 is the release tensile wave, 5 is the shock wave front, and 6 is the interface stress sampling point.
[0029] Figure 4 This is the space-time cloud diagram of the normal stress of multilayer Ti / TiN with a modulation period of 1200 nm in the present invention.
[0030] Figure 5 Schematic diagram of the structure of multilayer Ti / TiN with a modulation period of 300 nm in the present invention and the corresponding cross-sectional SEM image.
[0031] Figure 6 This is the space-time cloud diagram of the normal stress of multilayer Ti / TiN with a modulation period of 300 nm in the present invention.
[0032] Figure 7 Schematic diagram of the structure of multilayer Ti / TiN with a modulation period of 75 nm in the present invention and the corresponding cross-sectional SEM image.
[0033] Figure 8 This is the space-time cloud diagram of the normal stress of multilayer Ti / TiN with a modulation period of 75 nm in the present invention.
[0034] Fig. 9 The figure is a comparison of the interface stress time history of multilayer Ti / TiN with modulation periods of 75, 300, and 1200 nm in the present invention.
[0035] Fig.10The figure is a comparison of the cutting performance of multilayer Ti / TiN with modulation periods of 75, 300, and 1200 nm in the present invention.
[0036] Fig.11 The figure is a comparison of the static mechanical properties of multilayer Ti / TiN with modulation periods of 75, 300, and 1200 nm in the present invention. DETAILED DESCRIPTION
[0037] The present invention is described in detail below with reference to the embodiments.
[0038] A tool coating dynamics design method based on stress wave propagation according to an embodiment of the present invention comprises the following steps:
[0039] Design material selection: In this embodiment, the EcoTurn 310 series CNC lathe is used to carry out cutting experiments. The CNC machine tool has a stable spindle transmission with high rigidity, high seismic resistance and high dynamic performance. The cutting tool uses a multi-layer Ti / TiN coated carbide tool. Therefore, it is determined that the tool substrate is WC alloy and the cutting material is Ti-6Al-4V alloy. Subsequently, the coating material is selected by the formula Obtain, where T is the transmission coefficient of the coating material with K sublayers, is the impedance ratio between the jth layer and the (j+1)th layer; The specific calculation method is ,in is the mass density of the coating material, is the longitudinal wave velocity under plane stress conditions. In order to improve the attenuation rate of the coating to stress waves, the transmission coefficient T should be as small as possible. Therefore, by comparing the T values under different system compositions, the coating system can be screened from the perspective of stress wave dynamics, and then based on the actual processing conditions, the coating's anti-oxidation temperature, the target material cost and other factors, the final coating material system can be determined. In this embodiment, a multilayer structure coating is taken as an example, and the most widely used TiN coating is selected as one of them. According to the above formula, the T values of CrN / TiN, ZrN / TiN, CrAlN / TiN, and Ti / TiN are calculated to be 0.999, 0.994, 0.988 and 0.897, respectively. Here, only the T value is considered, so Ti / TiN is selected as the coating.
[0040] In the cutting experiment, the coating modulation period of the tool is selected by the traditional static performance evaluation method. In this embodiment, a conventional multi-layer Ti / TiN coated cemented carbide tool is used, and the corresponding tool is installed on the lathe. The selected cutting material Ti-6Al-4V alloy is actually cut with a cutting speed of 40 m / min, a feed rate of 0.05 mm / rev, and an axial and radial cutting depth of 1 mm. The basic load data in the actual cutting process is obtained through in-situ detection. In this embodiment, an in-situ Kistler 9119AA2 dynamometer sensor is used for in-situ detection. The dynamometer is equipped with a 5080A charge amplifier and a 5697A data acquisition system. The measurement signal is converted into voltage through the charge amplifier channel, and finally the amplified force signal is transmitted to the data acquisition card. The matching DynoWare software processes and analyzes the cutting data. Finally, the cutting pressure after 10 cuts is obtained through in-situ detection, and the formula N is used. p =(N1+N2+……N n ) / n, the average cutting load force is calculated as Np=68 N, where N is the cutting pressure, n is the number of cutting times, and n≥1;
[0041] Based on the theoretical calculation formula of stress Calculate the impact stress =1.23 GPa, where S is the actual contact area of the cutting, and S=5.53×10 -8 m 2 Since the impact stress mainly depends on the cutting parameters, the impact stress of different material systems can be considered consistent under the same cutting parameters, so there is no need to verify it separately for multiple cutting materials.
[0042] The simulation model was established by using the ABAQUS finite element code to establish a two-dimensional explicit finite element model. In this embodiment, a 2D stress wave propagation model was used to obtain the impact stress from the basic load data. =1.23 GPa is the data input. Assuming that the coating interface is ideally smooth, the model boundary is constrained as follows. First, in terms of spatial scale, the WC substrate (~cm) exceeds the coating (~μm) by 10 4orders of magnitude, indicating that the stress wave is initially transmitted into the substrate only when it is reflected multiple times in the coating and tends to stress equilibrium. Therefore, a semi-infinite boundary is used on the lower bottom surface to reduce the amplitude of the stress wave reaching the lower bottom surface to approach 0 and no reflection occurs. Similarly, since the thickness of the coating surface (X direction) is much greater than the coating thickness (Y direction), in order to avoid improper reflection of stress waves at the boundaries on both sides, the boundary in the X direction is also set to a semi-infinite boundary, that is, according to the above theory, the left, right and lower boundaries are completely fixed, the upper boundary is the self-boundary, the left, right and lower boundaries are semi-infinite boundaries, and fixed constraints are applied, and the mesh is refined to refine the number of meshes to about 1,500,000, of which the intermediate mesh is set to CPS4R units and the boundary mesh is set to CINPS4 units. The finite element model for stress wave simulation is established as shown below. Figure 1 shown.
[0043] Cutting simulation: The material properties of the selected tool substrate, cutting material, and tool coating material are input into the simulation model. Since the input pressure is relatively small, 1.23 GPa, the material properties of the Ti and TiN layers are defined as pure elastic, where the mass density of Ti is 4500 kg / m 3 , Young's modulus is 110 GPa, Poisson's ratio is 0.33; the mass density of TiN is 5400 kg / m 3 , Young's modulus is 350 GPa, Poisson's ratio is 0.25; the mass density of the WC matrix is 15550 kg / m 3 , Young's modulus is 642GPa, and Poisson's ratio is 0.22. The simulation model is then used to simulate the cutting of three coated tools with modulation periods of 75, 300 and 1200 nm, respectively. The specific modulation ratio is TiN:Ti=5:1, with TiN on the top and Ti layer on the bottom.
[0044] For the cutting simulation with a period of 1200 nm, that is, the thickness of TiN is 1000 nm and the thickness of Ti is 200 nm in a single modulation period. Figure 2 As shown, the stress wave propagation process at the moment of high-speed cutting impact is settled to obtain the corresponding stress waveform structure as shown in Figure 3 As shown, the data in this figure reflect the transmission, reflection and scattering behaviors of the internal interface of the coating and the interface between the substrate and the coating.
[0045] For the cutting simulation with a period of 300 nm, that is, the thickness of TiN is 250 nm and the thickness of Ti is 50 nm in a single modulation period. Figure 5 As shown, the stress wave propagation process at the moment of high-speed cutting impact is settled to obtain the corresponding stress waveform structure.
[0046] For the cutting simulation of 75 nm period, that is, the thickness of TiN is 62.5 nm and the thickness of Ti is 12.5 nm in a single modulation period. Figure 7 As shown, the stress wave propagation process at the moment of high-speed cutting impact is settled to obtain the corresponding stress waveform structure.
[0047] Result analysis: The stress waveform structures obtained from the cutting simulations with the above three different modulation periods were calculated and analyzed, and the space-time cloud diagram of the normal stress was drawn.
[0048] For the 1200 nm period cutting simulation, the normal stress time-space cloud diagram is shown in the figure below: Figure 4 The results show that the stress head wave increases and decreases alternately at the interface between TiN and Ti layers, and complex reflections occur at the interface between TiN and Ti layers, as well as at the film-substrate interface. Stress concentration occurs within 1 μm of the top of the coating.
[0049] For the 300 nm period cutting simulation, the normal stress time-space cloud diagram is shown in the figure below: Figure 6 As shown in the figure, the range of stress concentration is not significantly different from that at 1200 nm. As the modulation period decreases, the reflection behavior of the stress wave in the layer is weakened, and the stress in the layer is reduced. However, the transmission attenuation of the stress head wave at the interface is weakened, and the stress reaching the film-substrate interface increases.
[0050] For the 75 nm period cutting simulation, the normal stress time-space cloud diagram is shown in Figure 2. Figure 8 As shown in the figure, the range of stress concentration is reduced compared with 1200 nm and 300 nm. Compared with 300 nm, as the modulation period decreases, the reflection behavior of the stress wave in the layer is further weakened, and the stress in the layer is significantly reduced. However, the transmission attenuation of the stress head wave at the interface is weakened, and the stress reaching the film-substrate interface is further increased.
[0051] The interfacial stress time history of Ti / TiN coatings with different modulation periods in the above three cutting simulations is compared. Fig. 9 As shown in the figure, the maximum compressive stress at the membrane-substrate interface is extracted from the figure, which is 756 MPa for 1200 nm, 840 nm for 300 nm, and 1039 MPa for 75 nm. That is, as the modulation period increases, the maximum compressive stress of the interface decreases.
[0052] According to the stress wave attenuation formula The stress wave attenuation capacity of different modulation periods is calculated and evaluated. is the maximum compressive stress at the membrane-base interface, extracted from the normal stress time-space cloud map. is the input impact pressure. It is 1.23 GPa, which is the maximum compressive stress corresponding to the modulation period. Calculation shows that the stress wave attenuation rates of 1200, 300 and 75 nm modulation periods are 38.5%, 31.7% and 15.5%, respectively. That is, with the increase of the modulation period, the attenuation ability of the Ti / TiN coating to stress waves gradually increases.
[0053] Tool design,According to the above analysis and the application of EcoTurn 310 series CNC lathe, a 1200 nm modulation period is selected to prepare the corresponding cutting tool, and the cutting coating tool with tool coating dynamics design based on stress wave propagation is obtained.
[0054] Comparative Example:
[0055] The lathe used in the embodiment is consistent with that used in the embodiment, and the Ti / TiN multilayer coatings of 75, 300 and 1200 nm are selected accordingly, that is, the coating structure is consistent with that in the embodiment, and the coating performance is evaluated by using the traditional static performance, and the hardness test is performed by using the TI-980 nanoindenter developed by Bruker-Hysitron. In order to truly reflect the performance of the Ti / TiN coating, the indentation depth does not exceed 1 / 10 of the coating thickness to avoid the influence of the substrate on the hardness. At the same time, each sample is measured 10 times, the dot position is random, and the average value is finally taken for comparison. Fig.11 As shown in the figure, the hardness of the modulation period of 75, 300 and 1200 nm is 25.2, 23.5 and 19.8 GPa respectively; the elastic modulus is 365, 347, 306 GPa respectively. With the increase of the modulation period, the hardness and elastic modulus gradually decrease. The highest hardness and elastic modulus are obtained at 75 nm, which is attributed to the decrease of the modulation period, the increase of the interlayer interface density, the modulus difference effect and the alternating stress field effect that increase the hardness of the coating. Therefore, according to the evaluation criteria of static performance, the Ti / TiN multilayer coating with a modulation period of 75 nm is the best.
[0056] According to the static performance evaluation system, a Ti / TiN multilayer coating with a modulation period of 75 nm should be used, but according to the design method provided by the present invention, a Ti / TiN multilayer coating with a modulation period of 1200 nm should be used. The conclusions of the two are completely opposite.
[0057] Finally, multi-arc ion plating technology was used to prepare Ti / TiN coatings with modulation periods of 75, 300 and 1200 nm on cemented carbide tools. The SEM images of their cross-sectional structures are shown in Figure 2. Figure 2 , Figure 5 and Figure 7 As shown in the attached figure, the results show that the structure of the prepared coating is basically consistent with the designed structure. Under the same cutting conditions as in the cutting experiment steps in the embodiment, the three cutting tools were subjected to actual high-speed cutting tests. The cutting results are shown in Fig.10 As shown in the figure, when the back tool face is worn by 0.25 mm, the cutting length is 1200nm>300nm>75nm, and as the modulation period increases, the cutting length of the Ti / TiN coating gradually increases. By comparing the stress wave attenuation capability and the cutting performance, the Ti / TiN coating with a modulation period of 1200 nm and a higher stress wave attenuation rate has better cutting performance. Therefore, it is also verified that the design method provided by the present invention is more in line with the dynamic environment of actual high-speed cutting than the traditional method of evaluating coating performance by static performance, and can effectively avoid the problems of fatigue cracking, tensile fracture and delamination of the tool coating caused by the inability of stress waves to quickly reach a stress equilibrium state during intermittent impact loads, and effectively prolong the service life of the tool coating and the stability of the cutting effect.
[0058] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A tool coating dynamics design method based on stress wave propagation, characterized in that: The steps include: Design material selection: determine the tool base material and cutting material according to the actual lathe model, and select the coating material in combination with the projection coefficient of the coating material; Cutting experiment: Use the traditional static performance evaluation method to select the coating modulation cycle of the tool, select the corresponding tool, and install the corresponding tool on the lathe to actually cut the selected cutting material. And obtain the basic load data in the actual cutting process through in-situ detection; A simulation model is established, with basic load data as data input, the upper boundary as the self-owned boundary, the left, right and lower boundaries as semi-infinite boundaries, and fixed constraints are applied, the mesh is refined, and a finite element model for stress wave simulation is established; Cutting simulation: input the material properties of the selected tool substrate, cutting material and tool coating material into the simulation model, use the simulation model to simulate the cutting of at least one coated tool with a modulation period between 75 and 1200 nm, perform data settlement on the stress wave propagation process at the moment of high-speed cutting impact, and obtain the corresponding stress waveform structure; Results analysis: The corresponding stress waveform structure is calculated and analyzed, and the normal stress time-space cloud diagram is drawn to evaluate the dynamic response behavior of the coating to the high-speed cutting stress wave. The dynamic performance of different coating systems and structures is evaluated by calculating the stress wave attenuation rate. Tool design, according to the dynamic properties of the coating and the lathe application, select the corresponding cutting tool with a suitable modulation period for preparation, and obtain the cutting coating tool with tool coating dynamics design based on stress wave propagation.
2. The tool coating dynamics design method based on stress wave propagation according to claim 1, characterized in that: In the design material selection step, the coating material is selected by the formula Obtain, where T is the transmission coefficient of the coating material with K sublayers, is the impedance ratio between the jth layer and the (j+1)th layer; The specific calculation method is ,in is the mass density of the coating material, is the longitudinal wave velocity under plane stress conditions.
3. The tool coating dynamics design method based on stress wave propagation according to claim 1, characterized in that: In the step of establishing a simulation model, the established finite element model is a two-dimensional explicit finite element model.
4. The tool coating dynamics design method based on stress wave propagation according to claim 1 is characterized by: In the cutting experiment, the in-situ detection obtains the cutting pressure of each cutting in the cutting process, obtains the average cutting load force by counting the cutting pressure at least once, calculates the impact stress based on the average cutting load force, and uses the impact stress as the basic load data.
5. The tool coating dynamics design method based on stress wave propagation according to claim 4 is characterized by: The calculation formula of the average cutting load force is N p =(N1+N2+……N n ) / n, where N is the cutting pressure detected by in-situ detection during cutting, n is the number of cutting times, n≥1; The impact stress calculation formula is: , where S is the actual contact area of the cutting, which is calculated from the scanning electron microscope photograph of the surface morphology after impact.
6. The tool coating dynamics design method based on stress wave propagation according to claim 1, characterized in that: In the cutting simulation step, the stress waveform structure includes the transmission, reflection and scattering behaviors of the internal interface of the coating and the interface between the substrate and the coating; wherein the material properties of the cutting material are elastic, elastoplastic or viscoelastic-plastic.
7. The tool coating dynamics design method based on stress wave propagation according to claim 1, characterized in that: In the design material selection step, the material of the tool substrate includes one of high-speed steel, stainless steel, cemented carbide and titanium alloy, and the thickness y2 is 0.002~20 mm; the coating material is one of transition metal, transition metal nitride, transition metal carbide, BN, diamond and diamond-like carbon, and the thickness y1 is 0.1~500 μm.
8. The tool coating dynamics design method based on stress wave propagation according to claim 7, characterized in that: The transition metals include Ti, Cr, and Zr; the transition metal nitrides include TiN, CrN, AlN, TaN, TiAlN, and TiSiN; and the transition metal carbides include TiC, CrC, TaC, CrAlC, and TiSiC.
9. The tool coating dynamics design method based on stress wave propagation according to claim 7, characterized in that: The coating structure of the coated tool in the cutting simulation step includes one of single layer, multi-layer, nano multi-layer, nano composite and gradient structures or a composite structure formed by a combination of two.
10. The tool coating dynamics design method based on stress wave propagation according to claim 4, characterized in that: In the result calculation step, the calculation formula of the stress wave attenuation rate is: ,in is the maximum compressive stress at the membrane-base interface, extracted from the normal stress time-space cloud map. is the input impact pressure.
Citation Information
Cited By
Dynamic stress regulation and control method of crusher in bio-fertilizer production process
CN120190033A