Tannic acid / polyethyleneimine nanofiltration composite membrane and preparation method thereof
By using the interfacial polymerization of tannic acid and polyethyleneimine in the nanofiltration membrane to form a crosslinking network, the interception rate of divalent cations is improved, and the interception rate of divalent scaling cations is solved in the existing nanofiltration membrane to the existing nanofiltration membrane is solved. The problem of low efficiency of industrial wastewater treatment is achieved.
Patent Information
- Application Number
- CN202411386592.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
The existing nanofiltration membrane has a low retention rate of divalent scaling cations (such as divalent magnesium ions and divalent calcium ions), which leads to pipeline scaling and corrosion problems and may cause toxicity to aquatic organisms.
Tannic acid and polyethyleneimine are used as monomers to form a crosslinked polyamide network through interfacial polymerization, which improves the crosslinking degree and pore size of the nanofiltration membrane and enhances the retention ability of divalent cations.
The nanofiltration membrane's retention rate of calcium ions is improved to 94.17% and the magnesium ions is reduced to 97.03%, effectively solving the pipeline scaling problem and improving the retention efficiency of metal cations.
Smart Images

Figure CN119034515A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite nanofiltration membrane preparation, and specifically relates to a tannic acid / polyethyleneimine nanofiltration composite membrane and a preparation method thereof. Background Art
[0002] Membrane separation technology began to appear in the 1930s, and in-depth research was carried out 50 years later. As a new type of chemical separation technology, it plays a significant role in industrial production. Among them, nanofiltration membrane technology is an efficient separation technology in water treatment. Compared with traditional desalination technology, it has the advantages of small pore size, good separation effect, and long service life. It has been widely used in the fields of medical, environmental protection, sewage treatment, etc. At present, most commercial nanofiltration membranes are composite membranes, which mainly separate solutes from water through particle size screening and electrostatic interaction. Nanofiltration separation technology can screen nanometer-scale particles and remove organic pollutants with a molecular weight of about 200-1500. In addition, it has the advantages of high efficiency, low cost, and environmental friendliness in separating salts.
[0003] Nowadays, the most widely used nanofiltration membrane is the polyamide nanofiltration membrane prepared by interfacial polymerization. Polyamide nanofiltration membrane can remove most heavy metals, organic matter and suspended solids in industrial wastewater. However, commercial nanofiltration membranes often show a low retention rate for divalent scaling cations (such as divalent magnesium ions and divalent calcium ions) in industrial wastewater, which will cause pipe scaling due to changes in thermodynamic conditions such as temperature and humidity, and deposit on the surface of the pipe, causing pipeline corrosion. At the same time, industrial wastewater containing more scaling ions may be toxic to aquatic organisms after discharge, thereby destroying the water ecological balance of a region. Due to the Donnnan effect, some nanofiltration composite membranes with negative charges on the surface have a low retention rate for scaling cations. Therefore, relevant researchers have developed positively charged nanofiltration membranes through electrostatic interactions and have been widely used in industrial wastewater treatment. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a tannic acid / polyethyleneimine nanofiltration composite membrane and a preparation method thereof to solve the problem that the prior art nanofiltration composite membrane has a low retention rate for divalent scaling cations.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane comprises the following steps:
[0007] S1, sequentially mixing deionized water, tannic acid and polyethyleneimine, obtaining an aqueous phase solution after magnetic stirring, soaking the base film in the aqueous phase solution, and obtaining a process film after drying;
[0008] S2, mixing n-heptane solution and trimesoyl chloride to obtain process solution one, mixing dichloromethane and ferric acetylacetonate to obtain process solution two, mixing process solution two and process solution one to obtain an organic phase solution, and after soaking the process membrane in the organic phase solution, obtaining a tannic acid / polyethyleneimine nanofiltration composite membrane.
[0009] A further improvement of the present invention is:
[0010] Preferably, in S1, the mass fraction of tannic acid in the aqueous solution is 0.03%.
[0011] Preferably, in S1, the mass fraction of polyethyleneimine in the aqueous phase solution is 0.42%.
[0012] Preferably, in S1, the infiltration time is 280-320 s.
[0013] Preferably, in S2, in the organic phase solution, the volume ratio of n-heptane solution to dichloromethane is 9:1.
[0014] Preferably, in S2, the mass fraction of iron acetylacetonate is 0.10%-0.15%.
[0015] Preferably, in S2, the mass fraction of trimesoyl chloride is 11%.
[0016] Preferably, in S2, the immersion time of the process membrane in the organic phase solution is 150-200 s.
[0017] Preferably, in S2, after mixing the n-heptane solution and trimesoyl chloride, the mixture is stirred at 35° C. to obtain process solution 1.
[0018] A tannic acid / polyethyleneimine nanofiltration composite membrane prepared by any one of the above preparation methods comprises a polyethersulfone ultrafiltration base membrane and a nanofiltration membrane attached to the polyethersulfone ultrafiltration base membrane, wherein the nanofiltration membrane is a cross-linked polyamide network formed by polyethyleneimine and trimesoyl chloride; the pores of the polyethersulfone ultrafiltration base membrane are filled with tannic acid, and tannic acid, polyethyleneimine, trimesoyl chloride and ferric acetylacetonate are attached to the nanofiltration membrane.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The invention discloses a tannic acid / polyethyleneimine nanofiltration composite membrane, which is a method of using tannic acid (TA) and ferric acetylacetonate (III) as aqueous phase and organic phase monomers, respectively, and adding PEI and TMC to the aqueous phase and performing interfacial polymerization. In this system, the phenolic hydroxyl group in TA can form a stable complex with the iron in ferric acetylacetonate, and the amine group in PEI performs nucleophilic attack on the acyl chloride group in TMC to form an amide bond, and the process is carried out at the interface to form a cross-linked polyamide network. At the same time, ferric acetylacetonate has abundant oxygen atoms, which can increase the compatibility of aqueous phase and organic phase, and the phenolic hydroxyl group in TA can also form an ester bond with the acyl chloride in TMC, further improving the crosslinking degree of the nanofiltration composite membrane, causing the membrane pore size to become smaller, thereby improving the interception rate of the nanofiltration membrane to divalent cations. The prepared nanofiltration composite membrane has a calcium ion interception rate of up to 94.17%, and a magnesium ion interception rate of up to 97.03%. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 : Scanning electron micrograph and atomic force microscopy of the composite nanofiltration membrane prepared in Example 1;
[0022] Among them, (a) is a scanning electron micrograph, and (b) is an atomic force micrograph;
[0023] Figure 2 : is the rejection rate curve diagram of the membrane obtained in Example 1. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0025] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0026] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0027] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0028] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0029] As the background technology raises, polyamide nanofiltration membranes can remove most heavy metals, organic matter and suspended solids in industrial wastewater. However, polyamide nanofiltration membranes have a very low retention rate for divalent cations (such as divalent magnesium ions and divalent calcium ions) in industrial wastewater, which makes it easy for scaling and corrosion problems to occur in the applied pipelines.
[0030] In order to solve the above problems, the first aspect of the present invention discloses a method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane. The base membrane used is a polyethersulfone ultrafiltration base membrane (PES ultrafiltration membrane), which is a membrane material made of polyethersulfone ultrafine fibers hot-melt bonded together, and belongs to a PES membrane for deep filtration.
[0031] Step 1, soaking the base film in an aqueous solution to form a process film;
[0032] First, deionized water, tannic acid and polyethyleneimine were added to the water phase bottle in sequence, and then the water phase bottle was placed on a magnetic stirrer and stirred for 20 minutes. It can be used after being stirred evenly.
[0033] In addition, in order to promote the IP reaction and form a highly cross-linked polyamide separation layer, and at the same time, tannic acid can improve the anti-biological fouling performance of the nanofiltration composite membrane, the mass fractions of tannic acid and polyethyleneimine in the aqueous solution are generally controlled at 0.03% and 0.42% respectively.
[0034] Finally, the base membrane is immersed in the aqueous solution for 280-320 seconds, and then the aqueous solution is poured out and the membrane surface is evenly blown dry with an ear bulb until no visible liquid remains. Through this process, tannic acid and polyethyleneimine can be deposited on the base membrane; at this time, the main structure of the base membrane is a polyethersulfone ultrafiltration membrane, and tannic acid and polyethyleneimine are attached to the surface of the base membrane.
[0035] Step 2, immersing the process membrane in an organic phase solution to cause an interfacial polymerization reaction to form a tannic acid / polyethyleneimine nanofiltration composite membrane;
[0036] First, 90% n-heptane solution and trimesoyl chloride are added to the organic phase bottle in sequence, and then the organic phase bottle is placed on a magnetic stirring water bath and stirred for 20 minutes. In order to fully dissolve it, the water bath temperature is generally controlled at 35°C to obtain process solution 1. In addition, since ferric acetylacetonate is not easily soluble in n-heptane solution, ferric acetylacetonate is generally first dissolved in dichloromethane solution, and finally the two are mixed evenly. Therefore, 10% dichloromethane and ferric acetylacetonate are added to a beaker in sequence and stirred evenly to obtain process solution 2, and then process solution 2 is poured into process solution 1, and stirred in the organic phase bottle for 10 minutes to mix the solutions evenly to obtain an organic phase solution.
[0037] In addition, in order to make the solution ratio uniform, the volume ratio of n-heptane and dichloromethane is 9:1. In order to make the tannic acid in the aqueous phase and the ferric acetylacetonate in the organic phase form a more stable complex, the mass fraction of ferric acetylacetonate is generally controlled at 0.10%-0.15%.
[0038] As a preferred embodiment, the mass fraction of trimesoyl chloride is 11%.
[0039] Finally, the process membrane is immersed in the organic phase solution for 150-200 seconds, and then the solution is poured out and naturally drained to obtain the tannic acid / polyethyleneimine nanofiltration composite membrane.
[0040] The second aspect of the present invention discloses a composite membrane prepared by the above method, wherein the main body of the prepared membrane is a polyethersulfone ultrafiltration base membrane, a nanofiltration membrane is attached to the polyethersulfone ultrafiltration membrane, tannic acid is filled in the pores of the polyethersulfone ultrafiltration base membrane, tannic acid molecules, polyethyleneimine, trimesoyl chloride and ferric acetylacetonate are attached to the nanofiltration membrane, and the main body of the nanofiltration membrane is a cross-linked polyamide network formed by polyethyleneimine and trimesoyl chloride. Different from the existing reaction of ferric acetylacetonate and tannic acid or polyethyleneimine and trimesoyl chloride, the present invention adds the four raw materials at the same time, and obtains a composite nanofiltration membrane with a compact structure, excellent anti-biological contamination performance and high retention rate for metal cations by optimizing the formula. The difference from other nanofiltration membranes is that ferric acetylacetonate can increase the compatibility of the aqueous phase and the organic phase. Tannic acid contains a large number of hydroxyl groups, which can not only form a stable complex with ferric acetylacetonate, but also form an ester bond with the acyl chloride in trimesoyl chloride, further improving the cross-linking degree of the nanofiltration composite membrane, thereby improving the retention rate of the nanofiltration membrane for divalent cations.
[0041] The ferric acetylacetonate polyamide membrane removes divalent cations mainly through screening effect and charge effect. Since the polyethyleneimine on the membrane surface has a high positive charge, charges of the same kind repel each other, so that metal cations are retained outside the membrane and the removed divalent cations remain in the solution.
[0042] The following is further described in conjunction with specific embodiments.
[0043] Example 1
[0044] Step 1, deionized water, tannic acid and polyethyleneimine are added to an aqueous phase bottle in sequence, and then the aqueous phase bottle is placed on a magnetic stirrer and stirred for 20 minutes, and an aqueous phase solution is obtained after uniform stirring; wherein the mass fraction of tannic acid is 0.03%, and the mass fraction of polyethyleneimine is 0.42%, and the base film is immersed in the aqueous phase solution for 300 seconds to obtain a process membrane;
[0045] Step 2, add 90% n-heptane solution and trimesoyl chloride to the organic phase bottle in sequence, then place the organic phase bottle on a magnetic stirring water bath and stir for 20 minutes, in order to fully dissolve it, the water bath temperature is controlled at 35°C, obtain process solution 1, add 10% dichloromethane and ferric acetylacetonate to the beaker in sequence and stir evenly, obtain process solution 2, then pour process solution 2 into process solution 1, stir in the organic phase bottle for 10 minutes, mix the solution evenly, and obtain an organic phase solution. Among them, the mass fraction of trimesoyl chloride in the organic phase solution is 0.11%, and the mass fraction of ferric acetylacetonate is 0.14%; immerse the process membrane in the organic phase solution for 200 seconds to obtain a tannic acid / polyethyleneimine nanofiltration composite membrane.
[0046] See also Figure 1 The scanning electron micrograph and atomic force micrograph of the composite nanofiltration membrane prepared in Example 1 are shown; it can be seen from the figure that the prepared nanofiltration composite membrane has a typical nodule structure.
[0047] The nanofiltration membrane prepared in this example was cut and installed on a nanofiltration membrane test instrument. Then, a calcium chloride solution with a concentration of 2 g / l was prepared, and the water inlet pipe was placed in the calcium chloride solution. Then, the test instrument was turned on and the pressure was set to 5 bar. The flow rate was adjusted to be stable at 50 m / s. 3 / h, the pressure and flow readings generally reach a stable state in about 15 minutes. At this time, start timing and use a weighed test tube to collect samples after 2 hours, then use a conductivity meter to measure the conductivity of the sample liquid, and finally convert the sample conductivity into retention rate.
[0048] Figure 2 The interception rate curve of the membrane obtained in Example 1 shows that the interception rate of the prepared nanofiltration composite membrane for sodium ions is 72.13%. Generally, under room temperature test conditions, the interception rate of calcium chloride can reach 94.17% when filtering a 2g / l calcium chloride solution, and the interception rate of magnesium chloride can reach 97.03% when filtering a 2g / l magnesium chloride solution. The application of the present invention to industrial wastewater treatment can effectively solve the problem of equipment scaling.
[0049] The method of the present invention is not limited to the preparation of polyamide composite nanofiltration membrane, but also suitable for preparing other high-performance interfacial polymerization separation membranes. The pores of polyamide will affect the separation performance of reverse osmosis membrane, greatly reducing the retention rate. The present invention adds ferric acetylacetonate in the oil phase to increase the cross-linking of the polyamide membrane during interfacial polymerization, and at the same time, the iron ions in the ferric acetylacetonate can coordinate with the oxygen atoms in TMC, so that the electrophilicity of TMC is enhanced, thereby accelerating the formation of highly cross-linked amide bonds with PEI, resulting in a smaller membrane pore size, and improving the retention rate of the nanofiltration membrane to scale ions.
[0050] Example 2
[0051] Step 1, deionized water, tannic acid and polyethyleneimine are added to an aqueous phase bottle in sequence, and then the aqueous phase bottle is placed on a magnetic stirrer and stirred for 20 minutes, and an aqueous phase solution is obtained after uniform stirring; wherein the mass fraction of tannic acid is 0.03%, and the mass fraction of polyethyleneimine is 0.42%, and the base film is immersed in the aqueous phase solution for 280 seconds to obtain a process membrane;
[0052] Steps: add 90% n-heptane solution and trimesoyl chloride to the organic phase bottle in sequence, then place the organic phase bottle on a magnetic stirring water bath and stir for 20 minutes, in order to fully dissolve it, the water bath temperature is controlled at 35°C, obtain process solution one, add 10% dichloromethane and ferric acetylacetonate to a beaker in sequence and stir evenly, obtain process solution two, then pour process solution two into process solution one, stir in the organic phase bottle for 10 minutes, mix the solutions evenly, and obtain an organic phase solution. Among them, the mass fraction of trimesoyl chloride in the organic phase solution is 11%, the mass fraction of ferric acetylacetonate is 0.1%, and the process membrane is immersed in the organic phase solution for 190 seconds to obtain a tannic acid / polyethyleneimine nanofiltration composite membrane.
[0053] Example 3
[0054] Step 1, deionized water, tannic acid and polyethyleneimine are added to an aqueous phase bottle in sequence, and then the aqueous phase bottle is placed on a magnetic stirrer and stirred for 20 minutes, and an aqueous phase solution is obtained after uniform stirring; wherein the mass fraction of tannic acid is 0.03%, and the mass fraction of polyethyleneimine is 0.42%, and the base film is immersed in the aqueous phase solution for 320 seconds to obtain a process membrane;
[0055] Steps: add 90% n-heptane solution and trimesoyl chloride to the organic phase bottle in sequence, then place the organic phase bottle on a magnetic stirring water bath and stir for 20 minutes. In order to fully dissolve it, the water bath temperature is controlled at 35°C to obtain process solution 1, add 10% dichloromethane and ferric acetylacetonate to a beaker in sequence and stir evenly to obtain process solution 2, then pour process solution 2 into process solution 1, stir in the organic phase bottle for 10 minutes to mix the solution evenly, and obtain an organic phase solution. Among them, the mass fraction of trimesoyl chloride in the organic phase solution is 11%, and the mass fraction of ferric acetylacetonate is 0.15%. The process membrane is immersed in the organic phase solution for 180 seconds to obtain a tannic acid / polyethyleneimine nanofiltration composite membrane.
[0056] Example 4
[0057] Step 1, deionized water, tannic acid and polyethyleneimine are added to the water phase bottle in sequence, and then the water phase bottle is placed on a magnetic stirrer and stirred for 20 minutes, and an aqueous phase solution is obtained after stirring evenly; wherein the mass fraction of tannic acid is 0.03%, and the mass fraction of polyethyleneimine is 0.42%, and the base film is immersed in the aqueous phase solution for 290 seconds to obtain a process membrane;
[0058] Steps: add 90% n-heptane solution and trimesoyl chloride to the organic phase bottle in sequence, then place the organic phase bottle on a magnetic stirring water bath and stir for 20 minutes. In order to fully dissolve it, the water bath temperature is controlled at 35°C to obtain process solution 1, add 10% dichloromethane and ferric acetylacetonate to a beaker in sequence and stir evenly to obtain process solution 2, then pour process solution 2 into process solution 1, stir in the organic phase bottle for 10 minutes to mix the solution evenly, and obtain an organic phase solution. Among them, the mass fraction of trimesoyl chloride in the organic phase solution is 11%, and the mass fraction of ferric acetylacetonate is 0.13%. The process membrane is immersed in the organic phase solution for 170 seconds to obtain a tannic acid / polyethyleneimine nanofiltration composite membrane.
[0059] Example 5
[0060] Step 1, deionized water, tannic acid and polyethyleneimine are added to an aqueous phase bottle in sequence, and then the aqueous phase bottle is placed on a magnetic stirrer and stirred for 20 minutes, and an aqueous phase solution is obtained after uniform stirring; wherein the mass fraction of tannic acid is 0.03%, and the mass fraction of polyethyleneimine is 0.42%, and the base film is immersed in the aqueous phase solution for 310 seconds to obtain a process membrane;
[0061] Step 2, add 90% n-heptane solution and trimesoyl chloride to the organic phase bottle in sequence, then place the organic phase bottle on a magnetic stirring water bath and stir for 20 minutes, in order to fully dissolve it, the water bath temperature is controlled at 35 ° C, obtain process solution 1, add 10% dichloromethane and ferric acetylacetonate to the beaker in sequence and stir evenly, obtain process solution 2, then pour process solution 2 into process solution 1, stir in the organic phase bottle for 10 minutes, mix the solution evenly, and obtain an organic phase solution. Among them, the mass fraction of trimesoyl chloride in the organic phase solution is 11%, and the mass fraction of ferric acetylacetonate is 0.15%. The process membrane is immersed in the organic phase solution for 160 seconds to obtain a tannic acid / polyethyleneimine nanofiltration composite membrane.
[0062] Example 6
[0063] Step 1, deionized water, tannic acid and polyethyleneimine are added to an aqueous phase bottle in sequence, and then the aqueous phase bottle is placed on a magnetic stirrer and stirred for 20 minutes, and an aqueous phase solution is obtained after uniform stirring; wherein the mass fraction of tannic acid is 0.03%, and the mass fraction of polyethyleneimine is 0.42%, and the base film is immersed in the aqueous phase solution for 320 seconds to obtain a process membrane;
[0064] Steps: add 90% n-heptane solution and trimesoyl chloride to the organic phase bottle in sequence, then place the organic phase bottle on a magnetic stirring water bath and stir for 20 minutes, in order to fully dissolve it, the water bath temperature is controlled at 35°C, obtain process solution one, add 10% dichloromethane and ferric acetylacetonate to a beaker in sequence and stir evenly, obtain process solution two, then pour process solution two into process solution one, stir in the organic phase bottle for 10 minutes, mix the solutions evenly, and obtain an organic phase solution. Among them, the mass fraction of trimesoyl chloride in the organic phase solution is 11%, and the mass fraction of ferric acetylacetonate is 0.12%, and the process membrane is immersed in the organic phase solution for 200 seconds to obtain a tannic acid / polyethyleneimine nanofiltration composite membrane.
[0065] The invention discloses a tannic acid / polyethyleneimine nanofiltration composite membrane, which is a kind of TA and ferric acetylacetonate (III) used as aqueous phase and organic phase monomers respectively, and PEI and TMC are added by aqueous phase to carry out interfacial polymerization reaction. In this system, the phenolic hydroxyl group in TA can form a stable complex with the iron in ferric acetylacetonate, and the amine group in PEI carries out nucleophilic attack on the acyl chloride group in TMC to form amide bond, and the process is carried out at the interface to form a cross-linked polyamide network. At the same time, ferric acetylacetonate has abundant oxygen atoms, can increase the compatibility of aqueous phase and organic phase, and the phenolic hydroxyl group in TA can also form ester bond with the acyl chloride in TMC, further improves the crosslinking degree of nanofiltration composite membrane, causes membrane pore size to become smaller, thereby improves the retention rate of nanofiltration membrane to divalent cations.
[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane, characterized in that: The following steps are involved: S1, sequentially mixing deionized water, tannic acid and polyethyleneimine, obtaining an aqueous phase solution after magnetic stirring, soaking the base film in the aqueous phase solution, and obtaining a process film after drying; S2, mixing n-heptane solution and trimesoyl chloride to obtain process solution one, mixing dichloromethane and ferric acetylacetonate to obtain process solution two, mixing process solution two and process solution one to obtain an organic phase solution, and after soaking the process membrane in the organic phase solution, obtaining a tannic acid / polyethyleneimine nanofiltration composite membrane.
2. The method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane according to claim 1, characterized in that: In S1, the mass fraction of tannic acid in the aqueous solution is 0.03%.
3. The method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane according to claim 1, characterized in that: In S1, the mass fraction of polyethyleneimine in the aqueous phase solution is 0.42%.
4. The method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane according to claim 1, characterized in that: In S1, the infiltration time was 280-320 s.
5. The method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane according to claim 1, characterized in that: In S2, in the organic phase solution, the volume ratio of the n-heptane solution to the dichloromethane is 9:
1.
6. The method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane according to claim 1, characterized in that: In S2, the mass fraction of iron acetylacetonate is 0.10%-0.15%.
7. The method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane according to claim 1, characterized in that: In S2, the mass fraction of trimesoyl chloride is 11%.
8. The method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane according to claim 1, characterized in that: In S2, the immersion time of the process membrane in the organic phase solution is 150-200 s.
9. The method for preparing a tannic acid / polyethyleneimine nanofiltration composite membrane according to claim 1, characterized in that: In S2, the n-heptane solution and trimesoyl chloride are mixed and stirred at 35° C. to obtain a process solution 1.
10. A tannic acid / polyethyleneimine nanofiltration composite membrane prepared by the preparation method according to any one of claims 1 to 9, characterized in that: It includes a polyethersulfone ultrafiltration base membrane and a nanofiltration membrane attached to the polyethersulfone ultrafiltration base membrane. The nanofiltration membrane is a cross-linked polyamide network formed by polyethyleneimine and trimesoyl chloride. The pores of the polyethersulfone ultrafiltration base membrane are filled with tannic acid, and tannic acid, polyethyleneimine, trimesoyl chloride and ferric acetylacetonate are attached to the nanofiltration membrane.
Citation Information
Cited By
Positive charge composite nanofiltration membrane based on PTFE and preparation method and application thereof
CN120169177A